Method for preparing DNA three-dimensional nanomaterial and DNA three-dimensional nanomaterial

By synthesizing long single strands of DNA under specific conditions under the action of DNA polymerase and topoisomerase, a stable DNA three-dimensional nanomaterial is solved, and the problems of complex preparation and poor stability of existing DNA three-dimensional materials are achieved, and high biocompatibility is achieved and long-term storage effects.

CN118895342APending Publication Date: 2024-11-05THE FIRST MEDICAL CENT CHINESE PLA GENERAL HOSPITAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310485811.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The preparation process of existing DNA three-dimensional nanomaterials is complex, has poor stability, insufficient biocompatibility, and cannot be stored for a long time, so it cannot adapt to the needs of complex microenvironments in the body.

Method used

By providing a DNA circular template, DNA polymerase and topoisomerase are used to synthesize long single strands of DNA under specific conditions to form stable DNA three-dimensional nanomaterials, avoiding reliance on heavy metal ions, and improving the biocompatibility and stability of the material.

Benefits of technology

It realizes the simple and efficient preparation of DNA three-dimensional nanomaterials with high biocompatibility and stability, which can be stored for a long time, avoids structural instability and cytotoxicity problems, and adapts to the complex microenvironment in the body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895342A_ABST
    Figure CN118895342A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a DNA three-dimensional nano material and the DNA three-dimensional nano material, and the method comprises the following steps: cooling a mixture containing a first DNA single strand, a second DNA single strand and a third DNA single strand from 90-97 DEG C to 25-37 DEG C at a speed of 2-4 DEG C / min, and reacting, enabling at least part of the first binding sites and at least part of the second binding sites to be combined with binding sites in the corresponding DNA single strand, the second DNA single strand and the third DNA single strand, and preparing the DNA three-dimensional nano material under the action of DNA topoisomerase. According to the method disclosed by the invention, by selecting a plurality of first base sequence segments distributed at intervals and a plurality of second base sequence segments distributed at intervals in a DNA long single strand and controlling synthesis conditions, sites capable of being mutually combined in the DNA long single strand are combined, and the DNA three-dimensional nano material with a stable structure is prepared by a three-step method; particularly, under the action of DNA topoisomerase, the stability of the material is improved. In addition, the three-dimensional DNA nano material can be rapidly compounded with different small molecules.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of DNA material preparation, and specifically relates to a method for preparing a DNA three-dimensional nanomaterial and a DNA three-dimensional nanomaterial. Background Art

[0002] Deoxyribonucleic acid (DNA) carries the genetic information necessary for the synthesis of RNA and proteins and is an essential biomacromolecule for the development and normal functioning of organisms. DNA nanomaterials are prepared based on the principle of base pairing and have high biocompatibility and programmability.

[0003] DNA nanomaterials have been widely used in biological and medical fields, such as cell recruitment, organoid construction, protein capture and signal detection. DNA materials can be divided into two-dimensional DNA materials and three-dimensional DNA materials. Two-dimensional DNA materials include DNA aptamers and DNA nanonets. However, the functions of two-dimensional DNA materials are single and cannot adapt to the complex microenvironment in the body. Three-dimensional DNA materials include DNA tetrahedrons, DNA supramolecular hydrogels, etc. The construction of three-dimensional DNA materials depends on heavy metal ions and has poor biocompatibility. Moreover, the preparation process of three-dimensional DNA materials is complicated, the stability is poor, and they cannot be stored for a long time. Summary of the invention

[0004] In view of this, the present application provides a method for preparing a DNA three-dimensional nanomaterial and a DNA three-dimensional nanomaterial, aiming to provide a method for continuously and stably preparing a DNA three-dimensional nanomaterial with a stable structure.

[0005] In a first aspect, the present invention provides a method for preparing a three-dimensional DNA nanomaterial, comprising:

[0006] A DNA circular template is provided, comprising: a first circular DNA template, a second circular DNA template and a third circular DNA template, wherein the first circular DNA template, the second circular DNA template and the third circular DNA template respectively comprise: a plurality of first base sequence segments distributed at intervals and a plurality of second base sequence segments distributed at intervals, and the first base sequence segment and / or the second base sequence segment in the first circular DNA template can match at least part of the base sequence segments in the second circular DNA template and the third circular DNA template respectively;

[0007] According to the DNA circular template, a reaction is carried out under the action of a DNA polymerase to obtain a long single-stranded DNA whose bases are at least partially complementary to the DNA circular template, wherein the long single-stranded DNA includes a first single-stranded DNA, a second single-stranded DNA, and a third single-stranded DNA; the first single-stranded DNA, the second single-stranded DNA, and the third single-stranded DNA respectively contain: a plurality of first binding sites distributed at intervals and a plurality of second binding sites distributed at intervals; the first binding site and / or the second binding site in the first single-stranded DNA can respectively complementarily bind to at least a portion of the bases of the second single-stranded DNA and the third single-stranded DNA;

[0008] A mixture containing a first DNA single strand, a second DNA single strand and a third DNA single strand is cooled from 90-97°C to 25-37°C at a rate of 2-4°C / min and reacted so that at least a portion of the first binding site and at least a portion of the second binding site bind to the binding sites in the corresponding DNA single strand, the second DNA single strand and the third DNA single strand, and under the action of DNA topoisomerase, a DNA three-dimensional nanomaterial is prepared.

