Structural color solution composition and application thereof

Through the polyelectrolyte-induced structural color solution composition, the regular arrangement structure is formed by ultrasound and static treatment, which solves the problem of complex construction and color adjustment difficulty of structural color ink in the prior art, and realizes the formation of structural color at ultra-low concentrations and the convenience of multi-mode processing.

CN118895067APending Publication Date: 2024-11-05QINGDAO UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411088977.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The construction process of existing structural color inks is complex, requiring high concentration of particles and difficult to tune colors through simple methods, and there are limitations in the construction of three-dimensional structures.

Method used

Using a polyelectrolyte-induced structural color solution composition, the surface of the microspheres is covered with polyanionic electrolyte by ultrasonic and static treatment, forming a self-assembled monomer and forming a regular arrangement structure, and the structure color formation is achieved using hydrogen bonds and electrostatic repulsion effects.

Benefits of technology

The formation of structural colors at ultra-low concentrations is achieved, the color adjustment process is simplified, the use of microspheres is reduced, and the structural colors can be maintained in multi-mode processing, which is suitable for the preparation of low-viscosity thermally cured structural colors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004985973310000011
    Figure HDA0004985973310000011
  • Figure HDA0004985973310000012
    Figure HDA0004985973310000012
  • Figure HDA0004985973310000013
    Figure HDA0004985973310000013
Patent Text Reader

Abstract

The invention discloses a structural color solution composition and application thereof, the composition comprises microspheres, polyanion electrolyte and water, and the composition can form a structural color solution after ultrasonic treatment and standing. According to the method, the super-low-concentration charged microspheres can form the structural color in the solution by utilizing the synergistic effect of hydrogen bond aggregation and electrostatic repulsion of the polyanion electrolyte, and other complex treatment is not needed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of structural color ink, and in particular relates to a structural color solution composition and application thereof. Background Art

[0002] Eco-friendly, long-lasting and low-toxic structural colors are widely found in nature, such as feathers or scales of birds, fish and insects. Most of these natural structural colors are produced by periodically arranged micro / nano structures, which form colors through interference, reflection, scattering or diffraction with visible light. Inspired by this phenomenon in nature, researchers have developed a variety of artificial structural color materials using colloidal micro / nanoparticles, liquid crystals, photolithography or block copolymers.

[0003] However, to date, the construction of complex structural color patterns with multiple colors usually relies on complex step-by-step manufacturing of different photonic crystal inks, or is achieved by adjusting the local lattice constant / refractive index. This process is not only time-consuming, but also increases dramatically in difficulty as the number of required colors increases. In addition, the generation process of structural colors often requires time-consuming fine evaporation or electrophoresis-induced self-assembly, and these traditional self-assembly strategies have certain limitations in the construction of three-dimensional structures. Therefore, it is very desirable to develop a simple and universal strategy to construct photonic crystals with excellent processing flexibility and convenience for practical applications. Summary of the invention

[0004] The purpose of the present invention is to solve the problems that current structural color inks often require high-concentration particles, have a complex construction process, cannot be toned by simple methods, and have a single processing model, and to provide a polyelectrolyte-induced structural color solution composition and its application.

[0005] One of the objectives of the present invention is to provide a structural color solution composition, which includes microspheres, polyanion electrolytes and water.

[0006] In a preferred embodiment, the polyanion electrolyte is selected from polymers containing multiple hydroxyl groups and multiple anionic groups.

[0007] In a further preferred embodiment, the polyanion electrolyte is selected from at least one of sodium alginate, carrageenan, and sodium carboxymethyl cellulose.

[0008] The inventors found during the experiment that non-polyelectrolytes (such as uncharged polymer polyvinyl alcohol (PVA)) and polycationic polyelectrolytes (such as chitosan (CS)) cannot form structural colors in the second purpose of the present invention.

[0009] In a further preferred embodiment, the molecular weight of the polyanion electrolyte is 1 to 2 million Da, preferably 200,000 to 1.5 million Da, for example 10,000 Da, 50,000 Da, 100,000 Da, 200,000 Da, 500,000 Da, 800,000 Da, 1 million Da, 1.2 million Da, 1.5 million Da, 1.8 million Da or 2 million Da.

