Graphene modified water-based acrylate anticorrosive paint and preparation method thereof

Through the preparation of graphene modified aqueous acrylate anticorrosion coating, combined with graphene slurry and aqueous acrylate varnish, the problem of insufficient impact resistance of aqueous acrylate anticorrosion coating is solved, and high impact resistance and strong adhesion of the coating film is achieved And good salt spray resistance, suitable for moderate corrosion protection.

CN118895071AInactive Publication Date: 2024-11-05XINGTAI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410387418.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-01
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The impact resistance of existing aqueous acrylate anticorrosion coatings is poor, making it difficult to meet the comprehensive performance needs in the fields of moderate anticorrosion and light anticorrosion.

Method used

Use graphene slurry to combine with specific aqueous acrylate varnish and prepare it by the preparation of graphene powder, dispersant, defoaming agent, filler, neutralizing agent, film forming additive, anti-flash rust additive and thickening agent. Graphene modified aqueous acrylate anticorrosion coating is produced, and the graphene content is controlled at 1-5% to improve the impact resistance of the coating.

Benefits of technology

When the graphene content is 3%, the impact resistance of the coating film reaches 40cm, the hardness reaches 5H, the adhesion reaches level 0 standard, the salt water and salt spray resistance are both in line with national standards, and there is no crack or shedding on the surface of the coating film. The hardness is suitable, the adhesion is strong, and the salt spray resistance is up to 1200h.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895071A_ABST
    Figure CN118895071A_ABST
Patent Text Reader

Abstract

The invention relates to a graphene modified water-based acrylate anticorrosive coating which is prepared from graphene slurry and water-based acrylate varnish. The graphene slurry is prepared from water, graphene powder, a first dispersing agent and a first defoaming agent. The water-based acrylate varnish is prepared from water, a water-based acrylic emulsion, a second dispersing agent, a filler, a second defoaming agent, a neutralizer, a coalescing agent, an anti-flash-rust aid and a thickening agent. A coating prepared from the coating with the graphene content of 3% has the impact resistance of 40cm, the pencil hardness of 5H and the adhesive force of 0 grade, and meets the national standard in a saline water test and in a salt spray test of 1200 hours.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of coatings and anti-corrosion technology, and specifically to a graphene-modified water-based acrylate anti-corrosion coating and a preparation method thereof. Background Art

[0002] The coatings industry has gradually become an important industry that cannot be lacking in various fields. However, solvent-based coatings contain a large amount of volatile organic solvents (VOCs), which have become part of the source of air pollution. Water-based coatings have become a new trend in the development of the coatings industry due to their low pollution, easy purification, and non-irritating characteristics. Water-based acrylic anti-corrosion coatings have the advantages of easy construction, fast drying, weather resistance, and water resistance. They are generally used in moderate and mild corrosion protection fields. Water-based acrylic anti-corrosion coatings are single-component coatings. Compared with two-component coatings, they have the advantages of easy storage and easy use, but compared with two-component coatings, their performance is poorer, especially their impact resistance is poorer.

[0003] A Chinese invention patent application with publication number CN109627872A discloses a water-based acrylic anti-corrosion coating containing graphene, which uses a water-based acrylic emulsion and a water-based epoxy resin as main resins to prepare the coating. Its adhesion and salt spray resistance are evaluated, but its impact resistance is not evaluated. Summary of the invention

[0004] The purpose of the present application is to provide a graphene-modified water-based acrylate anti-corrosion coating with excellent impact resistance, thereby overcoming the defects in the above-mentioned prior art. Specifically, the present application uses a specific water-based acrylic emulsion and necessary additives to prepare a varnish, which is then mixed with a graphene slurry prepared from a specific graphene to obtain a graphene-modified water-based acrylate anti-corrosion coating.

[0005] In order to solve the above technical problems, this application provides the following technical solutions.

