A preparation process for a phase change energy storage high-strength cement-based material

By using modified phase change materials in phase change energy storage cement-based materials, combined with red brick micropowder, magnesium phosphate cement and sodium alginate powder, and treated in calcium chloride solution and phosphide solution, high-strength and corrosion-resistant The phosphated film layer solves the problems of poor mechanical properties and paraffin leakage in traditional phase change energy storage materials, and achieves efficient energy storage and release.

CN118894709BActive Publication Date: 2024-12-03SHANDONG JIAOTONG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411398296.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-12-03
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

The mechanical properties of traditional phase change energy storage cement-based materials are poor and the strength of phase change materials are low, resulting in the problems of mechanical properties deterioration and excessive leakage loss of paraffin during use of the prepared materials.

Method used

The precursor particles are formed by red brick micro powder, magnesium phosphate cement, sodium alginate powder and paraffin. After treatment in methanol or ethanol aqueous solution of calcium chloride, the surface is modified in nano-silica phosphide solution. Form a high-strength, corrosion-resistant phosphated film layer to enhance the binding force and heat storage capacity of phase change materials.

Benefits of technology

Improve the compressive strength and thermal conductivity of phase-change energy storage cement-based materials, extend the service life of phase-change materials, enhance compatibility with cement matrix, reduce the adverse effects of mechanical properties, and realize the building energy Efficient storage and release.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894709B_ABST
    Figure CN118894709B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of cement-based material preparation, and specifically discloses a preparation process of a phase-change energy storage high-strength cement-based material, comprising the following steps: (1) adding red brick powder, magnesium phosphate cement, sodium alginate powder, and iron powder to molten paraffin liquid, mixing and cooling, and crushing the solid mixture to obtain precursor particles. (2) placing the precursor particles in a methanol or ethanol aqueous solution containing calcium chloride and stirring them, and obtaining pretreated particles after completion. (3) placing the pretreated particles in a phosphating solution containing nano-silicon dioxide and allowing them to stand to obtain a modified phase-change material. (4) mixing calcium sulfosilicate-sulfoaluminate cement, silicate cement, coarse aggregate, fine aggregate, modified phase-change material, fly ash, fiber, and water reducer, and then adding mixing water to mix well to obtain the modified phase-change material. The modified phase-change material of the present invention not only has high strength itself, but also has good compatibility with cement-based materials, thereby improving mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement-based material preparation, and in particular to a preparation process of a phase-change energy storage high-strength cement-based material. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] As the main cementitious material for concrete, my country's annual cement production has ranked first in the world for more than 20 years, and has exceeded 2 billion tons per year since 2010. Under the new dry process cement production conditions, the production of 1 ton of silicate cement requires 1.2-1.3 tons of lime raw materials, 0.3-0.4 tons of clay raw materials, 0.05-0.15 tons of iron or aluminum-silica correction raw materials, 0.1 tons of standard coal and 90-100kW·h of electricity resources, and emits about 1 ton of carbon dioxide.

[0004] Calcium sulfosilicate-sulfoaluminate cement (TSAC) is a new type of low-carbon solid waste cement made from industrial solid waste. Compared with ordinary Portland cement, calcium sulfosilicate-sulfoaluminate cement has a lower formation temperature, which helps to reduce coal-fired energy consumption and carbon dioxide emissions. Adding phase change materials (PCMs) to calcium sulfosilicate-sulfoaluminate cement to form phase change energy storage cement-based materials can achieve energy storage and release, enhance the thermal storage capacity of buildings, reduce indoor temperature fluctuations, and thus reduce the energy consumption of buildings, which helps to indirectly reduce carbon dioxide emissions and promote the development of low-carbon, green, and energy-saving buildings. The traditional method is usually to wrap the phase change material and then add it to the cement-based material, but due to the poor compatibility between the two and the low strength of the composite phase change material itself, the mechanical properties of the prepared phase change energy storage cement-based material have been greatly deteriorated. Summary of the invention

[0005] The present invention provides a preparation process of a phase-change energy storage high-strength cement-based material. The obtained modified phase-change material not only has high strength itself, but also has good compatibility with cement-based materials, thereby effectively improving the mechanical properties of the prepared phase-change energy storage cement-based material.