[0010] In a preferred embodiment, the surface of the microsphere contains groups that can form electrostatic interactions with hydroxyl groups.

[0011] In a further preferred embodiment, the microspheres are selected from microspheres containing carboxyl groups on the surface, for example, selected from PS-PMMA-PAA microspheres, PS-COOH microspheres, SiO 2 -COOH microspheres.

[0012] In a further preferred embodiment, the particle size of the microspheres is 120-350 nm, preferably 150-300 nm, more preferably 170-260 nm, for example 120 nm, 140 nm, 160 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm, 320 nm, 340 nm or 350 nm.

[0013] In a preferred embodiment, the mass concentration of the polyanion electrolyte in the composition is 0.01wt% to 5wt%, for example, 0.01wt%, 0.02wt%, 0.04wt%, 0.06wt%, 0.08wt%, 0.1wt%, 0.2wt%, 0.5wt%, 0.8wt%, 1wt%, 2wt%, 3wt%, 4wt% or 5wt%.

[0014] In a preferred embodiment, the concentration of the microspheres in the composition is 0.01 v / v% to 1.0 v / v%, for example, 0.01 v / v%, 0.02 v / v%, 0.05 v / v%, 0.08 v / v%, 0.1 v / v%, 0.2 v / v%, 0.5 v / v%, 0.8 v / v% or 1.0 v / v%.

[0015] In a preferred embodiment, the composition optionally contains carbon black.

[0016] In a further preferred embodiment, the content of carbon black in the composition is 0.001wt% to 0.01wt%, for example, 0.001wt%, 0.002wt%, 0.003wt%, 0.004wt%, 0.005wt%, 0.006wt%, 0.007wt%, 0.008wt%, 0.009wt% or 0.01wt%.

[0017] The structural color solution composition of the present invention is obtained as follows: adding the polyanion electrolyte aqueous solution to the microspheres to obtain the composition.

[0018] Wherein, the microspheres can be added in the form of microsphere dispersion, and the dispersion is an aqueous solution.

[0019] The second object of the present invention is to provide a method for preparing a structural color solution, comprising: ultrasonicating and allowing the composition described in the first object of the present invention to stand to obtain the structural color solution.

[0020] In a preferred embodiment, after ultrasonic and static treatment, the polyanion electrolyte covers the surface of the microsphere to form self-assembly monomers (increasing the amount of charge carried by the surface of the microsphere), and the self-assembly monomers assemble to form a regular arrangement (through the dual effects of surface polyanion electrolyte aggregation and charge repulsion, assembled into a local regular arrangement structure).

[0021] In the present invention, the polyanion electrolyte can form a coating on the surface of the microspheres, which on the one hand enhances the repulsive force between the microspheres, and on the other hand promotes the aggregation of the microspheres through hydrogen bond interactions. This dual effect of repulsion and aggregation synergistically acts on the microspheres, prompting them to arrange into a short-range ordered structure. As a result, the microspheres are able to self-assemble into a short-range ordered array, thereby forming a structural color that does not change with the observation angle.

[0022] In a preferred embodiment, the mass concentration of the polyanion electrolyte in the structural color solution is 0.01wt% to 5wt%, for example, 0.01wt%, 0.02wt%, 0.04wt%, 0.06wt%, 0.08wt%, 0.1wt%, 0.2wt%, 0.5wt%, 0.8wt%, 1wt%, 2wt%, 3wt%, 4wt% or 5wt%.

[0023] During the experiment, the inventors found that in the system of the present invention, the concentration of polyanion electrolyte has a significant effect on the structural color: when the concentration of polyanion electrolyte is too low, the microspheres cannot be aggregated into a local ordered structure and cannot form structural color; when the concentration of polyanion electrolyte is too high, the induction effect of the polyanion electrolyte molecular chain is much greater than the repulsion between the microspheres, resulting in excessive aggregation of the microspheres, which also cannot form a local ordered structure and cannot form structural color.

[0024] In a preferred embodiment, the concentration of the microspheres in the structural color solution is 0.01 v / v% to 1.0 v / v%, for example, 0.01 v / v%, 0.02 v / v%, 0.05 v / v%, 0.08 v / v%, 0.1 v / v%, 0.2 v / v%, 0.5 v / v%, 0.8 v / v% or 1.0 v / v%.