[0006] In a first aspect, the present application provides a graphene-modified water-based acrylic anticorrosive coating, which is made of graphene slurry and water-based acrylic varnish. The graphene slurry is made of water, graphene powder, a first dispersant and a first defoamer. The water-based acrylic varnish is made of water, water-based acrylic emulsion, a second dispersant, a filler, a second defoamer, a neutralizer, a film-forming aid, an anti-flash rust aid and a thickener. The mass percentage of the graphene in the total weight of the graphene-modified water-based acrylic anticorrosive coating is 1-5%.

[0007] In one embodiment of the first aspect, the aqueous acrylic emulsion is an aqueous acrylic emulsion with a brand name of XG-9018 produced by Hengshui Xinguang New Material Technology Co., Ltd.; and the graphene powder is a graphene powder with a brand name of HX-Gx produced by Qingdao Haoxin New Energy Technology Co., Ltd.

[0008] In one embodiment of the first aspect, the first dispersant and the second dispersant are each independently an aqueous dispersant BYK190 or BYK346; the first defoamer and the second defoamer are each independently Tego810.

[0009] In one embodiment of the first aspect, the filler includes at least one of barium sulfate, talc, zinc phosphate and titanium dioxide.

[0010] In one embodiment of the first aspect, the neutralizing agent is dimethylethanolamine. The film-forming aid is C-12 sold by Dow Chemical Company. The anti-flash rust aid is D1600 sold by Shanghai Tianyu Chemical Technology Co., Ltd. The thickener is RM-12W sold by Dow Chemical Company.

[0011] In one embodiment of the first aspect, based on the total weight of the aqueous acrylic varnish being 100 parts by weight, the aqueous acrylic varnish comprises the following components: 40-50 parts by weight of aqueous acrylic emulsion, 0.05-0.15 parts by weight of a second dispersant, 15-25 parts by weight of a filler, 0.05-0.15 parts by weight of a second defoamer, 0.05-0.15 parts by weight of a neutralizer, 1-3 parts by weight of a film-forming aid, 0.5-0.8 parts by weight of an anti-flash rust aid, and 0.3-0.5 parts by weight of a thickener. Based on weight, the graphene slurry comprises the following components: 1-5 parts by weight of a first dispersant, 0.05-0.15 parts by weight of a first defoamer, 1-5 parts by weight of graphene, and 90 parts by weight of water.

[0012] In one embodiment of the first aspect, based on 100 parts by weight of the total weight of the aqueous acrylic varnish, the aqueous acrylic varnish comprises the following components: 40-50 parts by weight of aqueous acrylic emulsion XG-9018, 0.05-0.15 parts by weight of a second dispersant BYK346, 15-25 parts by weight of a filler, 0.05-0.15 parts by weight of a second defoamer Tego 810, 0.05-0.15 parts by weight of a neutralizer dimethylethanolamine, 1-3 parts by weight of a film-forming aid C-12, 0.5-0.8 parts by weight of an anti-flash rust aid D1600, and 0.3-0.5 parts by weight of a thickener RM-12W.

[0013] In one embodiment of the first aspect, based on 100 parts by weight of the total weight of the aqueous acrylic varnish, the aqueous acrylic varnish comprises the following components: 40 parts by weight of aqueous acrylic emulsion XG-9018, 0.1 parts by weight of a second dispersant BYK346, 10 parts by weight of titanium dioxide R930, 6 parts by weight of talc, 6 parts by weight of zinc phosphate, 0.1 parts by weight of a second defoamer Tego810, 0.1 parts by weight of a neutralizer dimethylethanolamine, 2 parts by weight of a film-forming aid C-12, 0.6 parts by weight of an anti-flash rust aid D1600, and 0.3 parts by weight of a thickener RM-12W.

[0014] Based on weight, the graphene slurry comprises the following components: 5.0 parts by weight of a first dispersant BYK190, 0.1 parts by weight of a first defoamer Tego810, 1-5 parts by weight of graphene HX-Gx, and 90 parts by weight of water.

