Preparation method of crystalline polyimide covalent organic framework material

By heating polyamine monomers and aromatic polycarboxylic acid monomers in the reactor under normal pressure, combined with the use of acid additives, the preparation time of polyimide covalent organic frame materials was successfully shortened, and the solution was solved The problems of cumbersome operation and high energy consumption in the prior art have achieved an environmentally friendly and economical production process.

CN118894989BActive Publication Date: 2024-12-06TIANJIN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411396897.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-12-06
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

The existing preparation methods for crystalline polyimide covalent organic frame materials are cumbersome, time-consuming and require the use of unfriendly organic solvents and catalysts, which limits their application in industrial production.

Method used

The reactor is sealed under normal pressure, and the condensation reaction is prepared by mixing polyamine monomers, aromatic polycarboxylic acid monomers and acid additives and heating them to carry out the condensation reaction, thereby preventing the crystalline polyimide covalent organic frame material. Vacuum operation and the use of harmful solvents significantly shorten the reaction time and energy consumption.

Benefits of technology

The rapid preparation of crystalline polyimide covalent organic frame materials is achieved, which reduces the complexity and cost of the process, and uses environmentally friendly acid additives, which improves the economic and environmental protection of production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894989B_ABST
    Figure CN118894989B_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a crystalline polyimide covalent organic framework material, belonging to the field of porous organic materials. The method for preparing the crystalline polyimide covalent organic framework material comprises: uniformly mixing polyamine monomers, aromatic polycarboxylic acid monomers and acid additives and then loading them into a reactor, sealing the reactor under normal pressure; heating the sealed reactor to perform a condensation reaction at 120°C to 250°C for 0.1h to 12h to obtain a crystalline polyimide covalent organic framework material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous organic materials, and in particular relates to a method for preparing a crystalline polyimide covalent organic framework material. Background Art

[0002] Covalent organic framework materials are crystalline porous materials constructed by organic monomers cross-linked by covalent bonds, and have a highly regular two-dimensional plane or three-dimensional spatial network structure. Covalent organic framework materials have the characteristics of large specific surface area, uniform and designable pore size, easy modification and functionalization, and good thermal stability and chemical stability. Through the rational design of its structure, covalent organic framework materials with specific physical and chemical properties can be prepared. These materials are widely used in gas adsorption and separation, energy storage and conversion, heterogeneous catalysis, and optical recognition and sensing. According to the connection method between monomers, the covalent organic framework materials currently developed mainly include borate esters, imides, amides, and imides. Among them, polyimide covalent organic framework materials are suitable for use in lithium-ion batteries and other areas with high safety requirements due to their particularly excellent stability.

[0003] Current crystalline polyimide covalent organic framework materials are mainly prepared through solvothermal reactions in a vacuum environment, that is, raw materials such as organic monomers, catalysts and organic solvents are loaded into a container with a specific structure, the raw materials are solidified by cooling, the reaction system is evacuated to a vacuum and sealed, and after heating for several days, the crystalline polyimide covalent organic framework material is obtained. However, the process is relatively cumbersome and time-consuming, and often requires the use of environmentally unfriendly organic solvents and catalysts. These factors limit the large-scale industrial production of crystalline polyimide covalent organic framework materials.

[0004] Therefore, it is of great practical significance to develop a method for preparing crystalline polyimide covalent organic framework materials that is simple to operate, low in energy consumption, and green and environmentally friendly to replace the existing vacuum and solvent thermal methods. Summary of the invention

[0005] In view of the above technical problems, the present invention provides a method for preparing a crystalline polyimide covalent organic framework material, in order to at least partially solve the above technical problems. In this regard, the technical solution provided by the present invention is as follows.

[0006] According to an embodiment of the present invention, the present invention provides a method for preparing a crystalline polyimide covalent organic framework material, comprising: uniformly mixing a polyamine monomer, an aromatic polycarboxylic acid monomer and an acid auxiliary agent, loading the mixture into a reactor, and sealing the reactor under normal pressure; heating the sealed reactor to carry out a condensation reaction at 120°C to 250°C for 0.1h to 12h to obtain a crystalline polyimide covalent organic framework material.

