Preparation method of spherical TATB / TKX-50 compound

The problem of uneven complex and poor dispersion in the preparation of spherical composite explosives was solved by ultrasonic method, and high compaction density and high compaction density were achieved The spherical TATB/TKX-50 complex with good diffusion reduces the sensitivity of TKX-50 and improves the overall performance.

CN118894752AActive Publication Date: 2024-11-05SOUTHWEAT UNIV OF SCI & TECH +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410892989.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-05
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The prior art has problems such as uneven composite, irregular morphology, unsatisfactory reduction effect and unsafe preparation process when preparing spherical composite explosives, especially it is difficult to achieve effective sphericalization and good diffusion of TATB and TKX-50.

Method used

Ultrasonic method is used to completely dissolve TATB and TKX-50 in a reasonable proportion of solvent mixing, add surfactant to form an emulsion, and prepare spherical composites through extraction, filtration, washing and drying steps, using modified Tween-80 as the surface Active agent to improve particle size distribution and dispersion.

Benefits of technology

The sensitivity of TKX-50 was successfully reduced, the compaction density and diffusion of TATB/TKX-50 composite was improved, the particle size distribution was concentrated, and the rest angle reached 27°, which significantly improved the processing process performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894752A_ABST
    Figure CN118894752A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a spherical TATB / TKX-50 compound, which comprises the following steps: mixing a solvent A and a solvent B, heating and stirring to obtain a TATB / TKX-50 compound solvent; the preparation method comprises the following steps: adding a certain amount of TATB and TKX-50 into a TATB / TKX-50 composite solvent, carrying out ultrasonic treatment, heating to a certain temperature to completely dissolve TATB and TKX-50 as a discontinuous phase, adding a certain amount of a surfactant and a continuous phase reagent into the discontinuous phase, and carrying out rotary oscillation, stirring or ultrasonic treatment to obtain an emulsion; and extracting, filtering, washing and drying to obtain the spherical TATB / TKX-50 compound. The spherical TATB / TKX-50 compound prepared by the method is good in sphericity and high in balling efficiency, the size of the spherical TATB / TKX-50 compound can be regulated and controlled within the range of 30-200 microns, the spherical TATB / TKX-50 compound has good free-running property, the crystal form is not changed, the thermal decomposition performance is improved, the activation energy is reduced, the energy release rate is improved, and the mechanical sensitivity is greatly reduced. In addition, compared with a material mixture, the free-running property and the stacking density are improved to a certain degree, the processing technology performance is improved, and high practicability is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of preparing high-energy insensitive spherical composite energetic materials, and more specifically, the present invention relates to a method for preparing a spherical TATB / TKX-50 composite. Background Art

[0002] Energetic materials play a vital role in weapon systems, and their research and development focus is on high performance and safety. At present, single-element high-energy insensitive materials have faced bottlenecks due to long research and development cycles, high costs, and limited room for performance improvement. In contrast, composite energetic materials have become a research hotspot due to their high energy density, adjustability, and excellent safety. 1,1'-dihydroxy-5,5'-tetrazole-1,1'-dioxohydroxylamine salt (TKX-50), a new type of high-energy compound, is often used in composite materials because of its high detonation velocity and detonation pressure, simple synthesis, and low toxicity. However, this type of high-energy material is often accompanied by a higher sensitivity. The minimum impact energy (BAM sensitivity) of TKX-50 is 5J, and the characteristic drop height H50 is 16.6cm, indicating that its sensitivity still needs to be optimized.

[0003] 1,3,5-Triamino-2,4,6-trinitrobenzene (TATB) is a low-sensitivity energetic material that is extremely insensitive to external stimuli such as heat, light, shock waves, friction and mechanical impact, which allows it to reduce the mechanical sensitivity of energetic materials while still maintaining their energy. Therefore, the application of TATB in composite energetic materials has significant potential. In addition, the sphericalization of explosives can achieve the purpose of reducing the sensitivity of explosives, and also has the advantages of good fluidity, good mechanical properties, large specific surface area and high bulk density. Therefore, the preparation of TATB / TKX-50 spherical high-energy insensitive composite explosive is of great significance for improving its comprehensive performance.

