Manufacturing method of multifunctional paper-like cold stamping film and packaging bag
By modifying mica powder and chitosan composite and forming an alumina coating layer on the polyethylene film, the waterproof performance and compatibility problems of the packaging bag materials are solved, and the gas and water vapor barrier properties of the packaging bags are significantly improved, and the lengthening of the packaging bags is extended. The storage cycle of packaging products is improved and the environmental protection and practicality of the materials are improved.
Patent Information
- Application Number
- CN202410972478.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing packaging bag materials have shortcomings in waterproof performance and food safety. The paper packaging bags have poor waterproof performance, plastic packaging bags have poor hand feel and have a great impact on the environment, and the compatibility of mica powder and polyvinyl alcohol coatings is poor. Influence its application.
Using natural material cinnamaldehyde as a modifier, mica powder and chitosan composites are modified to reduce the hydrophilicity of mica, and alumina coating layer is formed on the BOPE polyethylene film substrate and polyvinyl alcohol is coated. Coatings improve their mechanical properties, water resistance and gas barrier properties.
It significantly improves the gas barrier and water vapor barrier properties of the packaging bag, extends the storage cycle of the packaging, improves the compatibility and reactivity of the materials, and enhances the practicality and environmental protection of the packaging bag.
Smart Images

Figure BDA0004953630280000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of packaging bag materials and relates to a multifunctional paper-like cold stamping film and a manufacturing method of a packaging bag. Background Art
[0002] With the rapid growth of social economy and the gradual improvement of people's quality of life, packaging bags have become an indispensable item in daily life due to their rich colors, multi-functions and various shapes. Generally speaking, flexible packaging bags can be divided into three categories: paper packaging bags, plastic packaging bags and paper-plastic composite packaging bags.
[0003] Although paper packaging bags have the advantage of being recyclable, they have poor waterproof performance, which makes the food inside easily get damp and deteriorate. In addition, the production process of pulp not only consumes a lot of forest resources, but also leaves certain chemical substances in the paper, which easily leads to food safety problems. Plastic packaging bags have better toughness and are also oil- and water-resistant, but they feel poor and consumers have a relatively low perception of their quality.
[0004] In recent years, paper-plastic composite packaging bags have become the most popular packaging products. They cleverly combine the advantages of paper packaging bags and plastic packaging bags. They not only have the oil and water resistance of plastic packaging bags, but also have the recyclability of paper packaging bags, which greatly improves the practicality and environmental protection of packaging. Polyvinyl alcohol-based materials have many advantages such as green and degradable. Among the methods of improving the barrier properties of materials, surface coating is relatively easy to achieve, with simple process and relatively low production cost.
[0005] Mica powder is a non-metallic mineral containing multiple components, among which the main component is SiO2, which is generally around 49% and Al2O3 is around 30%. Its structure is a layered complex aluminum silicate composed of pairs of aluminum-oxygen octahedra. It has high resistance to heat and acid and alkali corrosion. Its lamellar structure can enhance the barrier properties of film materials to oxygen and water vapor. However, as an inorganic filler, it has poor compatibility with polyvinyl alcohol coatings, which affects its application in film materials. Summary of the invention
[0006] The purpose of the present invention is to provide a method for manufacturing a multifunctional paper-like cold-stamping film and a packaging bag. The present invention uses cinnamaldehyde grafted oleic acid of natural materials as a modifier to modify the mica powder and chitosan complex, while reducing the hydrophilicity of the mica, introducing organic groups, increasing its reactivity and compatibility with the polyvinyl alcohol coating system, and improving its mechanical properties, water resistance and gas barrier properties. Finally, an aluminum oxide coating layer is formed on the BOPE polyethylene film substrate and the polyvinyl alcohol coating is coated and cured, and the packaging bag finally obtained can increase the storage period of the packaged product.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A multifunctional paper-like cold-foil film is obtained by curing a polyvinyl alcohol coating, wherein the polyvinyl alcohol coating comprises the following components by weight: 38-44 parts of polyvinyl alcohol, 1.8-2.1 parts of a cross-linking agent, 0.1-0.2 parts of EDC, 7-10 parts of modified mica, 0.06-0.09 parts of an antioxidant and 34-40 parts of deionized water.