[0007] In the embodiment of the present invention, the sealed reactor is heated at normal pressure to carry out condensation reaction without vacuum operation, thereby preparing a crystalline polyimide covalent organic framework material. The present invention provides a new method for synthesizing a crystalline polyimide covalent organic framework material, which significantly shortens the reaction time, reduces the complexity, energy consumption and cost of the preparation process, and avoids the use of expensive pressure reactors. In addition, the present invention uses low-cost, harmless acid additives to replace toxic solvents and catalysts used in traditional solvent thermal processes, which has high economic and environmental significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 This is a schematic diagram of the preparation principle of the crystalline polyimide covalent organic framework material in an embodiment of the present invention;

[0009] Figure 2 is an X-ray diffraction spectrum (XRD) diagram of the crystalline polyimide covalent organic framework material in Examples A1 to A6 of the present invention, wherein a is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A1, b is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A2, c is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A3, d is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A4, e is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A5, and f is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A6;

[0010] Figure 3 is an XRD pattern of the crystalline polyimide covalent organic framework material in Example B1 of the present invention;

[0011] Figure 4 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example C1 of the present invention;

[0012] Figure 5 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example C7 of the present invention;

[0013] Figure 6 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example D1 of the present invention;

[0014] Figure 7 is an XRD pattern of the crystalline polyimide covalent organic framework material in Example D2 of the present invention;

[0015] Figure 8 is an XRD pattern of the crystalline polyimide covalent organic framework material in Example E1 of the present invention;

[0016] Fig. 9 is an XRD pattern of the crystalline polyimide covalent organic framework material in Example E2 of the present invention;

[0017] Fig.10 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example F1 of the present invention;

[0018] Fig.11 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example F2 of the present invention;

[0019] Fig.12 is an XRD pattern of the crystalline polyimide covalent organic framework material in Example G1 of the present invention;

[0020] Fig.13 is an XRD pattern of the crystalline polyimide covalent organic framework material in Example G2 of the present invention;

[0021] Fig.14 is an XRD pattern of the crystalline polyimide covalent organic framework material in Example H1 of the present invention;

[0022] Fig.15 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example H2 of the present invention;

[0023] Fig.16 is an XRD pattern of the crystalline polyimide covalent organic framework material in Example H3 of the present invention;

[0024] Fig.17 This is the XRD pattern of the solid product prepared under vacuum conditions in Comparative Example 1. DETAILED DESCRIPTION

[0025] Below, embodiments of the present invention will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of embodiments of the present invention. However, it is apparent that one or more embodiments may also be implemented without these specific details. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of concepts of the present invention.

[0026] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. The term "comprising" used herein indicates the existence of features, steps, operations, but does not exclude the existence or addition of one or more other features.

[0027] In the case of using expressions such as "at least one of A, B, and C, etc.", it should generally be interpreted in accordance with the meaning of the expression generally understood by those skilled in the art (for example, "a system having at least one of A, B, and C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.). In the case of using expressions such as "at least one of A, B, or C, etc.", it should generally be interpreted in accordance with the meaning of the expression generally understood by those skilled in the art (for example, "a system having at least one of A, B, or C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.).

[0028] In the related art, the preparation of crystalline polyimide covalent organic framework materials is mostly carried out in a vacuum environment, the preparation process is relatively complicated and cumbersome, and the requirements for the reactor used are also relatively strict. For example: in a vacuum environment, organic monomers, organic solvents and catalysts are subjected to solvent thermal reaction for 3 to 5 days to prepare polyimide covalent organic framework materials. This synthesis method inevitably uses a large amount of toxic organic solvents and catalysts, which is uneconomical and environmentally unfriendly, and takes a long time. Another method is to prepare polyimide covalent organic framework materials by a non-solvent method in a vacuum environment. Although this synthesis method avoids the use of harmful and toxic organic solvents, the synthesis time still requires more than 2 days, and the preparation process is still relatively complicated and energy consumption is high. In this regard, the present invention proposes a new synthesis method, which does not require vacuum operation and does not use harmful organic solvents. A reactor with a simple structure is used under normal pressure. Within a condensation reaction time of 0.5h to 12h, or even a shorter time, a polyimide covalent organic framework material with high crystallinity can be prepared, which significantly shortens the reaction time and reduces the complexity of the synthesis process.

[0029] Figure 1 Schematic diagram of the preparation principle of the crystalline polyimide covalent organic framework material in an embodiment of the present invention.

[0030] Specifically, Figure 1 As shown, the preparation method of the crystalline polyimide covalent organic framework material of the present invention comprises: uniformly mixing a polyamine monomer, an aromatic polycarboxylic acid monomer and an acid auxiliary agent and loading them into a reactor, and sealing the reactor under normal pressure; heating the sealed reactor to perform a condensation reaction at 120° C. to 250° C. for 0.1 h to 12 h to obtain a crystalline polyimide covalent organic framework material.