[0006] A preparation process of a phase-change energy storage high-strength cement-based material, comprising the following steps:

[0007] (1) Add red brick powder, magnesium phosphate cement, sodium alginate powder and iron powder to molten paraffin liquid, mix well and cool, and crush the obtained solid mixture to obtain precursor particles.

[0008] (2) The precursor particles are placed in a methanol or ethanol aqueous solution containing calcium chloride and stirred, and then dried to obtain pretreated particles.

[0009] (3) placing the pretreated particles in a phosphating solution containing nano-silicon dioxide, mixing them evenly and letting them stand, and obtaining a modified phase change material after completion.

[0010] (4) Calcium sulfosilicate-sulfoaluminate cement, silicate cement, coarse aggregate, fine aggregate, the modified phase change material, fly ash, fiber, and water reducing agent are used as raw materials. The above raw materials are mixed and then mixed with mixing water to obtain the cement-based material.

[0011] Furthermore, in step (1), the ratio of the red brick powder, magnesium phosphate cement, sodium alginate powder, iron powder, and paraffin liquid is 4-7 parts by weight: 2-3 parts by weight: 1-1.25 parts by weight: 2.2-2.8 parts by weight: 8-10 parts by weight. Optionally, the fineness of the red brick powder is 10-30 mesh, and the fineness of the iron powder is 300-400 mesh.

[0012] Furthermore, in step (1), the particle size of the precursor particles is 1-3 mm.

[0013] Furthermore, in step (2), the ratio of the precursor particles to the methanol or ethanol aqueous solution is 1 g: 10-50 ml. Optionally, the mass fraction of calcium chloride in the methanol or ethanol aqueous solution is not less than 2%.

[0014] Furthermore, in step (2), the mass fraction of the methanol or ethanol aqueous solution is 70-80%.

[0015] Furthermore, in step (2), the stirring treatment time is 20 to 40 minutes, thereby promoting the cross-linking and curing reaction of the precursor particles.

[0016] Furthermore, in step (3), the ratio of the pretreated particulate matter to the phosphating solution is 1 g: 10-20 ml.

[0017] Furthermore, in step (3), the phosphating solution comprises the following components: 20-35 g zinc oxide, 50-70 g nitric acid, 20-30 g phosphoric acid, 10-20 g nano-silicon dioxide, 0.15-0.5 g sodium fluoroborate, 0.5-1.5 g copper nitrate, 15-20 g ethylenediaminetetraacetic acid, and 800-1000 ml water.

[0018] Furthermore, in step (3), the standing time is 15 to 30 minutes, so as to encapsulate the surface of the precursor particles.

[0019] Furthermore, in step (4), the proportions of the components in the raw materials are: 80-100 parts by weight of calcium sulfosilicate-sulfoaluminate cement, 20-35 parts by weight of silicate cement, 230-300 parts by weight of coarse aggregate, 145-160 parts by weight of fine aggregate, 30-50 parts by weight of modified phase change material, 40-65 parts by weight of fly ash, 15-23 parts by weight of fiber, and 0.15-0.25 parts by weight of water reducer.

[0020] Furthermore, in step (4), the mixing water is added according to a water-cement ratio of 0.38-0.44.

[0021] Furthermore, in step (4), the fiber includes at least one of polyethylene fiber, polypropylene fiber, polyvinyl alcohol fiber, etc. Optionally, the length of the fiber is 10-25 mm.

[0022] Furthermore, in step (4), the water reducer includes any one of a polycarboxylate water reducer, a naphthalene-based water reducer, a lignin sulfonate water reducer, and the like.

[0023] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects:

