Core-shell structure conductive microsphere with amino cross-linked polymer microsphere as core and preparation method of core-shell structure conductive microsphere

By amination and in-situ reduction of chloromethylstyrene microspheres, core-shell conductive microspheres with high stability and good tolerance to organic solvents were prepared, solving the safety hazards and poor stability problems in traditional processes and improving the uniformity and stability of conductive microspheres.

CN118894954APending Publication Date: 2024-11-05ZHEJIANG FULAI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410935406.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional conductive microsphere preparation processes pose safety risks, and the lack of cross-linking of polymer chains leads to poor stability and insufficient tolerance to organic solvents, affecting the uniformity and stability of the conductive microspheres.

Method used

Alkyl diamine was used to amination chloromethylstyrene microspheres, introducing amino groups and performing partial crosslinking. Combined with in-situ reduction, palladium nanoparticles were prepared to activate the polymer microspheres. A uniform and dense conductive metal layer was then prepared by chemical plating.

Benefits of technology

The stability and tolerance to organic solvents of conductive microspheres were improved, and uniform and dense core-shell structured polymer conductive microspheres were prepared, which are suitable for high-performance anisotropic conductive films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894954A_ABST
    Figure CN118894954A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of conductive materials, and particularly relates to a core-shell structure conductive microsphere with an amino cross-linked polymer microsphere as a core and a preparation method of the core-shell structure conductive microsphere. The preparation method comprises the following steps: preparing polymer microsphere seeds by taking vinylbenzyl chloride as a monomer, realizing surface amination of polymer microspheres through an alkyl diamine reagent, then introducing Pd < 2 + > ions through coordination, and further uniformly coating the surfaces of the polymer microspheres with palladium nanoparticles through in-situ reduction to complete activation of the polymer microspheres, so as to obtain the palladium-loaded polymer microspheres. And finally, preparing the core-shell structure polymer conductive microsphere with a uniform and compact metal coating through a chemical plating process, wherein the core-shell structure polymer conductive microsphere is applied to preparation of a high-performance anisotropic conductive film. Through surface amination of the polymer microspheres, the use of a dangerous concentrated sulfuric acid reagent can be avoided, and the surface activation of the polymer microspheres can be efficiently and conveniently realized by utilizing a coordination-reduction strategy; meanwhile, through amination of alkyl diamine, partial crosslinking of the surfaces of the polymer microspheres can be achieved, and the polymer microspheres which are higher in stability and insoluble in organic solvents are prepared. The preparation method of the conductive microspheres has the advantages of being wide in raw material source, simple and convenient to operate and more uniform and compact in metal coating, and is suitable for industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive materials, and in particular relates to a method for preparing and activating amino-crosslinked polymer microspheres, and also relates to a method for preparing core-shell structured polymer conductive microspheres. Background Art

[0002] In the preparation process of traditional conductive microspheres, it is usually necessary to go through processes such as roughening, sensitization, activation and chemical plating. However, when the polymer microspheres are roughened, concentrated sulfuric acid is usually used for surface sulfonation under ultrasonic conditions, and a large amount of water is added after the reaction for dilution and centrifugal washing. Since the use of concentrated sulfuric acid will bring a lot of safety hazards, it is necessary to choose a safer and more convenient method for microsphere surface functionalization. In addition, in the polymer microspheres prepared with styrene as a monomer, the polymer chains are not cross-linked with each other, resulting in the lack of tolerance of the conductive microspheres prepared subsequently to organic solvents, thereby affecting the stability of the conductive microspheres. The preparation of ACF glue requires the conductive microspheres to be dispersed in organic solvents such as ethyl acetate, so the tolerance of the conductive microspheres to solvents is very important. However, when divinylbenzene is added for cross-linking, the polymerization activity of divinylbenzene is significantly higher than that of styrene, resulting in the widening of the size of the polymer microspheres and the obvious uneven morphology of the microspheres. Summary of the invention

[0003] In order to overcome the deficiencies of the prior art, the present invention provides a method for synthesizing and activating amino-crosslinked polymer microspheres and preparing core-shell structured polymer conductive microspheres.