[0031] In an embodiment of the present invention, in the reaction of synthesizing a crystalline polyimide covalent organic framework material, the initial stage of the reaction is condensed into an amorphous polyimide intermediate by a polyamine monomer and an aromatic polycarboxylic acid monomer and produces water, and further, with the participation of water, a dynamic reversible reaction is self-repaired to form a crystalline polyimide covalent organic framework material. The reason why the reaction time is long in the traditional method of preparing a crystalline polyimide covalent organic framework material under vacuum conditions is that under a vacuum environment, the water produced by the condensation of polyamine monomers and aromatic polycarboxylic acid monomers is quickly taken away by the vacuum and fills the reaction container, and most of the water in the reaction system is evenly distributed in the entire container in the form of steam, and the water concentration in contact with the amorphous polyimide intermediate is relatively low, resulting in a low reverse reaction rate of the reversible reaction, which leads to a long time for synthesizing a crystalline polyimide covalent organic framework material. In the present invention, no vacuum operation is performed, and heating is performed in a closed air atmosphere to carry out a condensation reaction. Due to the high pressure in the reaction system, the water produced during the synthesis of the covalent organic framework material evaporates slowly. The un-volatile water is on the surface of the amorphous polyimide intermediate, which makes the local concentration of water near the amorphous polyimide intermediate higher. Therefore, the reaction rate of the reversible reaction remains balanced and maintained at a relatively high reverse reaction rate, thereby significantly shortening the reaction time of synthesizing crystalline polyimide covalent organic framework materials while reducing the complexity, cost and energy consumption of synthesizing covalent organic framework materials.

[0032] According to an embodiment of the present invention, the polyamine monomer is selected from any one of 1,3,5-tris(4-aminophenyl)benzene, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1,3,5-tris(4-aminophenyl)amine, melamine, and 2,7,12-triamino-5H-diindeno[1,2-a:1',2'-c]fluorene-5,10,15-trione, preferably any one of 1,3,5-tris(4-aminophenyl)benzene, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, and 1,3,5-tris(4-aminophenyl)amine. The aromatic polycarboxylic acid monomer is a polycarboxylic acid of tetramer or higher, for example, any one of 1,2,4,5-benzenetetracarboxylic acid and 1,4,5,8-naphthalenetetracarboxylic acid.

[0033] According to an embodiment of the present invention, the acid auxiliary agent is selected from at least one of aliphatic carboxylic acid of C2~C8, phenylphosphonic acid, phosphoric acid, furoic acid, nicotinic acid, substituted or unsubstituted benzoic acid, wherein the substituent in benzoic acid is selected from any one of hydroxyl, halogen, sulfhydryl, methoxyl, and methylthio, wherein the preferred acid auxiliary agent is selected from at least one of furoic acid, phenylphosphonic acid, phosphoric acid, and benzoic acid substituted by a substituent selected from hydroxyl, halogen or sulfhydryl, and the halogen is selected from fluorine, chlorine or bromine. Specifically, the aliphatic carboxylic acid of C2~C8 can be selected from any one of acetic acid, butyric acid, hexanoic acid, and octanoic acid; the substituted benzoic acid can be selected from any one of salicylic acid, 2-fluorobenzoic acid, 2-chlorobenzoic acid, 2-bromobenzoic acid, 2-mercaptobenzoic acid, 2-methoxybenzoic acid, and 2-methylthiobenzoic acid. More specifically, the preferred acid auxiliary agent is selected from at least one of salicylic acid, 2-fluorobenzoic acid, 2-chlorobenzoic acid, 2-bromobenzoic acid, 2-mercaptobenzoic acid, furoic acid, phenylphosphonic acid, and phosphoric acid. The acid auxiliary agent in the present invention can catalyze the formation of crystalline polyimide covalent organic framework materials from polyamine monomers and aromatic polycarboxylic acid monomers, wherein the acid auxiliary agent with stronger acidity is preferred, and the catalytic effect is better, so that the reaction time of the synthetic crystalline polyimide covalent organic framework material is shorter. In addition, the present invention selects low-cost, harmless acid auxiliary agents to replace the toxic solvents and catalysts used in traditional solvent thermal reactions, and the amount of the acid auxiliary agent is significantly less than the organic solvent used in traditional solvent thermal reactions, which has higher economic and environmental significance.

[0034] According to an embodiment of the present invention, in a reactor with a unit milliliter volume, the amount of polyamine monomer added is 0.017~0.17mmol, the molar ratio of aromatic polycarboxylic acid monomer to polyamine monomer is 0.5:1~5:1; the molar ratio of acid auxiliary agent to polyamine monomer is 1:1~10:1. In an embodiment of the present invention, when the reaction materials added to the reaction vessel with a unit milliliter volume are within this ratio range, the water vapor generated by the condensation of polyamine monomer and aromatic polycarboxylic acid monomer will cause a higher pressure in the container, inhibiting further volatilization of water. In particular, when the partial pressure of water vapor in the system reaches the saturated vapor pressure of water, the volatilization and condensation of water reach equilibrium, and the net volatilization rate drops to zero. In this case, the local concentration of water near the amorphous polyimide intermediate is the highest, thereby significantly accelerating the dynamic reversible reaction and effectively shortening the reaction time.

[0035] According to an embodiment of the present invention, the method for preparing a crystalline polyimide covalent organic framework material further comprises: adding water as an auxiliary agent.