[0024] The phase change material of the present invention uses red brick powder, magnesium phosphate cement, sodium alginate powder, iron powder and paraffin as raw materials. On the one hand, the good adsorption performance of the red brick powder is used to increase the storage capacity of paraffin in the phase change material, which helps to improve the efficiency of phase change energy storage. On the other hand, when the phase change material formed by the above raw materials is placed in a methanol or ethanol aqueous solution containing calcium chloride for treatment, the water therein enters through the pores and water absorption of the red brick powder, and the magnesium phosphate cement undergoes a hydration reaction to form a high-strength, high-adhesive gelled product, which not only converts the low-strength phase change material into a high-strength phase change material, reduces the adverse effects of the mechanical properties of the cement matrix caused by its own low strength, and realizes the utilization of solid waste such as construction waste red bricks. At the same time, after the calcium ions enter, the sodium alginate is prompted to undergo a cross-linking reaction to form a gel, and the cross-linked film formed after drying can encapsulate the phase change material. On the other hand, the present invention places the phase change material treated as above in a phosphating solution containing nano-silicon dioxide for surface modification treatment, and the iron powder in the surface layer of the phase change material is phosphated under the action of the phosphating solution, thereby forming a dense and corrosion-resistant phosphating film layer in the surface layer of the phase change material, and the phase change material is re-encapsulated to prevent excessive leakage and loss of paraffin during service, thereby improving the service life of the phase change material. At the same time, the iron powder in the phase change material can also play a heat-conducting role, increase the heat storage capacity and heat release rate of the phase change material. In addition, in this process, the nano-silicon dioxide in the phosphating solution is fixed on the surface of the phosphating film and the phase change material particles, and it undergoes a secondary hydration reaction with the hydration product calcium hydroxide of the cement-based material to form a hydrated calcium silicate gelling component CSH, which increases the bonding force between the phase change material particles and the cement matrix, improves the compatibility of the two, and reduces the adverse effects on the mechanical properties of the phase change energy storage cement-based material of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention and do not constitute an improper limitation of the present invention. The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein:

[0026] Figure 1 XRD pattern of calcium sulfosilicate-sulfoaluminate cement clinker used in the following examples;

[0027] Figure 2 The compressive strength test diagram of the specimen of the following Example 1;

[0028] Figure 3 The thermal conductivity test diagram of the specimen of the following Example 1. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer.

[0030] Unless otherwise defined, all professional and scientific terms used in the present invention have the same meaning as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. If not otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. Now, the technical solution of the present invention is further described in conjunction with specific embodiments.

[0031] The components of the calcium sulfosilicate-sulfoaluminate cement used in the following examples are as follows: Figure 1 As shown, its mineral composition is mainly composed of calcium sulfoaluminate (C4A3 ) and calcium sulfosilicate (C5S2 ) and also includes anhydrous gypsum (CaSO4).

[0032] Example 1

[0033] A preparation process of a phase-change energy storage high-strength cement-based material, comprising the following steps:

[0034] (1) Paraffin is heated to 60°C to form a melt, and then the components are mixed in a ratio of waste red brick powder (fineness 20 mesh), magnesium phosphate cement, sodium alginate powder, iron powder (fineness 300 mesh), and melt = 5 parts by weight: 2.4 parts by weight: 1.1 parts by weight: 2.5 parts by weight: 10 parts by weight, and stirred for 3 minutes. After completion, the mixture is cooled to room temperature, and the obtained solid mixture is crushed and sieved to obtain precursor particles with a particle size of 1-2 mm for later use.

[0035] (2) The precursor particles are placed in an ethanol aqueous solution containing calcium chloride, the ratio of the precursor particles to the ethanol aqueous solution is 1g:30ml, the mass fraction of calcium chloride in the ethanol aqueous solution is 5%, and the mass fraction of the ethanol aqueous solution is 80%. Then stir at a rate of 10r / min for 20min, filter out the particles after completion, and naturally dry for 1 hour to obtain pretreated particles for standby use.

[0036] (3) Mix 25g of zinc oxide, 60g of nitric acid, 22g of phosphoric acid, 15g of nano-silicon dioxide, 0.2g of sodium fluoroborate, 1.0g of copper nitrate, 17g of ethylenediaminetetraacetic acid, and 900ml of water, and stir evenly to obtain a phosphating solution. Then heat to 45°C, place the pretreated particles in the phosphating solution (the ratio of the two is 1g:10ml), stir and let stand for 20 minutes, then filter out the particles to obtain a modified phase change material for later use.

[0037] (4) Take the following raw materials: 90 parts by weight of calcium sulfosilicate-sulfoaluminate cement, 28 parts by weight of 42.5 ordinary Portland cement, 260 parts by weight of crushed stone coarse aggregate, 150 parts by weight of river sand fine aggregate, 40 parts by weight of the modified phase change material of this embodiment, 55 parts by weight of fly ash, 16 parts by weight of polyvinyl alcohol fiber with a length of 20 mm, and 0.2 parts by weight of polycarboxylate water reducer. Add the above raw materials into a mixer and mix for 2 minutes, then add mixing water according to a water-cement ratio of 0.4 and stir for 2 minutes to obtain a cement-based material slurry.