[0004] Although TATB has strong hydrogen bonding and rich hydrogen bonding networks, it is difficult for conventional solvents to destroy it. However, ionic liquids have provided an effective solution to the problem of TATB dissolution difficulties. Hoffman et al. used [Emim]OAc to dissolve TATB, and the solubility reached 9-10 g / 100 g. Fan et al. studied the solubility of TATB in the ionic liquid 1-butyl-3-methylimidazolium acetate at 110 ° C, with a solubility of 2.38 g / 100 g, and prepared TATB particles with an average particle size of 1.48 μm based on this. Qi Xiufang et al. investigated the effect of different ionic liquids and DMSO composite solvents on the solubility of TATB. The results showed that when m (methylimidazolium acetate of butanesulfonic acid) ∶ m (DMSO) was 1 ∶ 4, the composite solvent had the best dissolving ability for TATB, and the solubility reached 0.630 g / 100 g. However, ionic liquids are expensive, which increases the cost. This patent achieves cost control while dissolving TATB by reasonably adjusting the dosage ratio of ionic liquids and other solvents.

[0005] In the preparation of spherical high-energy insensitive composite explosives, Hou Guanchen et al. used nitrocellulose and conductive fillers as raw materials and prepared antistatic nitrocellulose composite materials by solvent-nonsolvent method, which was in the shape of a fibrous conductive network. Jing Suming et al. prepared binary composite crystalline explosive HMX / LLM-105 by solvent-nonsolvent method, which was partially rod-shaped and partially block-shaped, and there was a phenomenon of crystal interpenetration of two shapes. Chen Xing et al. used tetraethyl orthosilicate as a precursor and prepared octogen (HMX)-ammonium perchlorate (AP)-SiO2 nanocomposite energetic materials by sol-gel method, which was in the shape of a nano-mesh structure. Li Yuanyuan et al. prepared spherical CL-20 by ultrasonic dispersion treatment, wet crushing and high shear dispersion emulsification, respectively. The prepared CL-20 had a reduced particle size, a smooth surface and reduced mechanical sensitivity. Liu Chun and others conducted useful attempts and explorations in the preparation of ultrafine explosives using a high-energy ball mill, and obtained submicron ultrafine TATB explosives under optimized conditions.

[0006] The methods for preparing composite explosives reported in these documents have problems such as uneven compounding, irregular composite morphology, and unsatisfactory sensitivity reduction effect. The methods for preparing spherical explosives have problems such as difficulty in compounding two explosives or unsafe preparation processes. There are relatively few methods that can be used to prepare spherical composite explosives. At the same time, the existing mixture obtained by directly physically mixing TATB and TKX-50 has the problem of poor fluidity. Therefore, designing a method that can both sphericalize and realize the composite of the two, and a spherical composite with good fluidity, is an urgent problem to be solved in this field. Summary of the invention

[0007] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0008] In order to achieve these objects and other advantages according to the present invention, a method for preparing a spherical TATB / TKX-50 composite is provided, comprising the following steps:

[0009] Step 1: Mix solvent A and solvent B in a certain proportion, heat and stir to make solvent A and solvent B completely mixed, and obtain TATB / TKX-50 composite solvent;

[0010] Step 2: adding a certain amount of TATB and TKX-50 into a TATB / TKX-50 composite solvent, ultrasonicating and heating to a certain temperature to completely dissolve TATB and TKX-50, as a discontinuous phase, then adding a certain amount of surfactant and continuous phase reagent into the discontinuous phase, vortexing, stirring or ultrasonicating to obtain an emulsion;

[0011] Step 3: extracting, filtering, washing and drying to obtain a spherical TATB / TKX-50 complex.

[0012] Preferably, the solvent A is one or more of methanol, ether, dimethyl sulfoxide, dichloromethane, N,N-dimethylformamide, ethyl acetate, acetone, toluene, xylene, nitrogen-methylpyrrolidone, chloroform, and tetrahydrofuran.