[0036] In an embodiment of the present invention, polyamine monomers, aromatic polycarboxylic acid monomers, acid auxiliary agents and water are mixed evenly and then loaded into a reactor, and the reactor is sealed at normal pressure; the sealed reactor is heated to obtain a crystalline polyimide covalent organic framework material through a condensation reaction. Water is added to accelerate the reverse reaction rate in the reversible reaction of synthesizing the polyimide covalent organic framework material, thereby further shortening the reaction time and obtaining a polyimide covalent organic framework material with higher crystallinity.

[0037] According to an embodiment of the present invention, the molar ratio of water to polyamine monomer is 5 to 50: 1. Within this ratio range, the time for synthesizing polyimide covalent organic framework materials can be significantly shortened. If the ratio is higher or lower than this ratio range, the reaction time cannot be shortened or the polyimide covalent organic framework material cannot be obtained.

[0038] According to an embodiment of the present invention, with the addition of water as an auxiliary agent, a condensation reaction is carried out at 120° C. to 250° C. for 10 min to 30 min to obtain a crystalline polyimide covalent organic framework material.

[0039] The following schematically illustrates the preparation method of the crystalline polyimide covalent organic framework material. It should be noted that the examples are only some specific embodiments of the present invention and cannot limit the protection scope of the present invention.

[0040] Example

[0041] Example A1

[0042] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), and salicylic acid (249 mg, 1.8 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Figure 2 As shown in a in .

[0043] Example A2

[0044] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,4,5,8-naphthalenetetracarboxylic acid (137 mg, 0.45 mmol), and salicylic acid (249 mg, 1.8 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Figure 2 As shown in b.

[0045] Example A3

[0046] Weigh 2,4,6-tris(4-aminophenyl)-1,3,5-triazine (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), and salicylic acid (249 mg, 1.8 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Figure 2 As shown in c.

[0047] Example A4

[0048] Weigh 1,3,5-tri(4-aminophenyl)amine (87 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), and salicylic acid (249 mg, 1.8 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Figure 2 As shown in d.

[0049] Example A5

[0050] Weigh 2,7,12-triamino-5H-diindeno[1,2-a:1',2'-c]fluorene-5,10,15-trione (129 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), and salicylic acid (249 mg, 1.8 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 hour. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Figure 2 As shown in e.

[0051] Example A6

[0052] Melamine (38 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), and salicylic acid (249 mg, 1.8 mmol) were weighed, stirred and ground to mix evenly, and then transferred to a 6 mL glass bottle, sealed under normal pressure, and heated to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material was obtained, and its X-ray diffraction spectrum is shown as follows Figure 2 As shown in f.

[0053] Figure 2It is an X-ray diffraction spectrum (XRD) diagram of the crystalline polyimide covalent organic framework material in Examples A1 to A6 of the present invention, wherein a is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A1, b is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A2, c is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A3, d is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A4, e is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A5, and f is the XRD diagram of the crystalline polyimide covalent organic framework material in Example A6.

[0054] like Figure 2 As shown, the crystalline polyimide covalent organic framework material in Example A1 has obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5°; the crystalline polyimide covalent organic framework material in Example A2 has obvious diffraction peaks at 2.8°, 4.9°, 5.6° and 7.4°; the crystalline polyimide covalent organic framework material in Example A3 has obvious diffraction peaks at 2.8°, 5.8° and 7.7°; the crystalline polyimide covalent organic framework material in Example A4 has obvious diffraction peaks at 2.8°, 5.8° and 7.7°; The machine frame material has obvious diffraction peaks at 3.3°, 5.7°, 6.6° and 8.8°; the crystalline polyimide covalent organic framework material in Example A5 has obvious diffraction peaks at 2.8°, 5.6° and 7.4°; the crystalline polyimide covalent organic framework material in Example A6 has obvious diffraction peaks at 4.9°, 8.5°, 9.8° and 14.0°, etc., proving that the polyimide covalent organic framework materials in Examples A1 to A6 all have good crystallinity. Further, it can be seen from the above Examples A1 to A6 that in a sealed reactor at normal pressure, different types of polyamine monomers and different types of aromatic polycarboxylic acid monomers are used to carry out condensation reaction under the catalysis of an acid auxiliary agent, and polyimide covalent organic framework materials with high crystallinity can be obtained within a relatively short reaction time (1h), indicating that the present invention is not limited to the selection of polyamine monomers and aromatic polycarboxylic acid monomers, and has a certain universality.