[0015] In a second aspect, the present application provides a method for preparing the graphene-modified water-based acrylate anti-corrosion coating as described in the first aspect, characterized in that the method comprises the following steps:

[0016] S1: Preparation of graphene slurry

[0017] Mixing water, a first dispersant and a second defoamer to obtain a first dispersion, then adding graphene powder to the first dispersion, and continuing to disperse until the fineness of the graphene slurry is less than 10 microns to obtain the graphene slurry;

[0018] S2: Preparation of waterborne acrylic varnish

[0019] Mixing water, a second dispersant and a second defoamer to obtain a second dispersion, then adding a filler to the second dispersion, and continuing to disperse until the slurry fineness is less than or equal to 30 microns to obtain a third dispersion, and then mixing the third dispersion with a neutralizer, a water-based acrylic emulsion, a film-forming aid, an anti-flash rust aid and a thickener to obtain the water-based acrylic varnish;

[0020] S3: Preparation of graphene-modified waterborne acrylate anticorrosive coating

[0021] The graphene slurry and the water-based acrylic varnish are mixed according to a predetermined ratio to obtain the graphene-modified water-based acrylic anti-corrosion coating.

[0022] In one embodiment of the second aspect, in step S2, the third dispersion is prepared by grinding; the water-based acrylic varnish is prepared by ball milling, and the rotation speed of the ball milling is 1000-1200 rpm.

[0023] Compared with the prior art, the positive effects of the present invention are: when the graphene content is 3%, the coating prepared has an impact resistance of 40cm, and there is no crack or peeling on the coating surface; the hardness of the coating first increases and then decreases with the increase of the graphene content, and the hardness reaches 5H when the graphene content is 3%, without scratches, paint peeling, or leakage from the substrate surface; the adhesion can reach the level 0 standard; the salt water resistance test meets the standard; the salt spray resistance reaches 1200h, which meets the national standard. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The following drawings describe in detail the exemplary embodiments disclosed in this application. The same reference numerals represent similar structures in several views of the drawings. Those skilled in the art will understand that these embodiments are non-limiting, exemplary embodiments, and the drawings are only used for the purpose of illustration and description, and are not intended to limit the scope of this application. Other embodiments may also accomplish the inventive intent in this application. It should be understood that the drawings are not drawn to scale. Among them:

[0025] Figure 1 Show the film-forming and curing mechanism of waterborne acrylic resin;

[0026] Figure 2 The results of coating impact resistance tests showing different contents of graphene-modified coatings;

[0027] Figure 3 Shows the coating adhesion test results of coatings modified with different contents of graphene;

[0028] Figure 4 The coating hardness test results showing different contents of graphene modified coatings;

[0029] Figure 5 Showing the salt water resistance test results of coatings with different contents of graphene modified coatings;

[0030] Figure 6 Showing the salt spray resistance test results of coatings modified with different contents of graphene. DETAILED DESCRIPTION

[0031] Unless otherwise indicated, implied from the context, or customary in the prior art, all parts and percentages in this application are based on weight, and the test and characterization methods used are all current as of the filing date of this application. Where applicable, the contents of any patent, patent application or publication referred to in this application are fully incorporated herein by reference, and their equivalent patent families are also incorporated by reference, especially the definitions of synthesis techniques, product and processing designs, polymers, comonomers, initiators or catalysts disclosed in these documents in the art. If the definition of a specific term disclosed in the prior art is inconsistent with any definition provided in this application, the definition of the term provided in this application shall prevail.

[0032] Numerical ranges in this application are approximate values, so unless otherwise specified, they may include numerical values ​​outside the range. Numerical ranges include all numerical values ​​from the lower limit to the upper limit increased by 1 unit, provided that there is an interval of at least 2 units between any lower value and any higher value. For example, if the recorded component, physical or other properties (such as molecular weight, melt index, etc.) are 100 to 1000, it means that all single values ​​are clearly listed, such as 100, 101, 102, etc., and all sub-ranges, such as 100 to 166, 155 to 170, 198 to 200, etc. For a range containing a numerical value less than 1 or containing a fraction greater than 1 (such as 1.1, 1.5, etc.), 1 unit is appropriately regarded as 0.0001, 0.001, 0.01 or 0.1. For a range containing a single digit less than 10 (such as 1 to 5), 1 unit is usually regarded as 0.1. These are only specific examples of what is intended to be expressed, and all possible combinations of values ​​between the lowest and highest values ​​listed are considered to be clearly recorded in this application. It should also be noted that the terms "first", "second", etc. in this article do not limit the order of precedence, but are only used to distinguish substances with different structures.