[0038] 1. The cement-based material slurry prepared in this embodiment is poured into a mold, demolded after hardening and forming, and cured to an age of 28 days. Then, the compressive strength of the specimen is tested according to the Standard for Test Methods for Physical and Mechanical Properties of Concrete (GB / T 50081-2019). Figure 2 As shown), the 28d compressive strength was obtained = 46.12MPa.

[0039] 2. Pour the cement-based material slurry prepared in this embodiment into a mold, demold it after hardening and forming, and cure it to an age of 28 days. Then, perform a phase change cycle test on the obtained specimen, that is, place the specimen in an oven at 60°C for 2 hours, then take it out and cool it to room temperature, which is a phase change cycle. Perform 50 phase change cycles in succession according to the above method. Then observe whether there is paraffin frosting on the surface of the specimen, and evaluate whether the modified phase change material has leakage. The results show that there is no paraffin frosting on the surface of the specimen in this embodiment, indicating that the modified phase change material in this embodiment has no leakage.

[0040] 3. The thermal conductivity of the specimens prepared by the cement-based material slurry described in this embodiment was tested using a flat plate thermal conductivity tester according to the "Determination of Steady-State Thermal Resistance and Related Properties of Insulating Materials (Guarded Hot Plate Method)" (GB / T 10294-2008). Figure 3 As shown), the thermal conductivity is obtained as 0.683 W / (m·K).

[0041] Example 2

[0042] A preparation process of a phase-change energy storage high-strength cement-based material, comprising the following steps:

[0043] (1) Paraffin is heated to 60°C to form a melt, and then the components are mixed in a ratio of waste red brick powder (fineness 10 mesh), magnesium phosphate cement, sodium alginate powder, iron powder (fineness 350 mesh), and melt = 4 parts by weight: 2 parts by weight: 1 part by weight: 2.2 parts by weight: 8 parts by weight, and stirred for 3 minutes. After completion, the mixture is cooled to room temperature, and the obtained solid mixture is crushed and sieved to obtain precursor particles with a particle size of 1-2 mm for later use.

[0044] (2) The precursor particles are placed in an ethanol aqueous solution containing calcium chloride, the ratio of the precursor particles to the ethanol aqueous solution is 1g:10ml, the mass fraction of calcium chloride in the ethanol aqueous solution is 4%, and the mass fraction of the ethanol aqueous solution is 75%. Then stir at a rate of 10r / min for 30min, filter out the particles after completion, and naturally dry for 1 hour to obtain pretreated particles for standby use.

[0045] (3) Mix 35g of zinc oxide, 70g of nitric acid, 30g of phosphoric acid, 20g of nano-silicon dioxide, 0.5g of sodium fluoroborate, 1.5g of copper nitrate, 20g of ethylenediaminetetraacetic acid, and 1000ml of water, and stir evenly to obtain a phosphating solution. Then heat to 45°C, place the pretreated particles in the phosphating solution (the ratio of the two is 1g:10ml), stir and let stand for 15 minutes, then filter out the particles to obtain a modified phase change material for later use.

[0046] (4) Take the following raw materials: 80 parts by weight of calcium sulfosilicate-sulfoaluminate cement, 20 parts by weight of 42.5 ordinary Portland cement, 230 parts by weight of crushed stone coarse aggregate, 145 parts by weight of river sand fine aggregate, 30 parts by weight of the modified phase change material of this embodiment, 40 parts by weight of fly ash, 15 parts by weight of polyethylene fiber with a length of 25 mm, and 0.25 parts by weight of sodium lignin sulfonate water reducer. Add the above raw materials into a mixer and mix for 2 minutes, then add mixing water according to a water-cement ratio of 0.44 and stir for 2 minutes to obtain a cement-based material slurry.

[0047] The same method as in Example 1 was used to test the 28d compressive strength, leakage, and thermal conductivity of the test piece made of the cement-based material slurry of this embodiment. The compressive strength was 43.87 MPa, and there was no leakage of the modified phase change material. The thermal conductivity was 0.625 W / (m·K).