[0025] The inventors found during the experiment that in the system of the present invention, when the concentration of microspheres is lower than 0.01 v / v%, no structural color will appear; and when the concentration of microspheres is too high, the structural color will weaken.

[0026] In the present invention, microspheres can produce structural color phenomenon at ultra-low concentrations (0.01 v / v% to 1.0 v / v%), which is 3 orders of magnitude lower than the previously reported concentration of microsphere photonic crystals (30 v / v% to 50 v / v%), greatly reducing the amount of microspheres used.

[0027] In the present invention, by utilizing the synergistic effect of hydrogen bond aggregation and electrostatic repulsion of polyanion electrolytes, ultra-low concentration of charged microspheres can form structural colors in solution without the need for other complicated treatments.

[0028] In a preferred embodiment, the ultrasonication is performed for 2 to 40 minutes, for example, 2 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes.

[0029] In a preferred embodiment, the standing is performed for 5 to 30 minutes, for example, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes or 30 minutes.

[0030] In a preferred embodiment, the structural color solutions of different colors can be obtained by using microspheres of different particle sizes.

[0031] In a further preferred embodiment, the preparation method further optionally comprises: mixing the structural color solutions of different colors in any proportion to obtain a structural color solution of a new color.

[0032] In the present invention, the structural color solutions of different colors can be mixed to obtain a structural color solution with a new color.

[0033] In the present invention, the synergistic effect of hydrogen bonding aggregation and electrostatic repulsion of polyelectrolytes is used to induce the self-assembly of colloidal nanoparticles to prepare photonic crystal structural color ink. In this process, the polyelectrolytes cover the surface of the microspheres and play a dual role: on the one hand, the hydrogen bonding between the polyelectrolytes promotes the aggregation of the microspheres; on the other hand, the electrostatic repulsion of the polyelectrolytes increases the repulsive force between the colloidal nanoparticles. This dual effect of repulsion and aggregation jointly promotes the nanoparticles to form a short-range ordered arrangement structure. As a result, the nanoparticles can self-assemble into a short-range ordered array, thereby forming an angle-independent structural color.

[0034] The third object of the present invention is to provide a method for preparing a low-viscosity thermosetting structural color ink, comprising: mixing raw materials including the composition described in one of the objects of the present invention, polymer monomers, crosslinking agents, and initiators, ultrasonicating, and allowing to stand.

[0035] In a preferred embodiment, the polymer monomer is selected from polymerizable monomers having an amide structure in the side chain, preferably at least one selected from acrylamide, methacrylamide, N-isopropylacrylamide, and diacetoneacrylamide.

[0036] In a further preferred embodiment, the mass fraction of the polymer monomer in the low-viscosity thermosetting structural color ink water is 10-70%, preferably 20%-50%, for example 10%, 20%, 30%, 40%, 50%, 60% or 70%.

[0037] In a preferred embodiment, the cross-linking agent is selected from N,N'-methylenebisacrylamide.

[0038] In a further preferred embodiment, the mass fraction of the crosslinking agent in the low-viscosity thermosetting structural color ink is 0.01% to 10%, preferably 0.05% to 5%, for example 0.01%, 0.02%, 0.05%, 0.08%, 0.1%, 0.2%, 0.5%, 0.8%, 1% 2%, 3%, 4% or 5%.

[0039] In a preferred embodiment, the initiator is selected from a thermal initiator and / or a photoinitiator. Preferably, the thermal initiator is at least one of ammonium persulfate and potassium persulfate, and the photoinitiator is selected from at least one of photoinitiator 2959 and photoinitiator 184.

[0040] In a further preferred embodiment, the mass fraction of the initiator in the low viscosity thermosetting structural color ink is 0.5% to 15%, preferably 1% to 10%, for example 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.

[0041] In a preferred embodiment, the ultrasonication is performed for 2 to 40 minutes, for example, 2 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes.

[0042] In a preferred embodiment, the standing is performed for 5 to 30 minutes, for example, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes or 30 minutes.

[0043] The low-viscosity thermosetting structural color ink of the present invention can be processed in multiple modes, including injection molding, painting, and 3D printing.