[0004] The surface modification method of the present invention uses alkyl diamine to aminize chloromethyl styrene microspheres, which can not only introduce amino groups with coordination ability on the microsphere surface, but also realize partial cross-linking on the surface of the polymer microsphere. Since the two ends of the partial alkyl diamine can react with two chloromethyl groups to form quaternary ammonium salts, the polymer chains on the surface of the microsphere are cross-linked to form a network, thereby significantly improving the tolerance and stability of the polymer microsphere to solvents. Since the amino groups can coordinate with transition metal ions, polymer microspheres coated with palladium nanoparticles on the surface are prepared by in-situ reduction, activation of the polymer microspheres is realized, and conductive microspheres with uniform and dense conductive layers are prepared in subsequent chemical plating.

[0005] After surface metal functionalization, polymer microspheres can be used to prepare anisotropic conductive film (ACF). In order to solve the problem that uniform and dense conductive microspheres are difficult to prepare and have poor stability, we prepared core-shell composite conductive microspheres suitable for ACF by amination, coordination, activation and chemical plating of the surface of chloromethylstyrene microspheres, with amino-crosslinked polymer microspheres as the core and uniform and dense conductive metal as the shell.

[0006] To achieve the above purpose, the specific technical solutions adopted by the present invention are as follows:

[0007] In a first aspect, the present invention provides a method for preparing a core-shell structured conductive microsphere with an amino-crosslinked polymer microsphere as a core, comprising the following steps:

[0008] Step (1), adding chloromethylstyrene monomer, initiator and stabilizer into ethanol, heating and reacting for a period of time under nitrogen atmosphere, centrifuging and washing after the reaction, to obtain polymer microsphere seeds with chloromethyl functionalization on the surface;

[0009] Step (2), dispersing the polymer microsphere seeds in ethanol, adding alkyl diamine, mixing evenly and heating to react for a period of time, centrifuging and washing after the reaction to obtain aminated polymer microspheres;

[0010] Step (3), adding the aminated polymer microspheres to an ethanol solution of sodium tetrachloropalladate, stirring for a certain period of time, and centrifuging and washing to obtain a microsphere having Pd on the surface. 2+ Polymer microspheres after ion coordination;

[0011] Step (4), Pd 2+ The coordinated polymer microspheres are added to a sodium borohydride aqueous solution for in-situ reduction to obtain polymer microspheres coated with palladium nanoparticles, thereby achieving surface activation of the microspheres;

[0012] Step (5), chemically plating the polymer microspheres to deposit a conductive metal layer on the surface of the microspheres under ultrasonic conditions to obtain core-shell structured polymer conductive microspheres.

[0013] Preferably, in step (1), the initiator is selected from one or more of AIBN, AIBMe, and BPO; more preferably, AIBMe has good solubility in ethanol and the prepared polymer microspheres are more uniform; the stabilizer is PVP; the reaction temperature is 60-75°C; and the reaction time is 2-10h.

[0014] Preferably, in step (2), the alkyl diamine is selected from one or more of ethylene diamine, propylene diamine, butyl diamine, and hexyl diamine; the reaction temperature is 40-70° C.; the reaction time is 4-18 h; and the volume percentage of the alkyl diamine is 0.5-5% based on the reaction system.

[0015] Preferably, in step (3), the concentration of sodium tetrachloropalladate is 10-50 mM, and the stirring time is 5-20 min.

[0016] Preferably, in step (4), the concentration of the sodium borohydride solution is 10-200 mM; and the in situ reduction reaction time is 5-30 min.

[0017] Preferably, in step (5), the conductive metal layer is a nickel layer; the chemical plating solution for depositing the conductive metal layer is a mixture of a metal salt, a chelating agent and a reducing agent; the conductive metal layer is deposited by a chemical deposition method, the chemical deposition temperature is room temperature, the reaction conditions are ultrasound; and the chemical deposition time is 0.5-2h.