[0033] When used with respect to chemical compounds, unless expressly specified otherwise, the singular includes all isomeric forms and vice versa (e.g., "hexane" includes all isomers of hexane, individually or collectively). In addition, nouns using "a," "an," or "the" also include their plural forms unless expressly specified otherwise.

[0034] The terms "comprising", "including", "having" and their derivatives do not exclude the presence of any other components, steps or processes, and are irrelevant to whether these other components, steps or processes are disclosed in this application. To eliminate any doubt, unless explicitly stated, all compositions using the terms "comprising", "including", or "having" in this application may include any additional additives, adjuvants or compounds. On the contrary, except for those necessary for operating performance, the term "essentially consisting of..." excludes any other components, steps or processes from the scope of any description of the term below. The term "consisting of..." does not include any components, steps or processes that are not specifically described or listed. Unless explicitly stated, the term "or" refers to the listed individual members or any combination thereof.

[0035] Existing solvent-based coatings can cause serious environmental pollution problems, so more and more research has begun to focus on water-based coatings. However, existing water-based acrylic anti-corrosion coatings have poor mechanical properties, that is, poor impact resistance. To this end, the present application selects specific water-based acrylic emulsions and graphene to prepare anti-corrosion coatings, and obtains anti-corrosion coatings with beneficial comprehensive properties.

[0036] In one embodiment, the present application provides a graphene-modified water-based acrylate anticorrosive coating, which can be made of graphene slurry and water-based acrylate varnish. In a specific embodiment, the graphene slurry can be prepared by mixing water, a first dispersant, a first defoamer, and a specific graphene powder. In a specific embodiment, the water-based acrylate varnish can be prepared by mixing water, a water-based acrylic emulsion, a second dispersant, a filler, a second defoamer, a neutralizer, a film-forming aid, an anti-flash rust aid, and a thickener.

[0037] The inventor surprisingly found that when the water-based acrylic emulsion is a water-based acrylic emulsion with a brand name of XG-9018 produced by Hengshui Xinguang New Material Technology Co., Ltd., the graphene powder is a graphene powder with a brand name of HX-Gx produced by Qingdao Haoxin New Energy Technology Co., Ltd., and the weight percentage of graphene in the graphene-modified water-based acrylic anti-corrosion coating is controlled to be 1-5%, an anti-corrosion coating with good performance can be prepared. In particular, when the weight percentage of graphene is 3%, the impact strength of the anti-corrosion coating can reach 40cm, the pencil hardness can reach 5H, the adhesion can reach level 0, the salt water resistance test meets the standard, and the salt spray resistance test is 1200h, which meets the national standard.

[0038] Example

[0039] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solution of the present application. Unless otherwise specified, the reagents and raw materials used can be purchased through commercial channels. The experimental methods in the following examples that do not specify specific conditions are selected according to conventional methods and conditions, or according to the product specifications.

[0040] In the following examples, the equipment models used are as follows: QCJ-100 paint film impactor (Zhongstron (Tianjin) Measurement and Control Technology); disperser (Hangzhou Qiwei Instrument); XH2C002 electronic balance (Chengdu Besec Instrument); FQY-TESTER salt spray test chamber (Shanghai Tianchen Modern Environment); QHQ-A pencil hardness tester (Taizhou AiCe Instrument).