[0055] Similarly, the crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A1, and Examples A7 to A13 were carried out, except that other acid additives were used to replace salicylic acid for condensation reaction to obtain the crystalline polyimide covalent organic framework material. Among them, Example A7 used 2-fluorobenzoic acid (252 mg, 1.8 mmol) as an acid additive, Example A8 used 2-chlorobenzoic acid (282 mg, 1.8 mmol) as an acid additive, Example A9 used 2-bromobenzoic acid (362 mg, 1.8 mmol) as an acid additive, Example A10 used 2-mercaptobenzoic acid (278 mg, 1.8 mmol) as an acid additive, Example A11 used furoic acid (202 mg, 1.8 mmol) as an acid additive, Example A12 used phenylphosphonic acid (285 mg, 1.8 mmol) as an acid additive, and Example A13 used phosphoric acid (176 mg, 1.8 mmol) as an acid additive.

[0056] It has been found through experiments that under the same reaction conditions, only by changing the type of acid auxiliary agent, a crystalline polyimide covalent organic framework material with high crystallinity can be obtained. Furthermore, the acid auxiliary agents selected in Examples A7 to A13 have strong acidity, which is close to or slightly stronger than the acid auxiliary agent in Example A1, and can efficiently catalyze the condensation of polyamine monomers and aromatic polycarboxylic acid monomers to generate an amorphous polyimide intermediate, and further rearrange to a crystalline polyimide covalent organic framework through a dynamic reversible reaction, so that a crystalline polyimide covalent organic framework material with high crystallinity can be obtained within a short reaction time (1h).

[0057] Example B1

[0058] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), and benzoic acid (220 mg, 1.8 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 6 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Figure 3 shown.

[0059] Figure 3 : This is the XRD diagram of the crystalline polyimide covalent organic framework material in Example B1 of the present invention.

[0060] like Figure 3 As shown, the crystalline polyimide covalent organic framework material in Example B1 has obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5°, etc., proving that it has good crystallinity.

[0061] Example B2

[0062] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example B1, except that 2-methoxybenzoic acid (274 mg, 1.8 mmol) was used as an acid auxiliary, and the other reaction conditions were the same. After washing and drying, a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5° was obtained.

[0063] Example B3

[0064] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example B1, except that 2-methylthiobenzoic acid (303 mg, 1.8 mmol) was used as an acid auxiliary. After washing and drying, a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5° was obtained.

[0065] Example B4

[0066] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example B1, except that nicotinic acid (222 mg, 1.8 mmol) was used as an acid auxiliary agent. After washing and drying, a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5° was obtained.

[0067] Example B5

[0068] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example B1, except that acetic acid (108 mg, 1.8 mmol) was used as an acid auxiliary agent. After washing and drying, a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5° was obtained.

[0069] Example B6

[0070] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example B1, except that butyric acid (159 mg, 1.8 mmol) was used as an acid auxiliary agent. After washing and drying, a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5° was obtained.

[0071] Example B7

[0072] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example B1, except that hexanoic acid (209 mg, 1.8 mmol) was used as an acid auxiliary agent. After washing and drying, a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5° was obtained.

[0073] Example B8

[0074] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example B1, except that octanoic acid (260 mg, 1.8 mmol) was used as an acid auxiliary agent. After washing and drying, a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5° was obtained.

[0075] The acidity of the acid auxiliary agent used in Example B1 to Example B8 is weaker than that of the acid auxiliary agent in Example A1 and Example A7 to Example A13. The acid auxiliary agent in Example B1 to Example B8 can effectively catalyze the condensation of polyamine monomers and aromatic polycarboxylic acid monomers to generate imide and further rearrange to a crystalline polyimide covalent organic framework through a dynamic reversible reaction. It is only that the catalytic efficiency of Example B1 to Example B8 is lower than that of the acid auxiliary agent in Example A1 and Example A7 to Example A13. Therefore, it can be seen from the above-mentioned Example A1, Example A7 to Example A13, Example B1 to Example B8 that the strength of the acidity affects the synthesis reaction time of the crystalline polyimide covalent organic framework material, and the reaction time (6h) required to obtain a crystalline polyimide covalent organic framework material with higher crystallinity is more than the reaction time (1h) of Example A1 and Example A7 to Example A13, but significantly less than the time required in the prior art (more than 72h).

[0076] Example C1

[0077] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A1, except that the condensation reaction time was 12 h, thereby obtaining a crystalline polyimide covalent organic framework material, whose X-ray diffraction spectrum is as follows: Figure 4 shown.

[0078] Example C2

[0079] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A2, except that the condensation reaction time was 12 h, thereby obtaining a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 4.9°, 5.6° and 7.4°.

[0080] Example C3

[0081] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A3, except that the condensation reaction time was 12 h, thereby obtaining a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 5.8° and 7.7°.

[0082] Example C4

[0083] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A4, except that the condensation reaction time was 12 h, thereby obtaining a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 3.3°, 5.7°, 6.6° and 8.8°.

[0084] Example C5

[0085] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A5, except that the condensation reaction time was 12 h, thereby obtaining a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 2.8°, 5.6° and 7.4°.