[0018] In a second aspect, the present invention also provides a core-shell structured polymer conductive microsphere, which is prepared by the preparation method as described above. The core-shell structured polymer conductive microsphere is a composite microsphere with a polymer microsphere as the core and a conductive metal layer deposited on the surface of the polymer microsphere as the shell.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention provides a method for synthesizing and activating amine-crosslinked polymer microspheres. The prepared composite conductive microspheres have the characteristics of uniform and dense conductive layer and high stability, and overcome the defects of complicated and dangerous roughening process and low environmental tolerance of conductive microspheres in the preparation of traditional conductive microspheres. The method is simple to operate, low in cost, and has a uniform and dense metal coating, which is suitable for large-scale production. With the amine-crosslinked polymer microspheres as the core and the conductive metal layer as the shell, core-shell structured polymer conductive microspheres with uniform and dense conductive layer and high stability can be prepared, thereby obtaining a high-performance anisotropic conductive adhesive film. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a SEM photograph of the chloromethyl functionalized polymer microsphere seeds in Example 1 of the present invention.

[0022] Figure 2 This is a SEM photograph of the polymer microspheres after amination in Example 1 of the present invention.

[0023] Figure 3 These are photos of the microspheres dispersed in DMF solvent before and after amination in Example 1 of the present invention.

[0024] Figure 4 These are SEM photos of the aminated polymer microspheres in Example 1 of the present invention before and after being immersed in DMF.

[0025] Figure 5 The polymer microsphere Pd in ​​Example 1 of the present invention 2+ SEM photo after coordination.

[0026] Figure 6 This is a SEM photograph of the polymer microspheres after palladium reduction in Example 1 of the present invention.

[0027] Figure 7 This is a SEM photograph of the core-shell polymer composite microspheres aminated with ethylenediamine after nickel plating in Example 1 of the present invention.

[0028] Figure 8 This is a SEM photograph of the core-shell polymer composite microspheres aminated with propylenediamine after nickel plating in Example 2 of the present invention.

[0029] Fig. 9 This is a SEM photograph of the core-shell polymer composite microspheres aminated with butanediamine after nickel plating in Example 3 of the present invention.

[0030] Fig.10 This is a SEM photograph of the core-shell polymer composite microspheres after nickel plating under alkaline conditions in Comparative Example 1 of the present invention.

[0031] Fig.11 This is a SEM photograph of the core-shell polymer composite microspheres aminated with triethanolamine after nickel plating in Comparative Example 2 of the present invention.

[0032] Fig.12 This is a SEM photograph of the core-shell polymer composite microspheres synthesized under room temperature stirring in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0033] The present invention provides a core-shell structure polymer conductive microsphere, wherein the core-shell structure polymer conductive microsphere comprises a composite microsphere with an amine-crosslinked polymer microsphere as a core and a conductive metal layer deposited on the surface of the polymer microsphere as a shell. In the preparation method of the core-shell structure polymer conductive microsphere provided by the present invention, an alkyl diamine reagent is added in step (2), so that an amino group with coordination ability can be introduced on the surface of the polymer microsphere, and at the same time, partial crosslinking of the surface of the polymer microsphere can be achieved. Compared with the traditional polymer microsphere activation method, not only can the use of the dangerous concentrated sulfuric acid reagent required for the roughening of the traditional microspheres be avoided, but also the activation process of the polymer microspheres can be made simpler, safer, and more convenient to operate, and suitable for large-scale industrial production; at the same time, the conductive microspheres prepared based on the amino-crosslinked polymer microspheres have high stability and higher environmental tolerance.

[0034] The present invention realizes surface functionalization and partial crosslinking of polymer microspheres through amination of alkyl diamine, and prepares core-shell structure polymer composite microspheres with uniform and dense conductive metal layers and high stability. Since the introduced amino groups are evenly distributed on the surface of the microspheres, the palladium nanoparticles on the surface of the microspheres are more evenly distributed during the activation process, thereby making the surface coating of the conductive microspheres more uniform and dense; and the partially crosslinked amine groups can improve the tolerance of the conductive microspheres to organic solvents. Through this process, composite conductive microspheres with uniform and dense surface metal coatings and high stability can be obtained, thereby obtaining high-performance anisotropic conductive adhesive films.