[0013] Preferably, the B solvent is one or more of 1-butyl-3-methylimidazolium chloride, N-methylmorpholine-N-oxide, zinc chloride, ammonium fluoride, 1-allyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium methylphosphonate, 1-ethyl-3-methylimidazolium acetate, 1-alkyl-3-methylimidazolium propionate, 1-alkyl-3-methylimidazolium acetate, 1-alkyl-3-methylimidazolium alanine, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-methyl-3-octylimidazole tetrafluoroborate, and 1-butyl-3-methylimidazolium trifluoromethanesulfonate.

[0014] Preferably, the mass ratio of the solvent A to the solvent B is 1:100 to 100:1.

[0015] Preferably, the surfactant is one or more of gum arabic, shellac, polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate, cetyl pyridine, sodium dodecyl sulfate, sodium cetyl sulfate, sodium octadecyl sulfate, dodecyl dimethyl betaine, sodium dioctane succinate sulfonate, polyvinyl alcohol, polyethylene glycol, alkyl alcohol amide, Span-20 to Span-80, Tween-20 to Tween-80;

[0016] The mass proportion of the surfactant is 0.01% to 5% of the TATB / TKX-50 composite solvent.

[0017] Preferably, the mass ratio of the TATB, TKX-50 and the TATB / TKX-50 composite solvent is 1-10:1-10:100-200.

[0018] Preferably, in the step 2, the temperature for dissolving TATB and TKX-50 is any temperature between 50 and 120°C;

[0019] Cyclotron oscillation or ultrasonic frequency is 10~1000kH Z .

[0020] Preferably, the continuous phase is one or more of n-heptane, cyclohexane, ethyl ether, n-hexane, isooctane, pentane, dipropyl ether, and xylene;

[0021] The volume ratio of the continuous phase to the discontinuous phase is 1:20-20:1.

[0022] Preferably, in step 3, the extraction solvent used for extraction is one of distilled water, anhydrous ethanol, dimethylformamide and methanol;

[0023] The extraction method is a kind of dripping and spraying;

[0024] The reagent used for washing is one of distilled water, anhydrous ethanol and ethyl acetate;

[0025] The drying method is one of room temperature drying, vacuum drying and freeze drying.

[0026] Preferably, the cyclotron oscillation or ultrasonic frequency is used to adjust the size of the emulsion microspheres, and the particle size distribution of the spherical TATB / TKX-50 complex obtained after drying is 100 nm to 200 μm.

[0027] In order to further improve the particle size distribution of the TATB / TKX-50 composite, increase the compaction density and the fluidity of the TATB / TKX-50 composite, modified Tween-80 is used to replace the surfactant in step 2, wherein the modification method of the modified Tween-80 includes:

[0028] Under nitrogen protection, succinic anhydride, xylene and hydroxy silicone oil are added to a flask, the temperature is raised to 100-120°C for reaction for 3-6 hours, and then Tween-80 is added, the temperature is further raised to 200-260°C, and xylene is removed after the reaction to obtain Tween-80 modified with hydroxy silicone oil; wherein the mass ratio of succinic anhydride, xylene, hydroxy silicone oil and Tween-80 is 0.1-3:200-300:0.1-15:80-120;

[0029] A white carbon black suspension with a concentration of 0.01 to 0.5 g / mL is prepared, Tween-80 modified by hydroxy silicone oil is added to the white carbon black suspension, ultrasonically dispersed at a frequency of 50 to 60 kHz for 20 to 40 minutes, allowed to stand for evaporation and concentration, solid-liquid separation, and drying to obtain modified Tween-80; wherein the mass ratio of white carbon black to Tween-80 modified by hydroxy silicone oil is 1 to 10:50 to 250.

[0030] The present invention has at least the following beneficial effects: the present invention compounds TATB and TKX-50 to reduce the sensitivity of TKX-50. The composite of TATB and TKX-50 is sphericalized to further reduce the sensitivity of TKX-50 and improve the comprehensive performance such as processing performance.