[0086] Example C6

[0087] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A6, except that the condensation reaction time was 12 h, thereby obtaining a crystalline polyimide covalent organic framework material having obvious diffraction peaks at 4.9°, 8.5°, 9.8° and 14.0°.

[0088] Example C7

[0089] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A1, except that the condensation reaction time was 0.5 h, thereby obtaining a crystalline polyimide covalent organic framework material, whose X-ray diffraction spectrum is as follows: Figure 5 shown.

[0090] Figure 4 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example C1 of the present invention, Figure 5 This is the XRD diagram of the crystalline polyimide covalent organic framework material in Example C7 of the present invention.

[0091] like Figure 4~Figure 5 As shown, the crystalline polyimide covalent organic framework materials in Examples C1 and C7 have obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5°, etc., proving that they have good crystallinity. Figure 2 a and Figure 4~Figure 5 It can be seen that by using the synthesis method provided by the present invention, a crystalline polyimide covalent organic framework material with high crystallinity can be obtained within a time range of 0.5h to 12h. From the perspective of crystallinity and energy consumption, it is preferred to perform a condensation reaction for 1h.

[0092] Example D1

[0093] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A1, except that the crystalline polyimide covalent organic framework material was obtained by heating to 120°C. The X-ray diffraction spectrum of the crystalline polyimide covalent organic framework material is shown in FIG. Figure 6 shown.

[0094] Example D2

[0095] The crystalline polyimide covalent organic framework material was synthesized by the same preparation method as in Example A1, except that the crystalline polyimide covalent organic framework material was obtained by heating to 250° C., and its X-ray diffraction spectrum was as follows: Figure 7 shown.

[0096] Figure 6 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example D1 of the present invention; Figure 7 This is the XRD diagram of the crystalline polyimide covalent organic framework material in Example D2 of the present invention.

[0097] like Figure 6-7 As shown, the crystalline polyimide covalent organic framework materials in Examples D1 and D2 have obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5°, proving that they have good crystallinity. Figure 2 a in Figure 6~Figure 7 It can be seen that in the synthesis method provided by the present invention, a crystalline polyimide covalent organic framework material can be obtained in the temperature range of 120-250° C., wherein a polyimide covalent organic framework material with higher crystallinity can be obtained at 160-250° C. From the perspective of energy consumption and material crystallinity, it is preferred to carry out the condensation reaction at 160° C.

[0098] Example E1

[0099] Weigh 1,3,5-tri(4-aminophenyl)benzene (35 mg, 0.1 mmol), 1,2,4,5-benzenetetracarboxylic acid (38 mg, 0.15 mmol), and salicylic acid (83 mg, 0.6 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Figure 8 shown.

[0100] Example E2

[0101] Weigh 1,3,5-tri(4-aminophenyl)benzene (352 mg, 1 mmol), 1,2,4,5-benzenetetracarboxylic acid (381 mg, 1.5 mmol), and salicylic acid (829 mg, 6 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Fig. 9 shown.

[0102] Figure 8 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example E1 of the present invention, Fig. 9 This is the XRD diagram of the crystalline polyimide covalent organic framework material in Example E2 of the present invention.

[0103] like Figures 8 and 9 As shown, the crystalline polyimide covalent organic framework materials in Examples E1 and E2 have obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5°, proving that they have good crystallinity. Figure 2 a in Figure 8~Figure 9 It can be seen that in the synthesis method provided by the present invention, when the content of the reaction materials (i.e., polyamine monomers, aromatic polycarboxylic acid monomers and acid auxiliary agents) in the reactor per milliliter volume is relatively high (i.e., the amount of the polyamine monomer substance in the reactor with a volume of 1 mL is not less than 0.017 mmol), a polyimide covalent organic framework material with higher crystallinity can be obtained, and the higher the content of the reaction materials in the reactor per milliliter volume, the higher the crystallinity of the polyimide covalent organic framework material can be obtained.

[0104] Example F1

[0105] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (38 mg, 0.15 mmol), and salicylic acid (249 mg, 1.8 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, heat to 160 ° C for condensation reaction for 1 h, wash and dry to obtain a crystalline polyimide covalent organic framework material, whose X-ray diffraction spectrum is shown as follows Fig.10 shown.

[0106] Example F2

[0107] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (381 mg, 1.5 mmol), and salicylic acid (249 mg, 1.8 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Fig.11 shown.

[0108] Fig.10 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example F1 of the present invention, Fig.11 : This is the XRD pattern of the crystalline polyimide covalent organic framework material in Example F2 of the present invention.