[0044] In the present invention, under the combined effect of the induced aggregation of the polyanion electrolyte molecular chains and the charge repulsion between the microspheres, the microspheres are arranged into a locally ordered structure, which affects the reflection of light and forms a structural color. Scanning electron microscope image after hydrogel fixation ( Fig. 9 ) also confirmed this conclusion. The green area is a regularly arranged ordered structure, and the red area is randomly dispersed microspheres. The inventors speculate that the reflection of the microspheres is composed of two parts: (1) the reflection of the short-range ordered microstructure, which is the reason for the reflection peak; (2) the Rayleigh scattering of the unassembled isolated microspheres, which causes a larger diffuse reflectivity at a smaller wavelength.

[0045] The fourth object of the present invention is to provide a structural color hydrogel, which is obtained by polymerizing the low-viscosity heat-curable structural color ink described in the third object of the present invention.

[0046] In a preferred embodiment, the polymerization is photopolymerization or thermal polymerization.

[0047] In a further preferred embodiment, the photopolymerization is polymerization under UV, and the temperature of the thermal polymerization is 40-70°C (eg, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C).

[0048] Traditional structural color materials reported before often have the property of changing color when stretched, but the color of the structural color hydrogel described in the present invention is not sensitive to stretching, which is more inclined to the nature of dyes. The reason for this property is that the local ordered structure inside the structural color hydrogel is relatively small and evenly distributed. During the deformation process of the material, no large deformation will occur to change the structural color. In addition, the mechanical properties of the structural color hydrogel were tested, and it was found that the addition of microspheres would slightly increase the breaking strength.

[0049] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be regarded as specifically disclosed in this article.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] 1. By utilizing the synergistic effect of hydrogen bonding aggregation and electrostatic repulsion of polyelectrolytes, ultra-low concentrations of charged microspheres can form structural colors in solution without the need for other complex treatments;

[0052] Second, structural color ink can not only adjust the color by changing the particle size of the microspheres in the traditional way, but also adjust the color continuously by mixing different colors, which greatly facilitates the adjustment of structural color;

[0053] 3. The present invention designs a preparation and molding strategy for a polyelectrolyte-induced low-viscosity thermally curable structural color ink. The method is simple and flexible, and opens up a new path for the construction of structural color ink.

[0054] Fourth, the structural color hydrogel material prepared by using the low-viscosity heat-curing structural color ink can maintain its structural color for a long time, and the color remains almost unchanged after being placed for several months (for example, 8 months). BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 Digital photos of the structural color solutions prepared in Examples 1-5 (from left to right, respectively, Examples 1 to 5) and reflection spectra;

[0056] Figure 2 Digital photos of the structural color solutions prepared in Examples 6-10 (from left to right are Examples 6 to 10 respectively);

[0057] Figure 3 Digital photos of the structural color solutions prepared in Examples 11 to 15 (from left to right are Examples 11 to 15 respectively);

[0058] Figure 4 Digital photos and reflection spectra of the structural color solutions prepared in Examples 16-17;

[0059] Figure 5 Digital photos of the structural color hydrogels prepared in Examples 28-32;

[0060] Figure 6 This is a digital photo of the structural color hydrogel prepared in Example 33;

[0061] exist Figure 6 (a) Schematic diagram of high-viscosity structural color ink that can be painted; (b) stretchability and non-discoloration of photocurable patterns; (c) structural color patterns prepared by large-scale painting;

[0062] Figure 7 This is a digital photo of the structural color hydrogel prepared in Example 34;

[0063] Figure 8 Optical images of the structural color hydrogel prepared in Example 31 before and after stretching;

[0064] Fig. 9The SEM image of the structural color hydrogel prepared in Example 30 after freeze-drying is shown. DETAILED DESCRIPTION

[0065] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0066] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0067] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0068] Scanning electron microscope (SEM) test: The morphology of the hydrogel was characterized using a scanning electron microscope (FEIQuanta 250FEG) produced by Hitachi, Japan, at 10kV. It is a high-resolution microscope that uses the interaction of electron beams with samples to generate signals. The hydrogel samples were freeze-dried and then fractured at low temperature in liquid nitrogen. Before characterization, the surface was treated with gold spraying using an ion sputtering instrument.

[0069] UV / Visible spectrophotometer test: The reflectance spectrum of the sample is measured by UV / Visible spectrophotometer. A standard plate is used for calibration before the test. The measurement wavelength range is 380-800nm.