[0041] In the following examples, the brand information of the raw materials used is as follows: water-based acrylic emulsion XG-9018 (Hengshui Xinguang New Materials); graphene HX-Gx (Qingdao Haoxin New Energy Technology); neutralizer DMEA (Yangzi Petrochemical-BASF); film-forming agent C-12 (Dow Chemical); dispersant BYK346 (BYK Chemical); anti-flash rust agent D1600 (Shanghai Tianyu Chemical Technology Co., Ltd.); thickener RM-12W (Dow Chemical); titanium dioxide R930 (Ishihara, Japan); barium sulfate (Yichang Zhongtai New Materials); talc (Hangzhou Chongke New Materials); zinc phosphate (Tianjin Xinsheng Chemical); A200 gas silicon, water-based defoaming agent Tego810 (Evonik, Germany); dispersant BYK190 (BYK Chemical).

[0042] In the following examples and comparative examples, the performance parameters of the water-based acrylic emulsion XG-9018 are as follows: solid content of 47±1%, viscosity of 100-1000 mPa·s, glass transition temperature of 25°C, and minimum film-forming temperature of 23°C. The performance parameters of the water-based acrylic emulsion XG-9239 are as follows: solid content of 46±1%, viscosity of 100-1000 mPa·s, glass transition temperature of 40°C, and minimum film-forming temperature of 32°C.

[0043] In the following examples and comparative examples, the performance parameters of graphene HX-Gx are as follows: appearance is black powder, solid content is 5%, flake size (D50) is 8 microns, thickness is 10nm, and specific surface area is 50㎡ / g. The performance parameters of graphene JX-G01 are as follows: appearance is black-gray powder, solid content is 5%, flake size (D50) is 4 microns, and specific surface area is 30.2㎡ / g.

[0044] In the following examples, the coating performance test standards prepared in each example are as follows:

[0045] ① Impact resistance test standard: Test conducted according to the paint film impact resistance test method "GB / T1732-1993".

[0046] ② Adhesion test standard: graded according to the rating standards specified in GB / T9286-88.

[0047] ③ Pencil hardness test standard: According to the provisions of GB / T6739-86, the pencils used are graded from 6B to 6H, a total of 13 grades.

[0048] ④ Salt water resistance test standard: Determine the test results according to GB / T1766-2008.

[0049] ⑤Salt spray resistance test standard: Tested in accordance with GB / T1771-2007.

[0050] In the following examples, the general preparation process of the graphene-modified water-based acrylate anti-corrosion coating of each example is as follows:

[0051] ① Preparation of graphene slurry

[0052] Add water, dispersant BYK190 and defoamer Tego810 to the dispersion tank in sequence, mix and disperse for 5 minutes, then add 5% HX-Gx graphene powder. Disperse at high speed until the graphene slurry fineness is less than 10μm, then stop dispersing and store for later use.

[0053] ② Preparation process of graphene-modified water-based acrylic anti-corrosion coating

[0054] According to the formula, 500g of varnish and paint containing 5% graphene were prepared, and water, dispersant BYK190 and water-based defoamer were added to the dispersion tank respectively, and then fillers were added in turn, and high-speed dispersion was performed for 20 minutes until the slurry fineness was ≤30μm, and then grinding was stopped. Then, neutralizer, emulsion, film-forming agent, anti-flash rust agent and thickener were added in turn, and the varnish was prepared after dispersion at 1000r / min for 15 minutes.

[0055] The varnish and the paint containing 5% graphene were mixed according to a predetermined ratio to prepare water-based acrylic anti-corrosion coatings modified with graphene in different ratios.

[0056] Table 1 Raw materials and dosage of Examples 1-5 (parts by weight)

[0057]

[0058]

[0059] Examples 1-5

[0060] According to the formula shown in Table 1, water-based acrylic emulsion XG-9018 and graphene HX-Gx are used to prepare graphene-modified water-based acrylic anticorrosive coatings. The preparation process is as described above. The weight percentages of graphene in Examples 1-6 are different, namely 1%, 2%, 3%, 4%, and 5%.

[0061] Comparative Example 1

[0062] Comparative Example 1 is a water-based acrylic emulsion XG-9018 varnish, which does not contain graphene.