[0109] like Figures 10-11 As shown, the crystalline polyimide covalent organic framework materials in Examples F1 and F2 have obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5°, proving that they have good crystallinity. Figure 2 a in Figure 10~Figure 11 It can be seen that in the synthesis method provided by the present invention, a crystalline polyimide covalent organic framework material can be obtained when the molar ratio of the aromatic polycarboxylic acid monomer to the polyamine monomer is 0.5:1 to 5:1. Among them, when the molar ratio of the aromatic polycarboxylic acid monomer to the polyamine monomer is 1.5:1, a polyimide covalent organic framework material with higher crystallinity can be obtained.

[0110] Example G1

[0111] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), and salicylic acid (41 mg, 0.3 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Fig.12 shown.

[0112] Example G2

[0113] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), and salicylic acid (414 mg, 3 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 1 h. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Fig.13 shown.

[0114] Fig.12 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example G1 of the present invention, Fig.13 This is the XRD diagram of the crystalline polyimide covalent organic framework material in Example G2 of the present invention.

[0115] like Figures 12-13 As shown, the crystalline polyimide covalent organic framework materials in Examples G1 and G2 have obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5°, proving that they have good crystallinity. Figure 2 a in Figure 12~Figure 13 It can be seen that in the synthesis method provided by the present invention, the molar ratio of the acid auxiliary agent to the polyamine monomer is 1:1~10:1 to obtain a crystalline polyimide covalent organic framework material, among which, when the molar ratio of the acid auxiliary agent to the polyamine monomer is 6:1, a polyimide covalent organic framework material with higher crystallinity can be obtained.

[0116] Example H1

[0117] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), salicylic acid (249 mg, 1.8 mmol), and water (27 mg, 1.5 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 10 min. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Fig.14 shown.

[0118] Example H2

[0119] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), salicylic acid (249 mg, 1.8 mmol), and water (270 mg, 15 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 10 min. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Fig.15 shown.

[0120] Example H3

[0121] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), salicylic acid (249 mg, 1.8 mmol), and water (27 mg, 1.5 mmol), stir and grind to mix evenly, transfer to a 6 mL glass bottle, seal under normal pressure, and heat to 160 ° C for condensation reaction for 30 min. After washing and drying, a crystalline polyimide covalent organic framework material is obtained, and its X-ray diffraction spectrum is as follows Fig.16 shown.

[0122] Fig.14 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example H1 of the present invention, Fig.15 is the XRD pattern of the crystalline polyimide covalent organic framework material in Example H2 of the present invention, Fig.16 This is the XRD diagram of the crystalline polyimide covalent organic framework material in Example H3 of the present invention.

[0123] like Figures 14 to 16 As shown, the crystalline polyimide covalent organic framework materials in Examples H1 to H3 have obvious diffraction peaks at 2.8°, 4.9°, 5.7° and 7.5°, proving that they have good crystallinity. Figure 2 a in Figure 14~Figure 16 It can be seen that in the synthesis method provided by the present invention, adding water as an auxiliary agent can significantly shorten (10 min) the time required for synthesizing the crystalline polyimide covalent organic framework material and the product has higher crystallinity.

[0124] Comparative Example 1

[0125] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol) and salicylic acid (249 mg, 1.8 mmol), stir and grind to mix evenly, and then put them into a 6 mL glass tube. After evacuating the glass tube, melt the opening with a flame to seal it, and then heat it to 160 ° C for condensation reaction for 12 hours. After washing and drying, a solid product is obtained. The X-ray diffraction spectrum of the solid product is as follows Fig.17 shown.

[0126] Fig.17 This is the XRD pattern of the solid product prepared under vacuum conditions in Comparative Example 1.

[0127] like Fig.17 As shown, the diffraction peaks in the XRD pattern are not obvious, indicating that the solid product has no crystallinity.

[0128] Comparative Example 2

[0129] Weigh 1,3,5-tri(4-aminophenyl)benzene (11 mg, 0.03 mmol), 1,2,4,5-benzenetetracarboxylic acid (11 mg, 0.045 mmol) and salicylic acid (25 mg, 0.18 mmol), stir and grind to mix evenly, put into a 6 mL glass bottle, seal under normal pressure, heat to 160 ° C for condensation reaction for 1 h, wash and dry to obtain a solid product.

[0130] The solid product in Comparative Example 2 was tested by X-ray diffraction spectrum. The diffraction peaks in the obtained XRD pattern were not obvious, indicating that the solid product did not have crystallinity. This shows that when the method provided by the present invention is used, but the content of the reaction materials (i.e., polyamine monomers, aromatic polycarboxylic acid monomers and acid auxiliary agents) in the reactor per milliliter volume is too small (i.e., the amount of polyamine monomer material in the reactor with a volume of 1 mL is less than 0.017 mmol), a crystalline polyimide covalent organic framework material cannot be obtained.

[0131] Comparative Example 3

[0132] 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol), salicylic acid (249 mg, 1.8 mmol) and water (540 mg, 30 mmol) were weighed, stirred and ground to mix evenly, and then put into a 6 mL glass bottle, sealed under normal pressure, and heated to 160 ° C for condensation reaction for 1 hour, and no solid product was obtained. This shows that by using the synthesis method provided by the present invention, adding excessive water will not be able to obtain a crystalline polyimide covalent organic framework material.