[0070] Mechanical properties test: A universal testing machine (WDW-5T, China) was used to test the breaking strength and elongation of the samples. The maximum range of the universal testing machine is 250N, the tensile rate is 5mm / min, and the initial distance is 15mm. The length, width, height and other parameters of the hydrogel film were measured and recorded using instruments such as rulers, vernier calipers, and thickness gauges for use when processing data.

[0071] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0072] Preparation of PS-PMMA-PAA microspheres: A one-pot method was used to synthesize the aqueous dispersion solution of PS-PMMA-PAA microspheres. A precursor solution was prepared by adding 1.5 g of methyl methacrylate (MMA), 1.5 g of acrylic acid (AA), 28.5 g of styrene (St), 0.5 g of ammonium bicarbonate (buffering agent) and surfactant SDBS (mass ratio to monomer: 1:0.015-0.090) to 100 mL of deionized water. After stirring at 70 ° C for 30 minutes, 0.793 g of APS (initiator) was added to prepare a precursor solution of PS-PMMA-PAA microsphere particles. The synthesis of PS-PMMA-PAA microsphere particles was carried out at 80 ° C under mechanical stirring for 10 hours. The obtained aqueous dispersion solution of PS-PMMA-PAA microsphere particles was used directly without purification.

[0073] SiO 2 -COOH microspheres and PS-COOH microspheres were purchased from Jiangsu Zhichuan Technology Co., Ltd.

[0074] The microsphere particle dispersion solution is an aqueous solution.

[0075] [Example 1]

[0076] By adding 100 μL of a 267 nm PS-PMMA-PAA microsphere dispersion solution (20 v / v%) to a 20 ml, 0.3 wt % sodium alginate solution (molecular weight 200 kDa), after ultrasonic treatment for 5 minutes, the mixture solution was placed at room temperature and pressure for about 20 minutes to obtain a structural color solution A (such as Figure 1 shown).

[0077] [Example 2]

[0078] The process of Example 1 was repeated, except that the particle size of the microspheres was changed to 252 nm. The other operations were the same as those of Example 1, and another color of structural color solution B (such as Figure 1 shown).

[0079] [Example 3]

[0080] The process of Example 1 was repeated, except that the particle size of the microspheres was changed to 215 nm. The other operations were the same as those of Example 1, and another color of structural color solution C (such as Figure 1 shown).

[0081] [Example 4]

[0082] The process of Example 1 was repeated, except that the particle size of the microspheres was changed to 188 nm. The other operations were the same as those of Example 1 to obtain another color structural color solution D (such as Figure 1 shown).

[0083] [Example 5]

[0084] The process of Example 1 was repeated, except that the particle size of the microspheres was changed to 177 nm. The other operations were the same as those of Example 1, and another color of structural color solution E (such as Figure 1 shown).

[0085] [Example 6]

[0086] By adding 100 μL of a 267 nm PS-PMMA-PAA microsphere dispersion solution (20 v / v%) to a 20 ml, 0.3 wt % carboxymethyl cellulose (molecular weight 250 kDa) solution, after ultrasonic treatment for 5 minutes, the mixture solution was placed at room temperature and pressure for about 20 minutes to obtain a structural color solution (such as Figure 2 shown).

[0087] [Example 7]

[0088] The process of Example 6 was repeated, except that the particle size of the microspheres was changed to 252 nm. The other operations were the same as those of Example 1 to obtain a structural color solution of another color (such as Figure 2 shown).

[0089] [Example 8]

[0090] The process of Example 6 was repeated, except that the particle size of the microspheres was changed to 215 nm. The other operations were the same as those of Example 1 to obtain a structural color solution of another color (such as Figure 2 shown).

[0091] [Example 9]

[0092] The process of Example 6 was repeated, except that the particle size of the microspheres was changed to 188 nm. The other operations were the same as those of Example 1 to obtain a structural color solution of another color (such as Figure 2 shown).

[0093] [Example 10]

[0094] The process of Example 6 was repeated, except that the particle size of the microspheres was changed to 177 nm. The other operations were the same as those of Example 1 to obtain a structural color solution of another color (such as Figure 2 shown).