[0009] As a preferred technical solution of the present invention, the cross-linking agent is one or more of glutaraldehyde, vanillin and citral.
[0010] As a preferred technical solution of the present invention, the antioxidant is a mixture of antioxidant 168 and antioxidant 1010 in a mass ratio of 1:2.
[0011] As a preferred technical solution of the present invention, the EDC is 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide.
[0012] The invention discloses that the preparation of the modified mica comprises the following steps:
[0013] Step S1: cinnamaldehyde and an initiator are stirred and mixed, and then preheated. In a nitrogen atmosphere, oleic acid is added dropwise, stirred and mixed, and then heat-insulated to obtain a modifier;
[0014] Step S2: placing chitosan solution and mica powder in a container and stirring and mixing, adding anhydrous ethanol and a modifier, heating and stirring and mixing, removing the solvent by rotary evaporation, washing, placing in an oven for drying, and obtaining modified mica.
[0015] As a preferred technical solution of the present invention, mica powder can effectively increase the barrier properties of the material as well as the water resistance and anti-penetration properties of the film due to its unique flaky stacking structure.
[0016] As a preferred technical solution of the present invention, in step S1, the mass ratio of cinnamaldehyde, initiator and oleic acid is 20-23:30-36:1.0-1.2.
[0017] As a preferred technical solution of the present invention, in step S1, the preheating is heating to a temperature of 70-75°C; and the heat preservation treatment is heat preservation treatment at a temperature of 70-75°C for 4-6 hours.
[0018] As a preferred technical solution of the present invention, in step S1, the initiator is one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, diethyl azodicarboxylate, benzoyl peroxide and tert-butyl perbenzoate.
[0019] As a preferred technical solution of the present invention, in step S2, the stirring and mixing is stirring at a temperature of 30-36° C. for 30-45 minutes.
[0020] As a preferred technical solution of the present invention, in step S2, the heating and stirring and mixing is heating to 60-70°C and stirring and mixing for 6-8h.
[0021] As a preferred technical solution of the present invention, in step S2, the washing is performed by washing with anhydrous ethanol for 3 times; and the drying is performed by drying at a temperature of 80° C. to a constant weight.
[0022] As a preferred technical solution of the present invention, in step S2, the mass ratio of the chitosan solution, mica powder, anhydrous ethanol and modifier is 10-12: 5-7: 15-20: 0.6-1.0.
[0023] As a preferred technical solution of the present invention, in step S2, the chitosan solution is prepared by stirring and mixing chitosan and acetic acid aqueous solution in a dosage ratio of 0.10-0.13 g:4 mL, and the mass fraction of the acetic acid aqueous solution is 2%.
[0024] As a preferred technical solution of the present invention, the multifunctional paper-like cold stamping film is obtained by curing polyvinyl alcohol coating, and the preparation method of the polyvinyl alcohol coating includes the following steps: mixing polyvinyl alcohol and deionized water, heating to 65°C, adding modified mica, EDC and a cross-linking agent, and stirring for 30-45 minutes to obtain the polyvinyl alcohol coating.
[0025] The present invention discloses a method for preparing a packaging bag made by using a multifunctional paper-like cold stamping film, and the method for preparing the packaging bag comprises the following steps:
[0026] With the help of the electron beam gun of the electron beam winding coating equipment, the reactants of high-purity aluminum material and high-purity oxygen are evaporated onto the BOPE polyethylene film substrate in a high temperature environment of 1400-1600°C and a vacuum state to form an aluminum oxide coating layer. Then, polyvinyl alcohol water-based coating is applied on the aluminum oxide coating layer and cured, cut, folded in half, and heat-sealed to form packaging bags.
[0027] Beneficial effects of the present invention:
[0028] The present invention adopts cinnamaldehyde grafted oleic acid of natural materials as a modifier to modify the mica powder and chitosan complex, while reducing the hydrophilicity of the mica, introducing organic groups, increasing its reactivity and compatibility with the polyvinyl alcohol coating system, and improving its mechanical properties, water resistance and gas barrier properties. First, an aluminum oxide coating layer is formed on a BOPE polyethylene film substrate and the polyvinyl alcohol coating is applied for curing, and the packaging bag finally prepared can increase the storage period of the packaged product. DETAILED DESCRIPTION
[0029] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.