[0031] The spherical TATB / TKX-50 complex prepared by the present invention has high compaction density and high fluidity, and the angle of repose can reach 33°. Modified Tween-80 is used as a surfactant, and the modified Tween-80 not only acts as a surface active agent but also has the function of a dispersant to disperse the spherical TATB / TKX-50 complex particles. The obtained spherical TATB / TKX-50 complex particles are more concentrated and uniformly distributed, and the agglomeration between the spherical TATB / TKX-50 complex particles is further reduced. The particle sizes of most spherical TATB / TKX-50 complexes are distributed in the range of 40 to 80 μm, thereby improving the compaction density and fluidity of the spherical TATB / TKX-50 complex, and the angle of repose can reach 27°.

[0032] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a scanning electron microscope image of the spherical TATB / TKX-50 composite prepared in Example 6 of the present invention;

[0034] Figure 2 This is a particle size distribution diagram of the spherical TATB / TKX-50 composite prepared in Example 6 of the present invention;

[0035] Figure 3 This is the XRD pattern of the spherical TATB / TKX-50 composite prepared in Example 6 of the present invention;

[0036] Figure 4 This is the DSC graph of the spherical TATB / TKX-50 complex prepared in Example 6 of the present invention;

[0037] Figure 5This is a test chart of the bulk density and fluidity of the spherical TATB / TKX-50 composite prepared in Example 6 of the present invention. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0039] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0040] Embodiment 1:

[0041] A method for preparing a spherical TATB / TKX-50 complex comprises the following steps:

[0042] Step 1, weigh 10 g of dimethyl sulfoxide (DMSO) and 1-butyl-3-methylimidazolium acetate in a ratio of 4:1, add them into a beaker, heat to 50° C., stir well to dissolve, and cool to room temperature to obtain a TATB / TKX-50 composite solvent;

[0043] Step 2: 0.2 g TKX-50 and 0.1 g TATB were ultrasonically dissolved in 10 g TATB / TKX-50 composite solvent as a discontinuous phase at room temperature, and then 0.024 g Tween-80 was added as a surfactant and 10 mL cyclohexane was added as a discontinuous phase, and cyclotron oscillation was performed at a frequency of 50 kHz to obtain an emulsion system;

[0044] Step 3: Slowly add anhydrous ethanol to the emulsion system in a spraying manner for extraction, so that the ethanol gradually diffuses into the discontinuous phase, and TATB and TKX-50 gradually precipitate in the form of emulsion droplets to form a spherical complex, which is filtered, washed, and dried to obtain the final spherical TATB / TKX-50 complex.

[0045] Embodiment 2:

[0046] A method for preparing a spherical TATB / TKX-50 complex comprises the following steps:

[0047] Step 1, weigh 10 g of dimethyl sulfoxide (DMSO) and 1-butyl-3-methylimidazolium acetate in a ratio of 4:1, add them into a beaker, heat to 50° C., stir well to dissolve, and cool to room temperature to obtain a TATB / TKX-50 composite solvent;

[0048] Step 2: 0.2 g TKX-50 and 0.1 g TATB were ultrasonically dissolved in 10 g TATB / TKX-50 composite solvent as a discontinuous phase at room temperature, and then 0.024 g Tween-80 was added as a surfactant and 10 mL n-heptane was added as a discontinuous phase, and cyclotron oscillation was performed at a frequency of 50 kHz to obtain an emulsion system;

[0049] Step 3: Slowly add anhydrous ethanol to the emulsion system in a spraying manner for extraction, so that the ethanol gradually diffuses into the discontinuous phase, and TATB and TKX-50 gradually precipitate in the form of emulsion droplets to form a spherical complex, which is filtered, washed, and dried to obtain the final spherical TATB / TKX-50 complex.