[0048] Example 3

[0049] A preparation process of a phase-change energy storage high-strength cement-based material, comprising the following steps:

[0050] (1) Paraffin is heated to 60° C. to form a melt, and then the components are mixed in a ratio of waste red brick powder (fineness 30 mesh), magnesium phosphate cement, sodium alginate powder, iron powder (fineness 400 mesh), and melt = 7 parts by weight: 3 parts by weight: 1.25 parts by weight: 2.8 parts by weight: 10 parts by weight, and stirred for 3 minutes. After completion, the mixture is cooled to room temperature, and the obtained solid mixture is crushed and sieved to obtain precursor particles with a particle size of 1 to 3 mm for later use.

[0051] (2) The precursor particles are placed in a methanol aqueous solution containing calcium chloride, the ratio of the precursor particles to the methanol aqueous solution is 1g:50ml, the mass fraction of calcium chloride in the methanol aqueous solution is 2%, and the mass fraction of the methanol aqueous solution is 70%. Then stir at a rate of 10r / min for 40min, filter out the particles after completion, and naturally dry for 1 hour to obtain pretreated particles for use.

[0052] (3) Mix 20g of zinc oxide, 50g of nitric acid, 20g of phosphoric acid, 10g of nano-silicon dioxide, 0.15g of sodium fluoroborate, 0.5g of copper nitrate, 15g of ethylenediaminetetraacetic acid, and 800ml of water, and stir evenly to obtain a phosphating solution. Then heat to 45°C, place the pretreated particles in the phosphating solution (the ratio of the two is 1g:20ml), stir and let stand for 30 minutes, then filter out the particles to obtain a modified phase change material for standby use.

[0053] (4) Take the following raw materials: 100 parts by weight of calcium sulfosilicate-sulfoaluminate cement, 35 parts by weight of 42.5 ordinary Portland cement, 300 parts by weight of crushed stone coarse aggregate, 160 parts by weight of river sand fine aggregate, 50 parts by weight of the modified phase change material of this embodiment, 65 parts by weight of fly ash, 23 parts by weight of polypropylene fiber with a length of 10 mm, and 0.15 parts by weight of naphthalene-based water reducer. Add the above raw materials into a mixer and mix for 2 minutes, then add mixing water according to a water-cement ratio of 0.38 and stir for 2 minutes to obtain a cement-based material slurry.

[0054] The same method as in Example 1 was used to test the 28d compressive strength, leakage, and thermal conductivity of the test piece made of the cement-based material slurry of this embodiment. The compressive strength was 45.04 MPa, and there was no leakage of the modified phase change material. The thermal conductivity was 0.667 W / (m·K).

[0055] Example 4

[0056] A preparation process for a phase-change energy storage high-strength cement-based material. Compared with the above-mentioned Example 1, the precursor particles of this example are prepared by the following method: paraffin is heated to 60°C to form a molten liquid, and then the components are mixed in a ratio of waste red brick powder (fineness 20 mesh), sodium alginate powder, iron powder (fineness 300 mesh), and molten liquid = 5 parts by weight: 1.1 parts by weight: 2.5 parts by weight: 10 parts by weight, and stirred for 3 minutes. After completion, the mixture is cooled to room temperature, and the obtained solid mixture is crushed and sieved to obtain precursor particles with a particle size of 1~2 mm.

[0057] The same method as in Example 1 was used to test the 28d compressive strength, leakage, and thermal conductivity of the specimens made of the cement-based material slurry of this embodiment. The compressive strength was 38.21 MPa, and paraffin frosting appeared on the surface of the specimen, indicating that the modified phase change material of this embodiment had leakage. The thermal conductivity was 0.841 W / (m·K).

[0058] Example 5

[0059] A preparation process for a phase-change energy storage high-strength cement-based material. Compared with the above-mentioned Example 1, the precursor particles of this example are prepared by the following method: paraffin is heated to 60°C to form a molten liquid, and then the components are mixed in a ratio of magnesium phosphate cement, sodium alginate powder, iron powder (fineness 300 mesh), and molten liquid = 2.4 parts by weight: 1.1 parts by weight: 2.5 parts by weight: 10 parts by weight, and stirred for 3 minutes. After completion, the mixture is cooled to room temperature, and the obtained solid mixture is crushed and sieved to obtain precursor particles with a particle size of 1~2 mm.