[0030] A method for preparing a packaging bag made of a multifunctional paper-like cold foil film comprises the following steps:
[0031] With the help of the electron beam gun of the electron beam winding coating equipment, the reactants of high-purity aluminum material and high-purity oxygen are evaporated onto the BOPE polyethylene film substrate in a high temperature environment of 1400-1600°C and a vacuum state to form an aluminum oxide coating layer. Then, polyvinyl alcohol water-based coating is applied on the aluminum oxide coating layer and cured to form a multifunctional paper-like cold stamping film, which is then cut, folded in half, and heat-sealed to form packaging bags.
[0032] Example 1
[0033] A multifunctional paper-like cold-stamping film is obtained by curing a polyvinyl alcohol coating, wherein the polyvinyl alcohol coating comprises the following components by weight: 38 parts of polyvinyl alcohol, 1.8 parts of a cross-linking agent, 0.1 parts of EDC, 7 parts of modified mica, 0.06 parts of an antioxidant, and 34 parts of deionized water; the cross-linking agent is prepared by mixing glutaraldehyde and citral in a mass ratio of 2:1; the antioxidant is prepared by mixing antioxidant 168 and antioxidant 1010 in a mass ratio of 1:2;
[0034] The preparation of the modified mica comprises the following steps:
[0035] Step S1: stirring and mixing cinnamaldehyde and an initiator, preheating the mixture, adding oleic acid dropwise, stirring and mixing the mixture under a nitrogen atmosphere, and then heat-insulating the mixture to obtain a modifier; wherein the mass ratio of cinnamaldehyde, initiator and oleic acid is 20:30:1.0; the preheating is heating to 70°C; the heat-insulating treatment is heat-insulating treatment at 70°C for 4 hours; the initiator is azobisisobutyronitrile;
[0036] Step S2: placing chitosan solution and mica powder in a container and stirring and mixing, adding anhydrous ethanol and a modifier, heating and stirring and mixing, rotary evaporating to remove the solvent, washing, placing in an oven for drying, and obtaining modified mica; wherein, the stirring and mixing is stirring at 30°C for 30 minutes; the heating and stirring and mixing is heating to 60°C and stirring and mixing for 6 hours; the washing is washing 3 times with anhydrous ethanol; the drying is drying at 80°C to constant weight; the mass ratio of the chitosan solution, mica powder, anhydrous ethanol and modifier is 10:5:15:0.6; the chitosan solution is prepared by stirring and mixing chitosan and acetic acid aqueous solution in a dosage ratio of 0.10g:4mL, and the mass fraction of the acetic acid aqueous solution is 2%.
[0037] The preparation method of the polyvinyl alcohol coating comprises the following steps: mixing polyvinyl alcohol and deionized water, heating to 65° C., adding modified mica, EDC, an antioxidant and a crosslinking agent, and stirring for 30 minutes to obtain the polyvinyl alcohol coating.
[0038] Example 2
[0039] A multifunctional paper-like cold-stamping film is obtained by curing a polyvinyl alcohol coating, wherein the polyvinyl alcohol coating comprises the following components by weight: 40 parts of polyvinyl alcohol, 1.9 parts of a cross-linking agent, 0.13 parts of EDC, 8 parts of modified mica, 0.07 parts of an antioxidant, and 36 parts of deionized water; the cross-linking agent is prepared by mixing glutaraldehyde and citral in a mass ratio of 2:1; the antioxidant is prepared by mixing antioxidant 168 and antioxidant 1010 in a mass ratio of 1:2;
[0040] The preparation of the modified mica comprises the following steps:
[0041] Step S1: stirring and mixing cinnamaldehyde and an initiator, preheating the mixture, adding oleic acid dropwise, stirring and mixing the mixture under a nitrogen atmosphere, and then heat-insulating the mixture to obtain a modifier; wherein the mass ratio of cinnamaldehyde, initiator and oleic acid is 21:32:1.07; the preheating is heating to 72°C; the heat-insulating treatment is heat-insulating treatment at 72°C for 4.5h; the initiator is azobisisobutyronitrile;
[0042] Step S2: placing chitosan solution and mica powder in a container and stirring and mixing, adding anhydrous ethanol and a modifier, heating and stirring and mixing, rotary evaporating to remove the solvent, washing, placing in an oven for drying, and obtaining modified mica; wherein, the stirring and mixing is stirring at 32°C for 35 minutes; the heating and stirring and mixing is heating to 63°C and stirring and mixing for 6.7 hours; the washing is washing 3 times with anhydrous ethanol; the drying is drying at 80°C to constant weight; the mass ratio of the chitosan solution, mica powder, anhydrous ethanol and modifier is 10.7:5.7:17:0.7; the chitosan solution is prepared by stirring and mixing chitosan and acetic acid aqueous solution in a dosage ratio of 0.11 g:4 mL, and the mass fraction of the acetic acid aqueous solution is 2%.