[0050] Embodiment 3:

[0051] A method for preparing a spherical TATB / TKX-50 complex comprises the following steps:

[0052] Step 1, weigh 10 g of dimethyl sulfoxide (DMSO) and 1-butyl-3-methylimidazolium acetate in a ratio of 5:1, add them into a beaker, heat to 50° C., stir thoroughly to dissolve, and cool to room temperature to obtain a TATB / TKX-50 composite solvent;

[0053] Step 2: 0.2 g TKX-50 and 0.1 g TATB were ultrasonically dissolved in 10 g TATB / TKX-50 composite solvent as a discontinuous phase at room temperature, and then 0.024 g Span-80 was added as a surfactant and 10 mL cyclohexane was added as a discontinuous phase, and the emulsion system was obtained by cyclotron oscillation at a frequency of 50 kHz;

[0054] Step 3: Slowly add anhydrous ethanol to the emulsion system in a spraying manner for extraction, so that the ethanol gradually diffuses into the discontinuous phase, and TATB and TKX-50 gradually precipitate in the form of emulsion droplets to form a spherical complex, which is filtered, washed, and dried to obtain the final spherical TATB / TKX-50 complex.

[0055] Embodiment 4:

[0056] A method for preparing a spherical TATB / TKX-50 complex comprises the following steps:

[0057] Step 1, weigh 10 g of dimethyl sulfoxide (DMSO) and 1-alkyl-3-methylimidazole acetate in a ratio of 4:1, add them into a beaker, heat to 50° C., stir well to dissolve, and cool to room temperature to obtain a TATB / TKX-50 composite solvent;

[0058] Step 2: 0.2 g TKX-50 and 0.1 g TATB were ultrasonically dissolved in 10 g TATB / TKX-50 composite solvent as a discontinuous phase at room temperature, and then 0.03 g Tween-80 was added as a surfactant and 10 mL cyclohexane was added as a discontinuous phase, and cyclotron oscillation was performed at a frequency of 50 kHz to obtain an emulsion system;

[0059] Step 3: Slowly add anhydrous ethanol to the emulsion system in a spraying manner for extraction, so that the ethanol gradually diffuses into the discontinuous phase, and TATB and TKX-50 gradually precipitate in the form of emulsion droplets to form a spherical complex, which is filtered, washed, and dried to obtain the final spherical TATB / TKX-50 complex.

[0060] Embodiment 5:

[0061] A method for preparing a spherical TATB / TKX-50 complex comprises the following steps:

[0062] Step 1, weigh 10 g of dimethyl sulfoxide (DMSO) and 1-butyl-3-methylimidazolium acetate in a ratio of 4:1, add them into a beaker, heat to 50° C., stir well to dissolve, and cool to room temperature to obtain a TATB / TKX-50 composite solvent;

[0063] Step 2: 0.2 g TKX-50 and 0.1 g TATB were ultrasonically dissolved in 10 g TATB / TKX-50 composite solvent as a discontinuous phase at room temperature, and then 0.024 g Tween-80 was added as a surfactant and 15 mL n-heptane was added as a discontinuous phase, and cyclotron oscillation was performed at a frequency of 50 kHz to obtain an emulsion system;

[0064] Step 3: Slowly add anhydrous ethanol to the emulsion system in a spraying manner for extraction, so that the ethanol gradually diffuses into the discontinuous phase, and TATB and TKX-50 gradually precipitate in the form of emulsion droplets to form a spherical complex, which is filtered, washed, and dried to obtain the final spherical TATB / TKX-50 complex.

[0065] Embodiment 6:

[0066] A method for preparing a spherical TATB / TKX-50 complex comprises the following steps:

[0067] Step 1, weigh 10 g of DMSO and 1-alkyl-3-methylimidazolium acetate in a ratio of 4:1, add them into a beaker, heat to 50° C., stir thoroughly to dissolve, and cool to room temperature to obtain a TATB / TKX-50 composite solvent;

[0068] Step 2: 0.2 g TKX-50 and 0.1 g TATB were ultrasonically dissolved in 10 g TATB / TKX-50 composite solvent as a discontinuous phase at room temperature, and then 0.024 g Tween-80 was added as a surfactant and 10 mL cyclohexane was added as a discontinuous phase, and cyclotron oscillation was performed at a frequency of 50 kHz to obtain an emulsion system;

[0069] Step 3: Slowly add anhydrous ethanol to the emulsion system in a spraying manner for extraction, so that the ethanol gradually diffuses into the discontinuous phase, and TATB and TKX-50 gradually precipitate in the form of emulsion droplets to form a spherical complex, which is filtered, washed, and dried to obtain the final spherical TATB / TKX-50 complex.