[0035] The technical solution of the present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to these embodiments. Any changes or equivalent substitutions that do not deviate from the concept of the present invention are included in the protection scope of the present invention.

[0036] Embodiment 1:

[0037] This embodiment provides a core-shell structure polymer conductive microsphere and a preparation method thereof. The preparation method comprises the following steps:

[0038] (1) 4 mL of chloromethylstyrene monomer, 300 mg of PVP stabilizer and 60 mg of AIBMe initiator were dispersed in 25 mL of ethanol, heated to 70 °C under a nitrogen atmosphere, reacted for 8 h, and then the product was collected by centrifugation and washed three times with ethanol to obtain chloromethyl functionalized polymer microsphere seeds ( Figure 1 );

[0039] (2) Disperse 1 g of chloromethyl functionalized microsphere seeds in 50 mL of ethanol, add 2 mL of ethylenediamine, mix well, heat to 60 °C, continue to react for 12 h, collect the product by centrifugation, and wash it three times with ethanol to obtain aminated polymer microspheres ( Figure 2 ); The microspheres were immersed in DMF and compared before and after amination. It can be seen that the microspheres were partially cross-linked after amination and were insoluble in DMF ( Figure 3 ); Since the conductive microspheres need to be dispersed in solvents such as acetone when preparing ACF glue, the environmental tolerance of the conductive microspheres is relatively important. The SEM photos further show that the microspheres are not dissolved by DMF after amination ( Figure 4 );

[0040] (3) The aminated polymer microspheres were added to an ethanol solution of sodium tetrachloropalladate (Na2PdCl4 0.5 g / L), stirred for 10 min, centrifuged, and washed three times with ethanol to obtain Pd 2+ Coordinated polymer microspheres ( Figure 5 );

[0041] (4) Pd 2+ The coordinated polymer microspheres were added to a sodium borohydride aqueous solution (NaBH4 2g / L) for in-situ reduction, stirred for 10 min, centrifuged, and then added with deionized water and centrifuged and washed three times to obtain polymer microspheres with palladium nanoparticles uniformly coated on the surface ( Figure 6 ), to achieve activation of polymer microspheres;

[0042] (5) The activated polymer microspheres were placed in 50 mL of chemical plating solution (36 g / L nickel chloride, 32 g / L ammonium chloride, 38 g / L trisodium citrate, 28 g / L sodium acetate, 42 g / L sodium hypophosphite), ultrasonicated for 40 min, centrifuged, and washed three times with deionized water to obtain nickel-plated core-shell structure polymer conductive microspheres 1 ( Figure 7 ), it can be seen that the nickel-plated layer of the conductive microspheres is uniform and dense.

[0043] Embodiment 2:

[0044] This embodiment provides a core-shell structure polymer conductive microsphere and a preparation method thereof. The preparation method comprises the following steps:

[0045] (1) 4 mL of chloromethylstyrene monomer, 300 mg of PVP stabilizer and 60 mg of AIBMe initiator were dispersed in 25 mL of ethanol, heated to 70 °C under a nitrogen atmosphere, reacted for 8 h, and then the product was collected by centrifugation and washed three times with ethanol to obtain chloromethyl functionalized polymer microsphere seeds;

[0046] (2) Disperse 1 g of chloromethyl functionalized microsphere seeds in 50 mL of ethanol, add 2 mL of propylene diamine, mix well, heat to 60 °C, continue to react for 12 h, collect the product by centrifugation, and wash it three times with ethanol to obtain aminated polymer microspheres;

[0047] (3) The aminated polymer microspheres were added to an ethanol solution of sodium tetrachloropalladate (Na2PdCl4 0.5 g / L), stirred for 10 min, centrifuged, and washed three times with ethanol to obtain Pd 2+ Coordinated polymer microspheres;

[0048] (4) Pd 2+ The coordinated polymer microspheres were added to a sodium borohydride aqueous solution (NaBH4 2g / L) for in-situ reduction, stirred for 10 minutes, centrifuged, and then added with deionized water and centrifuged and washed three times to obtain polymer microspheres with palladium nanoparticles uniformly coated on the surface, thereby achieving activation of the polymer microspheres.