[0063] Results and Discussion

[0064] Selection of water-based acrylic emulsion

[0065] The water-based acrylic resin component has a relatively large influence on the film-forming property and cost of its water-based paint, so the selection of water-based acrylic resins needs to be considered in the formulation of water-based acrylic anti-corrosion coatings. In order to prepare a water-based acrylic resin topcoat with excellent performance for light and medium corrosion protection, this experiment mainly compares the solid content, viscosity, glass transition temperature and minimum film-forming temperature of two specifications of resin. The glass transition temperature and minimum film-forming temperature of the two specifications of acrylic resin are significantly different. The glass transition temperature is an important indicator for judging the paint film. The higher the Tg, the better the film-forming performance will be and the longer the surface drying time of the paint film will be.

[0066] This application uses two specifications of acrylic resin to prepare varnish according to the formula, and adds 5% graphene to the paint. The prepared paint is sprayed on cold-rolled steel plates and tinplate plates, and the coating film is tested for performance. Through performance test comparison, it can be seen that the paint prepared using the resin of XG-9018 specification has the best performance, so this experiment uses the resin of XG-9018 specification as the film-forming material. The basic formula and test data are shown in Table 2.

[0067] Table 2 Different acrylic base formulas and their coating properties

[0068]

[0069] The choice of graphene

[0070] The large specific surface area of ​​graphene allows it to form a uniform coverage in the coating, thereby protecting the substrate; at the same time, the two-dimensional sheet structure of graphene can produce a "maze effect" in the coating, slowing down the penetration of water, ions, and oxygen, delaying the corrosion process, and achieving the purpose of corrosion prevention. This experiment mainly screened graphene slurry and graphene powder based on the characteristics of sheet size, thickness, and specific surface area.

[0071] In order to screen out suitable graphene, this application uses HX-9018 water-based acrylic emulsion and two scales of graphene to make paint spray panels. From the data in Table 3, it can be seen that the varnish prepared by the acrylic emulsion of HX-9018 specification and the coating prepared by the graphene of HX-Gx specification have better adhesion, salt water resistance and surface drying time than the performance of the graphene prepared by JX-G01 specification. Therefore, based on comprehensive performance testing and cost considerations, the graphene of HX-Gx specification was finally selected.

[0072] Table 3.4 Performance test table of 750 varnish and HX-9018 and JX-G01 samples

[0073]

[0074]

[0075] Film-forming and curing mechanism of waterborne acrylic anticorrosive coatings

[0076] like Figure 1 As shown, water-based acrylic resin is basically prepared by emulsion polymerization. Its film-forming and curing mechanism is solvent volatilization and curing. No chemical reaction occurs during the process. The process mainly includes the following four stages. The first stage is the emulsion concentration stage. After the coating covers the surface of the substrate, the water in the coating gradually evaporates, making the emulsion slowly become viscous; the second stage is the contact stage between particles. With the continuous evaporation of water in the emulsion, the latex particles slowly gather together, from disorder to order, until reaching a dense state; the third stage is the particle deformation stage. Due to the gradual evaporation of water, when the water evaporates to a certain extent, the gap between the latex particles becomes small enough until they are squeezed together to cause particle deformation; the fourth stage is the particle agglomeration stage. Due to the extrusion of particles, deformation occurs. Under the action of pressure, the particles begin to slowly fuse together until the interface between the particles disappears, forming a high-density coating on the surface of the substrate.

[0077] Test results of coating performance of Examples 1-5

[0078] Figure 2 Showing the impact resistance test results of coatings modified with different contents of graphene. Figure 3 Showing the coating adhesion test results of graphene-modified coatings with different contents. Figure 4 The coating hardness test results of different graphene content modified coatings are shown. Figure 4 In the figure, sample number 1 corresponds to the anti-corrosion coating of Example 1, and sample numbers 2-6 correspond to the anti-corrosion coatings of Examples 1 to 5, respectively. Figure 5 Showing the salt water resistance test results of coatings modified with different contents of graphene. Figure 6 Showing the salt spray resistance test results of coatings modified with different contents of graphene.