[0060] The same method as in Example 1 was used to test the 28d compressive strength, leakage, and thermal conductivity of the test piece made of the cement-based material slurry of this embodiment. The compressive strength was 41.36 MPa, and there was no leakage of the modified phase change material. The thermal conductivity was 0.733 W / (m·K).

[0061] Example 6

[0062] A preparation process for a phase-change energy storage high-strength cement-based material. Compared with the above-mentioned Example 2, the precursor particles of this example are prepared by the following method: paraffin is heated to 60°C to form a molten liquid, and then the components are mixed in a ratio of waste red brick powder (fineness 10 mesh), magnesium phosphate cement, iron powder (fineness 350 mesh), and molten liquid = 4 parts by weight: 2 parts by weight: 2.2 parts by weight: 8 parts by weight, and stirred for 3 minutes. After completion, the mixture is cooled to room temperature, and the obtained solid mixture is crushed and sieved to obtain precursor particles with a particle size of 1~2 mm.

[0063] The same method as in Example 1 was used to test the 28d compressive strength, leakage, and thermal conductivity of the specimens made of the cement-based material slurry of this embodiment. The compressive strength was 44.09 MPa, and paraffin frosting appeared on the surface of the specimen, indicating that the modified phase change material of this embodiment had leakage. The thermal conductivity was 0.816 W / (m·K).

[0064] Example 7

[0065] A preparation process of a phase-change energy storage high-strength cement-based material, comprising the following steps:

[0066] Take the following raw materials: 100 parts by weight of calcium sulfosilicate-sulfoaluminate cement, 35 parts by weight of 42.5 ordinary Portland cement, 300 parts by weight of crushed stone coarse aggregate, 160 parts by weight of river sand fine aggregate, 50 parts by weight of the pretreated particles prepared in Example 3, 65 parts by weight of fly ash, 23 parts by weight of polypropylene fiber with a length of 10 mm, and 0.15 parts by weight of naphthalene-based water reducer. Add the above raw materials to a mixer and mix for 2 minutes, then add mixing water according to a water-cement ratio of 0.38 and stir for 2 minutes to obtain a cement-based material slurry.

[0067] The same method as in Example 1 was used to test the 28d compressive strength, leakage, and thermal conductivity of the specimens made of the cement-based material slurry of this embodiment. The compressive strength was 44.72 MPa, and paraffin frosting appeared on the surface of the specimen, indicating that the modified phase change material of this embodiment had leakage. The thermal conductivity was 0.923 W / (m·K).

[0068] Example 8

[0069] A preparation process for a phase-change energy storage high-strength cement-based material. Compared with the above-mentioned Example 2, the precursor particles of this example are prepared by the following method: paraffin is heated to 60°C to form a molten liquid, and then the components are mixed in a ratio of waste red brick powder (fineness 10 mesh), magnesium phosphate cement, sodium alginate powder, and molten liquid = 4 parts by weight: 2 parts by weight: 1 part by weight: 8 parts by weight, and stirred for 3 minutes. After completion, the mixture is cooled to room temperature, and the obtained solid mixture is crushed and sieved to obtain precursor particles with a particle size of 1~2 mm.

[0070] The same method as in Example 1 was used to test the 28d compressive strength, leakage, and thermal conductivity of the specimens made of the cement-based material slurry of this embodiment. The compressive strength was 43.18 MPa, and paraffin frosting appeared on the surface of the specimen, indicating that the modified phase change material of this embodiment had leakage. The thermal conductivity was 0.892 W / (m·K).

[0071] Example 9

[0072] A preparation process of a phase-change energy storage high-strength cement-based material. Compared with the above-mentioned embodiment 1, the modified phase-change material of this embodiment is prepared by the following method: 25g zinc oxide, 60g nitric acid, 22g phosphoric acid, 0.2g sodium fluoroborate, 1.0g copper nitrate, 17g ethylenediaminetetraacetic acid, and 900ml of clean water are mixed and stirred evenly to obtain a phosphating solution. Then, the mixture is heated to 45°C, and the pretreated particles prepared according to the method of embodiment 1 are placed in the phosphating solution (the ratio of the two is 1g:10ml), stirred and then allowed to stand for 20 minutes, and then the particles are filtered out to obtain a modified phase-change material.

[0073] The same method as in Example 1 was used to test the 28d compressive strength, leakage, and thermal conductivity of the test piece made of the cement-based material slurry of this embodiment. The compressive strength was 40.66 MPa, and there was no leakage of the modified phase change material. The thermal conductivity was 0.703 W / (m·K).