[0049] (5) The activated polymer microspheres were placed in 50 mL of chemical plating solution (36 g / L nickel chloride, 32 g / L ammonium chloride, 38 g / L trisodium citrate, 28 g / L sodium acetate, 42 g / L sodium hypophosphite), ultrasonicated for 40 min, centrifuged, and washed three times with deionized water to obtain nickel-plated core-shell structure polymer conductive microspheres 2 ( Figure 8 ), it can be seen that the nickel-plated layer of the conductive microspheres is uniform and dense.

[0050] Embodiment 3:

[0051] This embodiment provides a core-shell structure polymer conductive microsphere and a preparation method thereof. The preparation method comprises the following steps:

[0052] (1) 4 mL of chloromethylstyrene monomer, 300 mg of PVP stabilizer and 60 mg of AIBMe initiator were dispersed in 25 mL of ethanol, heated to 70 °C under a nitrogen atmosphere, reacted for 8 h, and then the product was collected by centrifugation and washed three times with ethanol to obtain chloromethyl functionalized polymer microsphere seeds;

[0053] (2) Disperse 1 g of chloromethyl functionalized microsphere seeds in 50 mL of ethanol, add 2 mL of diaminobutane, mix well, heat to 60 °C, continue the reaction for 12 h, collect the product by centrifugation, and wash it three times with ethanol to obtain aminated polymer microspheres;

[0054] (3) The aminated polymer microspheres were added to an ethanol solution of sodium tetrachloropalladate (Na2PdCl4 0.5 g / L), stirred for 10 min, centrifuged, and washed three times with ethanol to obtain Pd 2+ Coordinated polymer microspheres;

[0055] (4) Pd 2+ The coordinated polymer microspheres were added to a sodium borohydride aqueous solution (NaBH4 2g / L) for in-situ reduction, stirred for 10 minutes, centrifuged, and then added with deionized water and centrifuged and washed three times to obtain polymer microspheres with palladium nanoparticles uniformly coated on the surface, thereby achieving activation of the polymer microspheres.

[0056] (5) The activated polymer microspheres were placed in 50 mL of chemical plating solution (36 g / L nickel chloride, 32 g / L ammonium chloride, 38 g / L trisodium citrate, 28 g / L sodium acetate, 42 g / L sodium hypophosphite), ultrasonicated for 40 min, centrifuged, and washed three times with deionized water to obtain nickel-plated core-shell structure polymer conductive microspheres 3 ( Fig. 9 ), it can be seen that the nickel-plated layer of the conductive microspheres is uniform and dense.

[0057] Comparative Example 1:

[0058] This comparative example provides a core-shell structure polymer conductive microsphere and a preparation method thereof. Compared with the embodiment, the amination conditions are different, that is, amination under alkaline conditions. The preparation method comprises the following steps:

[0059] (1) 4 mL of chloromethylstyrene monomer, 300 mg of PVP stabilizer and 60 mg of AIBMe initiator were dispersed in 25 mL of ethanol, heated to 70 °C under a nitrogen atmosphere, reacted for 8 h, and then the product was collected by centrifugation and washed three times with ethanol to obtain chloromethyl functionalized polymer microsphere seeds;

[0060] (2) Disperse 1 g of chloromethyl functionalized microsphere seeds in 50 mL of sodium hydroxide ethanol solution, add 2 mL of ethylenediamine, mix well and heat to 60 °C, continue the reaction for 12 h, collect the product by centrifugation, and wash it three times with ethanol to obtain aminated polymer microspheres;

[0061] (3) The aminated polymer microspheres were added to an ethanol solution of sodium tetrachloropalladate (Na2PdCl4 0.5 g / L), stirred for 10 min, centrifuged, and washed three times with ethanol to obtain Pd 2+ Coordinated polymer microspheres;

[0062] (4) Pd 2+ The coordinated polymer microspheres were added to a sodium borohydride aqueous solution (NaBH4 2g / L) for in-situ reduction, stirred for 10 minutes, centrifuged, and then added with deionized water and centrifuged and washed three times to obtain polymer microspheres with palladium nanoparticles uniformly coated on the surface, thereby achieving activation of the polymer microspheres.