[0079] The coating impact resistance test is a method to test the impact resistance of the coating. The coating is tested according to the requirements of GB / T1732-2020. Figure 2 It can be seen that all the prepared coatings containing different proportions of graphene passed the impact resistance test without any cracks or peeling.

[0080] This application uses the cross-cut test method to test the coating adhesion according to GB / T9286-1998. Figure 3 It can be seen that the coatings of samples b, c and d reach the level 1 standard, among which the best is sample d, that is, the coating with a graphene content of 3%, and its adhesion can reach the level 0 standard, which meets the national requirements.

[0081] The pencil hardness test of this application is tested according to GB / T6739-2006. Figure 4 It can be seen that all the prepared coatings meet the national standards, among which the coating with a graphene content of 3% has the best effect, and the pencil hardness can reach 5H.

[0082] The salt water resistance test in this experiment is carried out according to GB / T9274-1988, and the substrate used in the salt water resistance test is tinplate. Figure 5 From the test results, it can be seen that the coating with a graphene content of 3% meets the standard and its salt spray resistance reaches 1200h, while coatings with other graphene contents do not meet the national standard requirements.

[0083] The salt spray resistance test is used to evaluate the salt spray corrosion resistance of the coating. The paint film is observed every 24 hours to see if there are any bubbling, rusting, cracking, peeling, etc. The test is carried out in accordance with GB / T1771-2007. Figure 6 It can be seen that the salt spray resistance time of the coating can reach 1200h before rust spots appear, which meets the national standards.

[0084] The above description of the embodiments is to facilitate those of ordinary skill in the art to understand and apply the present application. It is obvious that those familiar with the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without having to pay creative labor. Therefore, the present application is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the contents disclosed in the present application without departing from the scope and spirit of the present application are within the scope of the present application.

Claims

1. A graphene-modified water-based acrylate anti-corrosion coating, characterized in that: The graphene-modified water-based acrylic anti-corrosion coating is made of graphene slurry and water-based acrylic varnish; Wherein, the graphene slurry is made of water, graphene powder, a first dispersant and a first defoaming agent; The water-based acrylic varnish is made of water, water-based acrylic emulsion, a second dispersant, a filler, a second defoamer, a neutralizer, a film-forming aid, an anti-flash rust aid and a thickener; Wherein, the mass percentage of the graphene in the total weight of the graphene-modified water-based acrylate anti-corrosion coating is 1-5%.

2. The graphene-modified water-based acrylate anticorrosive coating according to claim 1, characterized in that: The water-based acrylic emulsion is a water-based acrylic emulsion with a brand name of XG-9018 produced by Hengshui Xinguang New Material Technology Co., Ltd.; and the graphene powder is a graphene powder with a brand name of HX-Gx produced by Qingdao Haoxin New Energy Technology Co., Ltd.

3. The graphene-modified water-based acrylate anticorrosive coating according to claim 1, characterized in that: The first dispersant and the second dispersant are each independently an aqueous dispersant BYK190 or BYK346; the first defoamer and the second defoamer are each independently Tego810.

4. The graphene-modified water-based acrylate anticorrosive coating according to claim 1, characterized in that: The filler includes at least one of barium sulfate, talcum powder, zinc phosphate and titanium dioxide.

5. The graphene-modified water-based acrylate anticorrosive coating according to claim 1, characterized in that: The neutralizing agent is dimethylethanolamine; The film-forming aid is C-12 sold by Dow Chemical Company; The anti-flash rust additive is D1600 sold by Shanghai Tianyu Chemical Technology Co., Ltd. The thickener is RM-12W sold by The Dow Chemical Company.