[0095] [Example 11]

[0096] By adding 100 μL of a 267 nm PS-PMMA-PAA microsphere dispersion solution (20 v / v%) to a 20 ml, 0.3 wt % k-carrageenan (molecular weight 300 kDa) solution, after ultrasonic treatment for 5 minutes, the mixture solution was placed at room temperature and pressure for about 20 minutes to obtain a structural color solution (such as Figure 3 shown).

[0097] [Example 12]

[0098] The process of Example 11 was repeated, except that the particle size of the microspheres was changed to 252 nm. The other operations were the same as those of Example 1 to obtain a structural color solution of another color (such as Figure 3 shown).

[0099] [Example 13]

[0100] The process of Example 11 was repeated, except that the particle size of the microspheres was changed to 215 nm. The other operations were the same as those of Example 1 to obtain a structural color solution of another color (such as Figure 3 shown).

[0101] [Example 14]

[0102] The process of Example 11 was repeated, except that the particle size of the microspheres was changed to 188 nm. The other operations were the same as those of Example 1 to obtain a structural color solution of another color (such as Figure 3 shown).

[0103] [Example 15]

[0104] The process of Example 11 was repeated, except that the particle size of the microspheres was changed to 177 nm. The other operations were the same as those of Example 1 to obtain a structural color solution of another color (such as Figure 3 shown).

[0105] [Example 16]

[0106] By adding 100 μL of PS-COOH microsphere particle dispersion solution with a particle size of 260 nm (20 v / v%) to 20 ml of 0.3 wt% sodium alginate (molecular weight 200 kDa) solution, after ultrasonic treatment for 5 minutes, the mixture solution is placed at room temperature and pressure for about 20 minutes to obtain a structural color solution.

[0107] [Example 17]

[0108] By adding 100 μL of SiO2 with a particle size of 260 nm to 20 ml of 0.3 wt% sodium alginate (molecular weight 200 kDa) solution, 2-COOH microsphere particle dispersion solution (20 v / v%), after ultrasonic treatment for 5 minutes, the mixture solution is placed at room temperature and pressure for about 20 minutes to obtain a structural color solution.

[0109] [Example 18]

[0110] Take 2.5mL of the above structural color solution A and 7.5ml of the above structural color solution B and place them in a beaker, add 1.25mg of carbon black, mix well and let stand for 20 minutes to obtain a new structural color solution AB, whose reflection spectrum peak is located between the structural color solutions A and B.

[0111] [Example 19]

[0112] The process of Example 18 was repeated, except that 2.5 mL of the structural color solution A and 7.5 mL of the structural color solution C were taken, and other conditions remained unchanged to obtain a new structural color solution AC.

[0113] [Example 20]

[0114] The process of Example 18 was repeated, except that 2.5 mL of the structural color solution A and 7.5 mL of the structural color solution D were taken, and other conditions remained unchanged to obtain a new structural color solution AD.

[0115] [Example 21]

[0116] The process of Example 18 was repeated, except that 2.5 mL of the structural color solution A and 7.5 mL of the structural color solution E were taken, and other conditions remained unchanged to obtain a new structural color solution AE.

[0117] [Example 22]

[0118] The process of Example 18 was repeated, except that 2.5 mL of the structural color solution B and 7.5 mL of the structural color solution C were taken, and other conditions remained unchanged to obtain a new structural color solution BC.

[0119] [Example 23]

[0120] The process of Example 18 was repeated, except that 2.5 mL of the structural color solution B and 7.5 mL of the structural color solution D were taken, and other conditions remained unchanged to obtain a new structural color solution BD.

[0121] [Example 24]

[0122] The process of Example 18 was repeated, except that 2.5 mL of the structural color solution B and 7.5 mL of the structural color solution E were taken, and other conditions remained unchanged to obtain a new structural color solution BE.

[0123] [Example 25]

[0124] The process of Example 18 was repeated, except that 2.5 mL of the structural color solution C and 7.5 mL of the structural color solution D were taken, and other conditions remained unchanged to obtain a new structural color solution CD.

[0125] [Example 26]

[0126] The process of Example 18 was repeated, except that 2.5 mL of the structural color solution C and 7.5 mL of the structural color solution E were taken, and other conditions remained unchanged to obtain a new structural color solution CE.