[0063] (5) The activated polymer microspheres were placed in 50 mL of chemical plating solution (36 g / L nickel chloride, 32 g / L ammonium chloride, 38 g / L trisodium citrate, 28 g / L sodium acetate, 42 g / L sodium hypophosphite), ultrasonicated for 40 min, centrifuged, and washed three times with deionized water to obtain nickel-plated core-shell structure polymer conductive microspheres 4 ( Fig.10 ), it can be seen that the nickel layer plated on the conductive microspheres is of poor quality and a uniform and dense nickel layer cannot be obtained.

[0064] Comparative Example 2:

[0065] This comparative example provides a core-shell structure polymer conductive microsphere and a preparation method thereof. Compared with the embodiment, the amination reagent is different, and triethanolamine is used. The preparation method comprises the following steps:

[0066] (1) 4 mL of chloromethylstyrene monomer, 300 mg of PVP stabilizer and 60 mg of AIBMe initiator were dispersed in 25 mL of ethanol, heated to 70 °C under a nitrogen atmosphere, reacted for 8 h, and then the product was collected by centrifugation and washed three times with ethanol to obtain chloromethyl functionalized polymer microsphere seeds;

[0067] (2) Disperse 1 g of chloromethyl functionalized microsphere seeds in 50 mL of ethanol, add 2 mL of triethanolamine, mix well, heat to 60 °C, continue the reaction for 12 h, collect the product by centrifugation, and wash it three times with ethanol to obtain aminated polymer microspheres;

[0068] (3) The aminated polymer microspheres were added to an ethanol solution of sodium tetrachloropalladate (Na2PdCl4 0.5 g / L), stirred for 10 min, centrifuged, and washed three times with ethanol to obtain Pd 2+ Coordinated polymer microspheres;

[0069] (4) Pd 2+ The coordinated polymer microspheres were added to a sodium borohydride aqueous solution (NaBH4 2g / L) for in-situ reduction, stirred for 10 minutes, centrifuged, and then added with deionized water and centrifuged and washed three times to obtain polymer microspheres with palladium nanoparticles uniformly coated on the surface, thereby achieving activation of the polymer microspheres.

[0070] (5) The activated polymer microspheres were placed in 50 mL of chemical plating solution (36 g / L nickel chloride, 32 g / L ammonium chloride, 38 g / L trisodium citrate, 28 g / L sodium acetate, 42 g / L sodium hypophosphite), ultrasonicated for 40 min, centrifuged, and washed three times with deionized water to obtain nickel-plated core-shell structure polymer conductive microspheres 5 ( Fig.11 ), it can be seen that the conductive microspheres are difficult to be plated with a nickel layer.

[0071] Comparative Example 3:

[0072] This comparative example provides a core-shell structure polymer conductive microsphere and a preparation method thereof. Compared with the embodiment, the chemical deposition reaction conditions of the conductive metal layer are different, and ultrasound is replaced by stirring. The preparation method comprises the following steps:

[0073] (1) 4 mL of chloromethylstyrene monomer, 300 mg of PVP stabilizer and 60 mg of AIBMe initiator were dispersed in 25 mL of ethanol, heated to 70 °C under a nitrogen atmosphere, reacted for 8 h, and then the product was collected by centrifugation and washed three times with ethanol to obtain chloromethyl functionalized polymer microsphere seeds;

[0074] (2) Disperse 1 g of chloromethyl functionalized microsphere seeds in 50 mL of ethanol, add 2 mL of ethylenediamine, mix well, heat to 60 °C, continue the reaction for 12 h, collect the product by centrifugation, and wash it three times with ethanol to obtain aminated polymer microspheres;

[0075] (3) The aminated polymer microspheres were added to an ethanol solution of sodium tetrachloropalladate (Na2PdCl4 0.5 g / L), stirred for 10 min, centrifuged, and washed three times with ethanol to obtain Pd 2+ Coordinated polymer microspheres;

[0076] (4) Pd 2+The coordinated polymer microspheres were added to a sodium borohydride aqueous solution (NaBH4 2g / L) for in-situ reduction, stirred for 10 minutes, centrifuged, and then added with deionized water and centrifuged and washed three times to obtain polymer microspheres with palladium nanoparticles uniformly coated on the surface, thereby achieving activation of the polymer microspheres.