[0043] The preparation method of the polyvinyl alcohol coating comprises the following steps: mixing polyvinyl alcohol and deionized water, heating to 65° C., adding modified mica, EDC, an antioxidant and a crosslinking agent, and stirring for 35 minutes to obtain the polyvinyl alcohol coating.
[0044] Example 3
[0045] A multifunctional paper-like cold-stamping film is obtained by curing a polyvinyl alcohol coating, wherein the polyvinyl alcohol coating comprises the following components by weight: 42 parts of polyvinyl alcohol, 2 parts of a cross-linking agent, 0.17 parts of EDC, 9 parts of modified mica, 0.08 parts of an antioxidant, and 38 parts of deionized water; the cross-linking agent is prepared by mixing glutaraldehyde and citral in a mass ratio of 2:1; the antioxidant is prepared by mixing antioxidant 168 and antioxidant 1010 in a mass ratio of 1:2;
[0046] The preparation of the modified mica comprises the following steps:
[0047] Step S1: stirring and mixing cinnamaldehyde and an initiator, preheating the mixture, adding oleic acid dropwise, stirring and mixing the mixture under a nitrogen atmosphere, and then heat-insulating the mixture to obtain a modifier; wherein the mass ratio of cinnamaldehyde, initiator and oleic acid is 22:34:1.13; the preheating is heating to 73°C; the heat-insulating treatment is heat-insulating treatment at 73°C for 5.5h; the initiator is azobisisobutyronitrile;
[0048] Step S2: placing chitosan solution and mica powder in a container and stirring and mixing, adding anhydrous ethanol and a modifier, heating and stirring and mixing, rotary evaporating to remove the solvent, washing, placing in an oven for drying, and obtaining modified mica; wherein, the stirring and mixing is stirring at 34°C for 40 minutes; the heating and stirring and mixing is heating to 67°C and stirring and mixing for 7.5 hours; the washing is washing 3 times with anhydrous ethanol; the drying is drying at 80°C to constant weight; the mass ratio of the chitosan solution, mica powder, anhydrous ethanol and modifier is 11.3:6.3:18:0.9; the chitosan solution is prepared by stirring and mixing chitosan and acetic acid aqueous solution in a dosage ratio of 0.12 g:4 mL, and the mass fraction of the acetic acid aqueous solution is 2%.
[0049] The preparation method of the polyvinyl alcohol coating comprises the following steps: mixing polyvinyl alcohol and deionized water, heating to 65° C., adding modified mica, EDC, an antioxidant and a crosslinking agent, and stirring for 40 minutes to obtain the polyvinyl alcohol coating.
[0050] Example 4
[0051] A multifunctional paper-like cold-stamping film is obtained by curing a polyvinyl alcohol coating, wherein the polyvinyl alcohol coating comprises the following components by weight: 44 parts of polyvinyl alcohol, 2.1 parts of a cross-linking agent, 0.2 parts of EDC, 10 parts of modified mica, 0.09 parts of an antioxidant, and 40 parts of deionized water; the cross-linking agent is prepared by mixing glutaraldehyde and citral in a mass ratio of 2:1; the antioxidant is prepared by mixing antioxidant 168 and antioxidant 1010 in a mass ratio of 1:2;
[0052] The preparation of the modified mica comprises the following steps:
[0053] Step S1: stirring and mixing cinnamaldehyde and an initiator, preheating the mixture, adding oleic acid dropwise, stirring and mixing the mixture under a nitrogen atmosphere, and then heat-insulating the mixture to obtain a modifier; wherein the mass ratio of cinnamaldehyde, initiator and oleic acid is 23:36:1.2; the preheating is heating to 75°C; the heat-insulating treatment is heat-insulating treatment at 75°C for 6 hours; the initiator is azobisisobutyronitrile;
[0054] Step S2: placing chitosan solution and mica powder in a container and stirring and mixing, adding anhydrous ethanol and a modifier, heating and stirring and mixing, rotary evaporating to remove the solvent, washing, placing in an oven for drying, and obtaining modified mica; wherein, the stirring and mixing is stirring at 36°C for 45 minutes; the heating and stirring and mixing is heating to 70°C and stirring and mixing for 8 hours; the washing is washing 3 times with anhydrous ethanol; the drying is drying at 80°C to constant weight; the mass ratio of the chitosan solution, mica powder, anhydrous ethanol and modifier is 12:7:20:1.0; the chitosan solution is prepared by stirring and mixing chitosan and acetic acid aqueous solution in a dosage ratio of 0.13g:4mL, and the mass fraction of the acetic acid aqueous solution is 2%.