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A preparation process of phase change energy storage high-strength cement-based material, characterized in that: The steps include: (1) Adding red brick powder, magnesium phosphate cement, sodium alginate powder and iron powder to molten paraffin liquid, mixing and cooling, and crushing the obtained solid mixture to obtain precursor particles; (2) placing the precursor particles in a methanol or ethanol aqueous solution containing calcium chloride for stirring, and then drying to obtain pretreated particles; (3) placing the pretreated particles in a phosphating solution containing nano-silicon dioxide, mixing and then allowing to stand, and obtaining a modified phase change material; (4) Calcium sulfosilicate-sulfoaluminate cement, silicate cement, coarse aggregate, fine aggregate, the modified phase change material, fly ash, fiber, and water reducing agent are used as raw materials; the above raw materials are mixed and then mixing water is added and mixed evenly to obtain the cement-based material.

2. The preparation process of phase change energy storage high-strength cement-based material according to claim 1, characterized in that: In step (1), the ratio of the red brick powder, magnesium phosphate cement, sodium alginate powder, iron powder and paraffin liquid is 4-7 parts by weight: 2-3 parts by weight: 1-1.25 parts by weight: 2.2-2.8 parts by weight: 8-10 parts by weight.

3. The preparation process of the phase change energy storage high-strength cement-based material according to claim 1, characterized in that: In step (1), the fineness of the red brick powder is 10-30 mesh; Alternatively, in step (1), the fineness of the iron powder is 300-400 mesh.

4. The preparation process of the phase change energy storage high-strength cement-based material according to claim 1, characterized in that: In step (1), the particle size of the precursor particles is 1-3 mm.

5. The preparation process of phase change energy storage high-strength cement-based material according to claim 1, characterized in that: In step (2), the ratio of the precursor particles to the methanol or ethanol aqueous solution is 1 g: 10-50 ml; Alternatively, in step (2), the mass fraction of calcium chloride in the methanol or ethanol aqueous solution is not less than 2%.

6. The preparation process of phase change energy storage high-strength cement-based material according to claim 1, characterized in that: In step (2), the mass fraction of the methanol or ethanol aqueous solution is 70-80%; or, in step (2), the stirring treatment time is 20-40 minutes.

7. The preparation process of phase change energy storage high-strength cement-based material according to claim 1, characterized in that: In step (3), the ratio of the pretreated particulate matter to the phosphating solution is 1 g: 10-20 ml.

8. The preparation process of phase change energy storage high-strength cement-based material according to claim 1, characterized in that: In step (3), the phosphating solution comprises the following components: 20-35 g zinc oxide, 50-70 g nitric acid, 20-30 g phosphoric acid, 10-20 g nano-silicon dioxide, 0.15-0.5 g sodium fluoroborate, 0.5-1.5 g copper nitrate, 15-20 g ethylenediaminetetraacetic acid, and 800-1000 ml water; or, in step (3), the standing time is 15-30 min.

9. The process for preparing the phase-change energy storage high-strength cement-based material according to any one of claims 1 to 8, characterized in that: The proportions of the components in the raw materials are: 80-100 parts by weight of calcium sulfosilicate-sulfoaluminate cement, 20-35 parts by weight of silicate cement, 230-300 parts by weight of coarse aggregate, 145-160 parts by weight of fine aggregate, 30-50 parts by weight of modified phase change material, 40-65 parts by weight of fly ash, 15-23 parts by weight of fiber, and 0.15-0.25 parts by weight of water reducer; or, in step (4), the mixing water is added according to a water-cement ratio of 0.38-0.

44.

10. The process for preparing the phase change energy storage high-strength cement-based material according to any one of claims 1 to 8, characterized in that: In step (4), the fiber includes at least one of polyethylene fiber, polypropylene fiber, and polyvinyl alcohol fiber; Alternatively, in step (4), the length of the fiber is 10 to 25 mm; Alternatively, in step (4), the water reducer includes any one of a polycarboxylate water reducer, a naphthalene-based water reducer, and a lignin sulfonate water reducer.

Citation Information

Cited By

  • Low-grade diatomite-based non-sintering phase change aggregate and preparation method thereof

    CN122878055A