[0127] [Example 27]

[0128] The process of Example 18 was repeated, except that 2.5 mL of the structural color solution D and 7.5 mL of the structural color solution E were taken, and other conditions remained unchanged to obtain a new structural color solution DE.

[0129] [Example 28]

[0130] 6.0g acrylamide monomer, 0.01g crosslinker (N,N'-methylenebisacrylamide), 0.06g thermal initiator ammonium persulfate, 20v / v% PS-PMMA-PAA microsphere particle dispersion solution with a particle size of 267nm (0.10mL) were added to 20mL sodium alginate (molecular weight 650,000 Da) solution (0.30wt%). After ultrasonic dispersion for 5 minutes, the mixed solution was placed at room temperature and pressure for about 20 minutes to obtain a low-viscosity heat-curable structural color ink. The low-viscosity heat-curable structural color ink was injected into the specified mold, heated to 50°C in an oven, and polymerized for 8 hours to obtain a structural color hydrogel.

[0131] [Example 29]

[0132] The process of Example 28 was repeated, except that the particle size of the microspheres was changed to 252 nm and other conditions remained unchanged.

[0133] [Example 30]

[0134] The process of Example 28 was repeated, except that the particle size of the microspheres was changed to 215 nm and other conditions remained unchanged.

[0135] like Fig. 9 The SEM images show that there are a large number of short-range ordered structures (green circles) and unassembled isolated microspheres (red circles). Due to the short-range ordered structures, the structural color is independent of the angle.

[0136] [Example 31]

[0137] The process of Example 28 was repeated, except that the particle size of the microspheres was changed to 188 nm and other conditions remained unchanged.

[0138] The structural color hydrogel obtained in Example 31 was stretched, and it can be seen that it does not change color after stretching.

[0139] [Example 32]

[0140] The process of Example 28 was repeated, except that the particle size of the microspheres was changed to 177 nm and other conditions remained unchanged.

[0141] [Example 33]

[0142] Painting structural color hydrogel:

[0143] 1. A composition A' was obtained by adding 100 μL of a PS-PMMA-PAA microsphere dispersion solution (20 v / v%) with a particle size of 267 nm to a 20 ml, 1.0 wt% mixed solution of sodium alginate (molecular weight of 200 kDa) and 1.0 wt% carrageenan (molecular weight of 300 kDa); the same operation was performed to obtain compositions B', C', D', and E' by changing the particle size of the microspheres (252 nm, 215 nm, 188 nm, and 177 nm);

[0144] 2. Add acrylamide (AM, 6.00 g), photoinitiator 2959 (2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 0.60 g), N',N'-methylenebisacrylamide (MBAA, 0.01 g), and carbon black (2.5 mg) to compositions A', B', C', D', and E', respectively. After ultrasonic dispersion for 5 minutes, let stand for 20 minutes to obtain low-viscosity thermal curing structural color inks of different colors.

[0145] The low-viscosity heat-curable structural color inks of different colors were used for writing and drawing with a brush and a pen made in the laboratory. The multicolor structural color pattern was then irradiated with an ultraviolet lamp (18 W, 365 nm) for 18 minutes. After polymerization, a multicolor pattern of a stretchable structural color hydrogel with a multicolor structural color pattern (such as Figure 6 shown).

[0146] exist Figure 6 As can be seen in the figure, when the floret hydrogel is stretched, it can be seen that it does not change color after stretching.

[0147] [Example 34]

[0148] 3D printing structural color hydrogel:

[0149] 1. A composition A" was obtained by adding 100 μL of a PS-PMMA-PAA microsphere particle dispersion solution (20 v / v%) with a particle size of 267 nm to a 20 ml, 1.0 wt% mixed solution of sodium alginate (molecular weight of 200 kDa) and 2.0 wt% carrageenan (molecular weight of 300 kDa); the same operation was performed to obtain compositions B", C", D", and E" by changing the particle size of the microspheres (252 nm, 215 nm, 188 nm, and 177 nm);

[0150] 2. Add acrylamide (AM, 6.00 g), photoinitiator 2959 (2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 0.60 g), N',N'-methylenebisacrylamide (MBAA, 0.01 g), and carbon black (2.5 mg) to compositions A", B", C", D", and E", respectively, to form low-viscosity thermal curing structural color inks of different colors.