[0055] The preparation method of the polyvinyl alcohol coating comprises the following steps: mixing polyvinyl alcohol and deionized water, heating to 65° C., adding modified mica, EDC, an antioxidant and a crosslinking agent, and stirring for 45 minutes to obtain the polyvinyl alcohol coating.
[0056] Comparative Example 1
[0057] Compared with Example 3, Comparative Example 1 is different in that cinnamaldehyde is not used, and the remaining components, preparation steps and parameters are the same.
[0058] Comparative Example 2
[0059] Compared with Example 3, Comparative Example 2 is different in that oleic acid is not used, and the other components, preparation steps and parameters are the same.
[0060] Comparative Example 3
[0061] Compared with Example 3, Comparative Example 3 is different in that chitosan is not used, and the other components, preparation steps and parameters are the same.
[0062] Comparative Example 4
[0063] Compared with Example 3, the difference in Comparative Example 4 is that mica powder replaces modified mica, and the other components, preparation steps and parameters are the same.
[0064] Comparative Example 5
[0065] Compared with Example 3, Comparative Example 5 is different in that EDC is not used, and the other components, preparation steps and parameters are the same.
[0066] The polyvinyl alcohol coatings obtained in Examples 1-4 and Comparative Examples 1-5 were tested as follows. The test results are shown in Table 1.
[0067] Oxygen barrier performance test: According to GB / T1038-2000; use an air permeability tester to test the oxygen barrier performance of the film, use a standard sample knife to cut the sample film into a circle with a diameter of 8.5 cm, measure three samples for each sample, and take the average value.
[0068] Water vapor barrier performance test: According to GB / T 1037-88, the film was cut into a circle with an area of 50cm2 and tested using a water vapor transmission rate tester.
[0069] Table 1 Test results of oxygen barrier properties and water vapor barrier properties
[0070]
[0071] From the test results in Table 1, it can be seen that compared with Comparative Examples 1-5, the oxygen barrier performance and water vapor barrier performance of the film prepared in Examples 1-4 are significantly better than those in Comparative Examples 1-5. This is because the present invention adopts cinnamaldehyde grafted with oleic acid from natural materials as a modifier, and utilizes the hydrogen bonding between mica powder and chitosan to allow chitosan to enter the interlayer structure of mica powder, introduce amino groups, and then connect the amino groups with the aldehyde groups of the modifier through chemical bonds, thereby reducing the hydrophilicity of mica and grafting the mica powder as an inorganic filler with an organic group containing an imine structure, thereby increasing its reactivity and compatibility with the polyvinyl alcohol coating system. The modifier contains a carbon-carbon long chain and a benzene ring structure, and can also serve as a plasticizer to adjust the fluidity of the polyvinyl alcohol coating, improve its mechanical properties and water resistance, and thus improve the gas barrier performance of the polyvinyl alcohol coating under high humidity conditions. In addition, the present invention uses an aldehyde-containing compound as a cross-linking agent to undergo an acetalization cross-linking reaction with the hydroxyl group of polyvinyl alcohol to form a three-dimensional cross-linked network structure, and introduces active functional groups into the mica modified by the modifier, thereby increasing the compatibility of the mica in the polyvinyl alcohol coating system, and then uses EDC to activate the carboxyl groups on the modified mica to further increase the binding force between the mica and the polyvinyl alcohol coating, thereby forming a denser cross-linked network structure and significantly improving the mechanical properties and barrier properties of the polyvinyl alcohol coating.