6. The graphene-modified water-based acrylate anticorrosive coating according to any one of claims 1 to 5, characterized in that: Based on 100 parts by weight of the total weight of the water-based acrylic varnish, the water-based acrylic varnish comprises the following components: 40-50 parts by weight of water-based acrylic emulsion, 0.05-0.15 parts by weight of a second dispersant, 15-25 parts by weight of a filler, 0.05-0.15 parts by weight of a second defoamer, 0.05-0.15 parts by weight of a neutralizer, 1-3 parts by weight of a film-forming aid, 0.5-0.8 parts by weight of an anti-flash rust aid, and 0.3-0.5 parts by weight of a thickener; Based on weight, the graphene slurry comprises the following components: 1-5 parts by weight of a first dispersant, 0.05-0.15 parts by weight of a first defoamer, 1-5 parts by weight of graphene, and 90 parts by weight of water.

7. The graphene-modified water-based acrylate anticorrosive coating according to claim 6, characterized in that: Based on 100 parts by weight of the total weight of the aqueous acrylic varnish, the aqueous acrylic varnish comprises the following components: 40-50 parts by weight of aqueous acrylic emulsion XG-9018, 0.05-0.15 parts by weight of a second dispersant BYK346, 15-25 parts by weight of a filler, 0.05-0.15 parts by weight of a second defoamer Tego 810, 0.05-0.15 parts by weight of a neutralizer dimethylethanolamine, 1-3 parts by weight of a film-forming aid C-12, 0.5-0.8 parts by weight of an anti-flash rust aid D1600, and 0.3-0.5 parts by weight of a thickener RM-12W.

8. The graphene-modified water-based acrylate anticorrosive coating according to claim 1, characterized in that: Based on the total weight of the water-based acrylic varnish being 100 parts by weight, the water-based acrylic varnish comprises the following components: 40 parts by weight of water-based acrylic emulsion XG-9018, 0.1 parts by weight of a second dispersant BYK346, 10 parts by weight of titanium dioxide R930, 6 parts by weight of talc, 6 parts by weight of zinc phosphate, 0.1 parts by weight of a second defoamer Tego810, 0.1 parts by weight of a neutralizer dimethylethanolamine, 2 parts by weight of a film-forming aid C-12, 0.6 parts by weight of an anti-flash rust aid D1600, and 0.3 parts by weight of a thickener RM-12W; Based on weight, the graphene slurry comprises the following components: 5.0 parts by weight of a first dispersant BYK190, 0.1 parts by weight of a first defoamer Tego810, 1-5 parts by weight of graphene HX-Gx, and 90 parts by weight of water.

9. The method for preparing the graphene-modified water-based acrylate anticorrosive coating according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: S1: Preparation of graphene slurry Mixing water, a first dispersant and a second defoamer to obtain a first dispersion, then adding graphene powder to the first dispersion, and continuing to disperse until the fineness of the graphene slurry is less than 10 microns to obtain the graphene slurry; S2: Preparation of waterborne acrylate varnish Mixing water, a second dispersant and a second defoamer to obtain a second dispersion, then adding a filler to the second dispersion, and continuing to disperse until the slurry fineness is less than or equal to 30 microns to obtain a third dispersion, and then mixing the third dispersion with a neutralizer, a water-based acrylic emulsion, a film-forming aid, an anti-flash rust aid and a thickener to obtain the water-based acrylic varnish; S3: Preparation of graphene-modified waterborne acrylate anticorrosive coating The graphene slurry and the water-based acrylic varnish are mixed according to a predetermined ratio to obtain the graphene-modified water-based acrylic anti-corrosion coating.

10. The preparation method according to claim 9, characterized in that: In step S2, the third dispersion is prepared by grinding; the water-based acrylic varnish is prepared by ball milling, and the rotation speed of the ball milling is 1000-1200 rpm.

Citation Information

Patent Citations

  • Graphene waterborne industrial coating and preparation method thereof

    CN105670474A

  • Preparation and application of waterborne graphene heavy anti-corrosion paint

    CN106189713A

  • Graphene modified steel structure water-based anti-corrosive paint and preparation method thereof

    CN107793865A

  • Water-based acrylic anti-corrosion coating and preparing method thereof

    CN109627880A

  • Environment-friendly high-hardness water-based graphene dipping paint and preparation method thereof

    CN116200081A