[0070] The scanning electron microscopy image of the spherical TATB / TKX-50 composite prepared in this example is as follows: Figure 1 As shown, it can be seen that the spherical TATB / TKX-50 composite prepared in this example has distinct particles, and the morphology of the spherical TATB / TKX-50 composite is a regular sphere with good sphericity.

[0071] The particle size distribution of the spherical TATB / TKX-50 composite prepared in this example is shown in FIG. Figure 2 As shown, it can be seen that the sizes of the spherical TATB / TKX-50 composites prepared in this example are mostly distributed between 40 and 80 μm.

[0072] Figure 3 The characteristic diffraction peaks of the raw materials TATB and TKX-50 are all present in the spherical TATB / TKX-50 composite prepared in this example, indicating that the composite is formed by the combination of TATB and TKX-50.

[0073] Figure 4 The spherical TATB / TKX-50 composite prepared in this example exhibits the exothermic peaks of the raw materials TATB and TKX-50, further indicating that the composite is formed by the composite of TATB and TKX-50.

[0074] Depend on Figure 5 It can be concluded that when the mass ratio of TATB to TKX-50 is 1:2, the spherical TATB / TKX-50 composite prepared in this example exhibits better bulk density and fluidity than the physical mixture. Figure 5 As shown, 0.6 g of a mixture obtained by directly mixing TATB and TKX-50 in a mass ratio of 1:2 and 0.6 g of the spherical TATB / TKX-50 composite obtained in this example were placed in test tubes of the same size, respectively, and vibrated and compacted to make the upper surfaces of the mixture and the spherical TATB / TKX-50 composite flat and no longer sinking, and the heights of the mixture and the spherical TATB / TKX-50 composite were measured respectively. Figure 5 It can be seen that the height of the spherical TATB / TKX-50 composite prepared in this example in the test tube is about 1.0 cm, which is significantly lower than the directly physically mixed TATB and TKX-50 mixture, indicating that the spherical TATB / TKX-50 composite prepared in this example has a greater compaction density.

[0075] like Figure 5 As shown, the repose angles of 0.6 g of a directly physically mixed mixture of TATB and TKX-50 and 0.6 g of the shaped TATB / TKX-50 composite prepared in this example were measured using the repose angle method. It can be seen from the figure that the repose angle of the directly physically mixed mixture is 47°, while the repose angle of the shaped TATB / TKX-50 composite prepared in this example is 33°, which is significantly lower than the repose angle of the directly physically mixed mixture. This indicates that the shaped TATB / TKX-50 composite prepared in this example has higher fluidity.

[0076] Embodiment 7:

[0077] A method for preparing a spherical TATB / TKX-50 complex comprises the following steps:

[0078] Step 1, weigh 10 g of DMSO and 1-butyl-3-methylimidazolium acetate in a ratio of 4:1, add them into a beaker, heat to 50° C., stir thoroughly to dissolve, and cool to room temperature to obtain a TATB / TKX-50 composite solvent;

[0079] Step 2: 0.2 g TKX-50 and 0.1 g TATB were ultrasonically dissolved in 10 g TATB / TKX-50 composite solvent as a discontinuous phase at room temperature, and then 0.024 g Tween-80 was added as a surfactant and 10 mL cyclohexane was added as a discontinuous phase, and cyclotron oscillation was performed at a frequency of 50 kHz to obtain an emulsion system;

[0080] Step 3: Slowly add anhydrous ethanol to the emulsion system by direct dropwise addition for extraction, so that the ethanol gradually diffuses into the discontinuous phase, and TATB and TKX-50 gradually precipitate in the form of emulsion droplets to form a spherical complex, which is filtered, washed, and dried to obtain the final spherical TATB / TKX-50 complex.