[0072] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A multifunctional paper-like cold foil film, characterized in that: The multifunctional paper-like cold stamping film is obtained by curing a polyvinyl alcohol coating, wherein the polyvinyl alcohol coating comprises the following components by weight: 38-44 parts of polyvinyl alcohol, 1.8-2.1 parts of a cross-linking agent, 0.1-0.2 parts of EDC, 7-10 parts of modified mica, 0.06-0.09 parts of an antioxidant, and 34-40 parts of deionized water; Wherein, the preparation of the modified mica comprises the following steps: Step S1: cinnamaldehyde and an initiator are stirred and mixed, and then preheated. In a nitrogen atmosphere, oleic acid is added dropwise, stirred and mixed, and then heat-insulated to obtain a modifier; Step S2: placing chitosan solution and mica powder in a container and stirring and mixing, adding anhydrous ethanol and a modifier, heating and stirring and mixing, removing the solvent by rotary evaporation, washing, placing in an oven for drying, and obtaining modified mica.
2. The multifunctional paper-like cold foil film according to claim 1, characterized in that: The cross-linking agent is one or more of glutaraldehyde, vanillin and citral; the antioxidant is a mixture of antioxidant 168 and antioxidant 1010 in a mass ratio of 1:
2.
3. The multifunctional paper-like cold foil film according to claim 1, characterized in that: In step S1, the mass ratio of cinnamaldehyde, initiator and oleic acid is 20-23:30-36:1.0-1.
2.
4. The multifunctional paper-like cold foil film according to claim 1, characterized in that: In step S1, the preheating is heating to a temperature of 70-75°C; and the heat preservation treatment is heat preservation treatment at a temperature of 70-75°C for 4-6 hours.
5. The multifunctional paper-like cold foil film according to claim 1, characterized in that: In step S1, the initiator is one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, diethyl azodicarboxylate, benzoyl peroxide and tert-butyl perbenzoate.
6. The multifunctional paper-like cold foil film according to claim 1, characterized in that: In step S2, the stirring and mixing is stirring at a temperature of 30-36°C for 30-45 minutes; the heating and stirring and mixing is heating to 60-70°C and stirring and mixing for 6-8 hours; the washing is washing 3 times with anhydrous ethanol; and the drying is drying at a temperature of 80°C to constant weight.
7. The multifunctional paper-like cold foil film according to claim 1, characterized in that: In step S2, the mass ratio of the chitosan solution, mica powder, anhydrous ethanol and modifier is 10-12: 5-7: 15-20: 0.6-1.
0.
8. The multifunctional paper-like cold foil film according to claim 1, characterized in that: In step S2, the chitosan solution is prepared by stirring and mixing chitosan and acetic acid aqueous solution in a dosage ratio of 0.10-0.13 g:4 mL, and the mass fraction of the acetic acid aqueous solution is 2%.
9. The multifunctional paper-like cold foil film according to claim 1, characterized in that: The multifunctional paper-like cold-stamping film is obtained by curing polyvinyl alcohol coating. The preparation method of the polyvinyl alcohol coating comprises the following steps: mixing polyvinyl alcohol and deionized water, heating to 65° C., adding modified mica, EDC and a cross-linking agent, and stirring for 30-45 minutes to obtain the polyvinyl alcohol coating.
10. A method for preparing a packaging bag using the multifunctional paper-like cold foil film according to any one of claims 1 to 9, characterized in that: The method for preparing the packaging bag comprises the following steps: With the help of the electron beam gun of the electron beam winding coating equipment, the reactants of high-purity aluminum material and high-purity oxygen are evaporated onto the BOPE polyethylene film substrate in a high temperature environment of 1400-1600°C and a vacuum state to form an aluminum oxide coating layer. Then, polyvinyl alcohol water-based coating is applied on the aluminum oxide coating layer and cured, cut, folded in half, and heat-sealed to form packaging bags.
Citation Information
Patent Citations
Preparation method of food packaging film
CN109504009A
Preparation method of aluminum-free lining paper
CN111676729A
Gas barrier film and packaging material
US20190126601A1