[0151] The low-viscosity heat-curable structural color ink has a high viscosity at high temperature (50° C.), and when the temperature drops to 32° C., the solution will quickly transform into a gel state.

[0152] The CELLINK BIO X 3D printer was used to perform 3D printing using the low-viscosity heat-curable structural color inks of different colors. During the 3D printing process, the ink temperature was controlled at 50° C. An ultraviolet lamp (18 W, 365 nm) was used to further cure for 20 minutes to obtain a structural color 3D hydrogel.

[0153] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A structural color solution composition comprising microspheres, a polyanion electrolyte and water.

2. The structural color solution composition according to claim 1, characterized in that: The polyanion electrolyte is selected from polymers containing multiple hydroxyl groups and multiple anion groups; preferably, the polyanion electrolyte is selected from at least one of sodium alginate, carrageenan, and sodium carboxymethyl cellulose; more preferably, the molecular weight of the polyanion electrolyte is 1 to 2 million Da, preferably 200,000 to 1.5 million Da; further preferably, the mass concentration of the polyanion electrolyte in the composition is 0.01wt% to 5wt%.

3. The structural color solution composition according to claim 1, characterized in that: The surface of the microsphere contains groups that can form electrostatic effects with hydroxyl groups. Preferably, the microsphere is selected from microspheres containing carboxyl groups on the surface. More preferably, the particle size of the microsphere is 120 to 350 nm, preferably 150 to 300 nm; further preferably, the concentration of the microsphere in the composition is 0.01 v / v% to 1.0 v / v%.

4. The structural color solution composition according to any one of claims 1 to 3, characterized in that: The composition optionally contains carbon black; preferably, the content of the carbon black in the composition is 0.001 wt% to 0.01 wt%.

5. A method for preparing a structural color solution, comprising: The composition according to any one of claims 1 to 4 is subjected to ultrasound and allowed to stand to obtain the structural color solution; preferably, the ultrasound is performed for 2 to 40 minutes, and / or the standing is performed for 5 to 30 minutes.

6. The preparation method according to claim 5, characterized in that: The preparation method further optionally includes: mixing the structural color solutions of different colors in any proportion to obtain a structural color solution of a new color.

7. A method for preparing a low-viscosity thermally curable structural color ink, comprising: The raw materials including the composition according to any one of claims 1 to 4, polymer monomers, a crosslinking agent and an initiator are mixed, ultrasonicated and allowed to stand.

8. The preparation method according to claim 7, characterized in that: The polymer monomer is selected from polymerizable monomers having an amide structure in the side chain, preferably at least one of acrylamide, methacrylamide, N-isopropylacrylamide, and diacetoneacrylamide; more preferably, the mass fraction of the polymer monomer in the low-viscosity thermal curing structural color ink water is 10% to 70%, preferably 20% to 50%; and / or, The cross-linking agent is selected from N,N'-methylenebisacrylamide. Preferably, the mass fraction of the cross-linking agent in the low-viscosity thermal curing structural color ink is 0.01% to 10%, preferably 0.05% to 5%; and / or, The initiator is selected from a thermal initiator and / or a photoinitiator. Preferably, the thermal initiator is at least one of ammonium persulfate and potassium persulfate, and the photoinitiator is at least one of photoinitiator 2959 and photoinitiator 184. More preferably, the mass fraction of the initiator in the low-viscosity thermal curing structural color ink is 0.5% to 15%, preferably 1% to 10%.

9. The preparation method according to claim 7 or 8, characterized in that: The ultrasonication is performed for 2 to 40 minutes, and / or the standing is performed for 5 to 30 minutes.

10. A structural color hydrogel obtained by polymerizing the low-viscosity heat-curable structural color ink according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • Preparation method of structural-color fabric

    CN106894245A

  • Preparation and application for dye-doped nanosphere type structural coloring ink used for textile digital jet printing

    CN106947318A

  • Preparation and application of writable structure coloring ink

    CN109810566A

  • Structural chromogenic finishing liquid for preparing high-stability photonic crystal, and application of structural chromogenic finishing liquid

    CN111379174A

  • Structural chromogenic cellulose fabric and preparation method thereof

    CN115323799A