[0081] Embodiment 8:

[0082] A method for preparing a spherical TATB / TKX-50 complex comprises the following steps:

[0083] Step 1, weigh 10 g of DMSO and 1-butyl-3-methylimidazolium acetate in a ratio of 4:1, add them into a beaker, heat to 50° C., stir thoroughly to dissolve, and cool to room temperature to obtain a TATB / TKX-50 composite solvent;

[0084] Step 2: 0.2 g TKX-50 and 0.1 g TATB were ultrasonically dissolved in 10 g TATB / TKX-50 composite solvent as a discontinuous phase at room temperature, and then 0.024 g Tween-80 was added as a surfactant and 15 mL cyclohexane was added as a discontinuous phase, and an emulsion system was obtained by vibrating ultrasound at a frequency of 50 kHz;

[0085] Step 3: Slowly add deionized water to the emulsion system by direct dropwise addition for extraction, so that ethanol gradually diffuses into the discontinuous phase, and TATB and TKX-50 gradually precipitate in the form of emulsion droplets to form a spherical complex, which is filtered, washed, and dried to obtain the final spherical TATB / TKX-50 complex.

[0086] Embodiment 9:

[0087] A method for preparing a spherical TATB / TKX-50 complex comprises the following steps:

[0088] Step 1, weigh 10 g of DMSO and 1-alkyl-3-methylimidazolium acetate in a ratio of 4:1, add them into a beaker, heat to 50° C., stir thoroughly to dissolve, and cool to room temperature to obtain a TATB / TKX-50 composite solvent;

[0089] Step 2: 0.2 g TKX-50 and 0.1 g TATB were ultrasonically dissolved in 10 g TATB / TKX-50 composite solvent as a discontinuous phase at room temperature, and then 0.024 g Tween-80 was added as a surfactant and 10 mL cyclohexane was added as a discontinuous phase, and cyclotron oscillation was performed at a frequency of 50 kHz to obtain an emulsion system;

[0090] Step 3: Slowly add deionized water to the emulsion system in a spraying manner for extraction, so that ethanol gradually diffuses into the discontinuous phase, and TATB and TKX-50 gradually precipitate in the form of emulsion droplets to form a spherical complex, which is filtered, washed, and dried to obtain the final spherical TATB / TKX-50 complex.

[0091] Example 10

[0092] This embodiment provides a method for preparing a spherical TATB / TKX-50 complex, which is different from that of Example 6 in that modified Tween-80 is used to replace Tween-80 in step 2, and the rest of the process is the same as that of Example 6; wherein the modification method of modified Tween-80 includes:

[0093] Under nitrogen protection, 1 g of succinic anhydride, 200 g of xylene, and 2 g of hydroxy silicone oil were added to the flask, the temperature was raised to 120°C for reaction for 6 h, and then 100 g of Tween-80 was added, and the temperature was continued to rise to 260°C. After the reaction, xylene was removed to obtain Tween-80 modified with hydroxy silicone oil;

[0094] 1200 mL of a white carbon black suspension with a concentration of 0.01 g / mL was prepared, 120 g of Tween-80 modified with hydroxy silicone oil was added to the white carbon black suspension, ultrasonically dispersed at a frequency of 60 kHz for 40 min, allowed to stand, evaporated and concentrated, solid-liquid separated, washed, and dried to obtain modified Tween-80.

[0095] According to the method of Example 6, the compaction density and repose angle of 0.6 g of the TATB / TKX-50 composite sample prepared in this example were measured, and the compaction height of 0.6 g of the TATB / TKX-50 composite sample in the test tube was measured to be 0.84 cm, which was significantly lower than 1.0 cm in Example 6, indicating that the particle size distribution of the TATB / TKX-50 composite prepared in this example was more uniform and had a larger compaction density; and the repose angle of the TATB / TKX-50 composite sample prepared in this example was 27°, which was significantly lower than 33° in Example 6, indicating that the TATB / TKX-50 composite prepared in this example had better fluidity.

[0096] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.

[0097] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for preparing a spherical TATB / TKX-50 complex, characterized in that: The following steps are involved: Step 1: Mix solvent A and solvent B in a certain proportion, heat and stir to make solvent A and solvent B completely mixed, and obtain TATB / TKX-50 composite solvent; Step 2: adding a certain amount of TATB and TKX-50 into a TATB / TKX-50 composite solvent, ultrasonicating and heating to a certain temperature to completely dissolve TATB and TKX-50, as a discontinuous phase, then adding a certain amount of surfactant and continuous phase reagent into the discontinuous phase, vortexing, stirring or ultrasonicating to obtain an emulsion; Step 3: extracting, filtering, washing and drying to obtain a spherical TATB / TKX-50 complex.