[0077] (5) The activated polymer microspheres were placed in 50 mL of chemical plating solution (36 g / L nickel chloride, 32 g / L ammonium chloride, 38 g / L trisodium citrate, 28 g / L sodium acetate, 42 g / L sodium hypophosphite), stirred at room temperature for 24 h, centrifuged, and washed three times with deionized water to obtain nickel-plated core-shell structure polymer conductive microspheres 6 ( Fig.12 ), it can be seen that the nickel layer plated on the conductive microspheres is of poor quality and a uniform and dense nickel layer cannot be obtained.

[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a core-shell conductive microsphere with an amino-crosslinked polymer microsphere as the core, It is characterized in that The preparation process includes the following steps: Step (1), adding chloromethylstyrene monomer, initiator and stabilizer into ethanol, heating and reacting for a period of time under nitrogen atmosphere, centrifuging and washing after the reaction, to obtain polymer microsphere seeds with chloromethyl functionalization on the surface; Step (2), dispersing the polymer microsphere seeds in ethanol, adding alkyl diamine, mixing evenly and heating to react for a period of time, centrifuging and washing after the reaction to obtain aminated polymer microspheres; Step (3), adding the aminated polymer microspheres to an ethanol solution of sodium tetrachloropalladate, stirring for a certain period of time, and centrifuging and washing to obtain a microsphere having Pd on the surface. 2+ Polymer microspheres after ion coordination; Step (4), Pd 2+ The coordinated polymer microspheres are added to a sodium borohydride aqueous solution for in-situ reduction to obtain polymer microspheres coated with palladium nanoparticles, thereby achieving surface activation of the microspheres; Step (5), chemically plating the polymer microspheres to deposit a conductive metal layer on the surface of the microspheres under ultrasonic conditions to obtain core-shell structured polymer conductive microspheres.

2. The preparation method according to claim 1, It is characterized in that In step (1), the initiator is selected from one or more of AIBN, AIBMe, and BPO; the stabilizer is PVP; the reaction temperature is 60-75° C.; and the reaction time is 2-10 h.

3. The preparation method according to claim 2, It is characterized in that In step (1), the initiator is AIBMe.

4. The preparation method according to claim 1, It is characterized in that In step (2), the alkyl diamine is selected from one or more of ethylene diamine, propylene diamine, butyl diamine, and hexamethylene diamine; the reaction temperature is 40-70° C.; the reaction time is 4-18 hours; and the volume percentage of the alkyl diamine is 0.5-5% based on the reaction system.

5. The preparation method according to claim 1, It is characterized in that In step (3), the concentration of sodium tetrachloropalladate is 10-50 mM, and the stirring time is 5-20 min.

6. The preparation method according to claim 1, It is characterized in that In step (4), the concentration of the sodium borohydride solution is 10-200 mM; and the in-situ reduction reaction time is 5-30 min.

7. The preparation method according to claim 1, It is characterized in that In step (5), the conductive metal layer is a nickel layer; the chemical plating solution for depositing the conductive metal layer is a mixture of a metal salt, a chelating agent and a reducing agent; the conductive metal layer is deposited by a chemical deposition method, the chemical deposition temperature is room temperature, the reaction conditions are ultrasound; and the chemical deposition time is 0.5-2h.

8. A core-shell structure polymer conductive microsphere, It is characterized in that The core-shell structured polymer conductive microspheres are prepared by the preparation method according to any one of claims 1 to 7, and are composite microspheres with polymer microspheres as cores and a conductive metal layer deposited on the surface of the polymer microspheres as shells.