[0133] Comparative Example 4

[0134] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic dianhydride (98 mg, 0.45 mmol) and salicylic acid (249 mg, 1.8 mmol), stir and grind to mix evenly, put into a 6 mL glass bottle, seal under normal pressure, heat to 160 ° C for condensation reaction for 1 h, wash and dry to obtain a solid product.

[0135] The solid product in Comparative Example 4 was subjected to an XRD test, and the test found that the diffraction peak in the XRD graph was not obvious, indicating that the product did not have crystallinity. This shows that the crystalline polyimide covalent organic framework material cannot be synthesized by using the synthesis method provided by the present invention and using aromatic polycarboxylic acid anhydride monomers instead of aromatic polycarboxylic acid monomers as reaction raw materials.

[0136] Comparative Example 5

[0137] Weigh 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol) and benzoic anhydride (204 mg, 0.9 mmol), stir and grind to mix evenly, put into a 6 mL glass bottle, seal under normal pressure, heat to 160 ° C for condensation reaction for 6 h, and wash and dry to obtain a solid product.

[0138] The solid product in Comparative Example 5 was subjected to an XRD test, and the test found that the diffraction peak in the XRD diagram was not obvious, indicating that the product did not have crystallinity. This shows that the crystalline polyimide covalent organic framework material cannot be synthesized by using the synthesis method provided by the present invention and using anhydride instead of acid auxiliary agent as the reaction raw material.

[0139] Comparative Example 6

[0140] 1,3,5-tri(4-aminophenyl)benzene (106 mg, 0.3 mmol), 1,2,4,5-benzenetetracarboxylic acid (114 mg, 0.45 mmol) and trifluoroacetic acid (205 mg, 1.8 mmol) were weighed, stirred and ground to mix evenly, and then placed in a 6 mL glass bottle, sealed under normal pressure, and heated to 160 ° C for condensation reaction for 1 hour, and no solid product was obtained. This shows that by using the synthesis method provided by the present invention, adding an acid with too strong acidity (such as trifluoroacetic acid) as an auxiliary agent, it is impossible to obtain a crystalline polyimide covalent organic framework material.

[0141] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a crystalline polyimide covalent organic framework material, characterized in that: The preparation method comprises: Mixing polyamine monomers, aromatic polycarboxylic acid monomers and acid auxiliary agents uniformly and loading them into a reactor, and sealing the reactor under normal pressure; The sealed reactor is heated to perform a condensation reaction at 120° C. to 250° C. for 0.1 h to 12 h to obtain a crystalline polyimide covalent organic framework material; The polyamine monomer is selected from any one of 1,3,5-tris(4-aminophenyl)benzene, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1,3,5-tris(4-aminophenyl)amine, melamine, and 2,7,12-triamino-5H-diindeno[1,2-a:1',2'-c]fluorene-5,10,15-trione; The aromatic polycarboxylic acid monomer is selected from any one of 1,2,4,5-benzenetetracarboxylic acid and 1,4,5,8-naphthalenetetracarboxylic acid; The acid auxiliary agent is selected from at least one of C2-C8 aliphatic carboxylic acid, phenylphosphonic acid, phosphoric acid, furoic acid, nicotinic acid, and substituted or unsubstituted benzoic acid, wherein the substituent in the benzoic acid is selected from any one of hydroxyl, halogen, thiol, methoxy, and methylthio; Among them, in the reactor with a volume of unit milliliter, the added amount of the polyamine monomer is 0.017~0.17mmol, the molar ratio of the aromatic polycarboxylic acid monomer to the polyamine monomer is 0.5:1~5:1; the molar ratio of the acid auxiliary agent to the polyamine monomer is 1:1~10:

1.

2. The preparation method according to claim 1, characterized in that: The acid auxiliary agent is selected from at least one of furoic acid, phenylphosphonic acid, phosphoric acid, and benzoic acid substituted with a substituent selected from hydroxyl, halogen or mercapto.

3. The preparation method according to any one of claims 1-2, characterized in that The preparation method further comprises: adding water as an auxiliary agent; The molar ratio of water to polyamine monomer is 5-50:

1.

4. The preparation method according to claim 3, characterized in that: The condensation reaction is carried out at 120° C. to 250° C. for 10 min to 30 min to obtain a crystalline polyimide covalent organic framework material.

Citation Information

Patent Citations

  • Covalent bond organic framework nanofiber as well as preparation method and application thereof

    CN114214751A

  • Anion hydrogen bond organic framework material based on carboxylic acid monomer as well as preparation method and application of anion hydrogen bond organic framework material

    CN114276552A