2. The method for preparing the spherical TATB / TKX-50 complex according to claim 1, characterized in that: The solvent A is one or more of methanol, ether, dimethyl sulfoxide, dichloromethane, N,N-dimethylformamide, ethyl acetate, acetone, toluene, xylene, nitrogen-methylpyrrolidone, chloroform, and tetrahydrofuran.

3. The method for preparing the spherical TATB / TKX-50 complex according to claim 1, characterized in that: The B solvent is one or more of 1-butyl-3-methylimidazolium chloride, N-methylmorpholine-N-oxide, zinc chloride, ammonium fluoride, 1-allyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium methylphosphonate, 1-ethyl-3-methylimidazolium acetate, 1-alkyl-3-methylimidazolium propionate, 1-alkyl-3-methylimidazolium acetate, 1-alkyl-3-methylimidazolium alanine, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-methyl-3-octylimidazole tetrafluoroborate, and 1-butyl-3-methylimidazolium trifluoromethanesulfonate.

4. The method for preparing the spherical TATB / TKX-50 complex according to claim 1, characterized in that: The mass ratio of the A solvent to the B solvent is 1:100 to 100:

1.

5. The method for preparing the spherical TATB / TKX-50 complex according to claim 1, characterized in that: The surfactant is one or more of gum arabic, shellac, polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate, cetyl pyridine, sodium dodecyl sulfate, sodium cetyl sulfate, sodium octadecyl sulfate, dodecyl dimethyl betaine, sodium dioctane succinate sulfonate, polyvinyl alcohol, polyethylene glycol, alkyl alcohol amide, Span-20 to Span-80, Tween-20 to Tween-80; The mass proportion of the surfactant is 0.01% to 5% of the TATB / TKX-50 composite solvent.

6. The method for preparing the spherical TATB / TKX-50 complex according to claim 1, characterized in that: The mass ratio of the TATB, TKX-50 and the TATB / TKX-50 composite solvent is 1-10:1-10:100-200.

7. The method for preparing the spherical TATB / TKX-50 complex according to claim 1, characterized in that: In the step 2, the temperature for dissolving TATB and TKX-50 is any temperature between 50 and 120°C; Cyclotron oscillation or ultrasonic frequency is 10~1000kH Z .

8. The method for preparing the spherical TATB / TKX-50 complex according to claim 1, characterized in that: The continuous phase is one or more of n-heptane, cyclohexane, ethyl ether, n-hexane, isooctane, pentane, dipropyl ether, and xylene; The volume ratio of the continuous phase to the discontinuous phase is 1:20-20:

1.

9. The method for preparing the spherical TATB / TKX-50 complex according to claim 1, characterized in that: In the step 3, the extraction solvent used for extraction is one of distilled water, anhydrous ethanol, dimethylformamide and methanol; The extraction method is a kind of dripping and spraying; The reagent used for washing is one of distilled water, anhydrous ethanol and ethyl acetate; The drying method is one of room temperature drying, vacuum drying and freeze drying.

10. The method for preparing the spherical TATB / TKX-50 complex according to claim 1, characterized in that: The cyclotron oscillation or ultrasonic frequency is used to adjust the size of the emulsion microspheres, and the particle size distribution of the spherical TATB / TKX-50 complex obtained after drying is 30nm-200μm.

Citation Information

Patent Citations

  • Method for preparing spherical organic micro-molecular monomer or compound through emulsion technology

    CN106748584A

  • Method for adjusting oxygen balance of energy-containing material based on emulsion method

    CN107473911A

  • Explosive material nanowire and preparation method thereof

    CN108164375A

  • Porous TATB explosive spherocrystal and preparation method thereof

    CN114456019A

  • Method for adjusting oxygen balance of TKX-50 based on oil-in-oil technology

    CN117776826A