[0009] According to an embodiment of one aspect of the present application, a method for preparing a DNA circular template comprises:

[0010] Providing a first single-stranded DNA raw material and a second single-stranded DNA raw material respectively, wherein the first single-stranded DNA raw material and the second single-stranded DNA raw material respectively include at least one first base sequence segment and at least one second base sequence segment distributed at intervals;

[0011] The first DNA raw material single strand, the second DNA raw material single strand and the base sequence connecting segment are mixed, and a DNA circular template is prepared under the action of DNA ligase.

[0012] According to an embodiment of one aspect of the present application, based on the DNA circular template, preparing a long single-stranded DNA having at least some bases complementary to the DNA circular template with the participation of a primer comprises:

[0013] The DNA circular template is amplified and reacted under the action of BST DNA polymerase to achieve rolling circle replication. The reaction temperature is 52-62° C. and the reaction time is 24-48 hours to obtain a long single-stranded DNA with at least some bases complementary to the DNA circular template.

[0014] According to an embodiment of one aspect of the present application, the molar ratio of the first DNA single strand, the second DNA single strand and the third DNA single strand is 1:(0.1-50):(0.1-50).

[0015] According to an embodiment of one aspect of the present application, the DNA three-dimensional nanomaterial includes one or more of a DNA nanoflower-shaped composite structure or a DNA nanogrid composite structure.

[0016] According to an embodiment of one aspect of the present application, a mixture comprising a first DNA single strand, a second DNA single strand and a third DNA single strand is cooled from 90-97°C to 25-37°C at a rate of 2-4°C / min and reacted under the action of metal ions, so that at least part of the first binding site and at least part of the second binding site are combined with the binding sites in the corresponding DNA single strand, the second DNA single strand and the third DNA single strand, and under the action of DNA topoisomerase, a DNA nanoflower-shaped composite structure is obtained, wherein the metal ions include one or more of magnesium ions, calcium ions, potassium ions and sodium ions.

[0017] According to an embodiment of one aspect of the present application, the volume of the DNA nanoflower-shaped composite structure is 0.0001-100 cubic microns; optionally ≥20 cubic microns; optionally, the DNA nanoflower-shaped composite structure has a spherical particle appearance and has stacked petal-shaped layers inside.

[0018] According to an embodiment of one aspect of the present application, the diameter of the DNA nanoflower-shaped composite structure is 200-5000 nm.

[0019] According to an embodiment of one aspect of the present application, the area of ​​the DNA nanomesh composite structure on the projection surface is 100 μm 2 -1mm 2 ; Optionally, the DNA nanomesh composite structure has a grid layered appearance.

[0020] In a second aspect, an embodiment of the present application provides a DNA three-dimensional nanomaterial prepared by the method of the first aspect.

[0021] Compared with the prior art, this application has at least the following beneficial effects:

[0022] The method provided by the present application can prepare a structurally stable three-dimensional DNA nanomaterial by selecting multiple first base sequence segments and multiple second base sequence segments distributed at intervals in a long single-stranded DNA, and then controlling the synthesis conditions, so that the sites that can bind to each other in the long single-stranded DNA can bind, especially under the action of DNA topoisomerase, so that it is supercoiled, thereby improving the stability of the material and avoiding the drawback that the structural stability of nanomaterials in related technologies completely depends on non-covalent bonds. Active sites for nucleic acid molecule binding are reserved on the three-dimensional DNA nanomaterial, which can quickly compound different small molecules to achieve functionalization.

[0023] The design and synthesis method of the DNA three-dimensional nanomaterial of the present application is simple, which greatly saves the production cost. And the synthesized DNA three-dimensional nanomaterial has the advantages of high biocompatibility and low cytotoxicity. The DNA nanomaterial designed in the present application has high stability and easy storage, and can be stored for more than 6 months, avoiding the characteristics of high disorder and short shelf life of DNA nanomaterials in related technologies. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.

[0025] Figure 1 A schematic diagram showing a process of preparing a DNA nanomesh composite structure according to an embodiment of the present application is shown;

[0026] Figure 2 A microscopic image of a DNA nanomesh composite structure according to an embodiment of the present application is shown;

[0027] Figure 3 A schematic diagram showing a process for preparing a DNA nanoflower-shaped composite structure according to an embodiment of the present application is shown;

[0028] Figure 4 A microscopic image of a DNA nanoflower-shaped composite structure according to an embodiment of the present application is shown;

[0029] Figure 5 A schematic diagram showing a process of preparing a dual-modality three-dimensional DNA nanomaterial according to an embodiment of the present application;

[0030] Figure 6 A microscopic image of the dual-mode DNA three-dimensional nanomaterial of an embodiment of the present application is shown;

[0031] Figure 7 The microscopic images of the DNA nanomesh composite structure before and after storage of Example 2 of the present application are shown;

[0032] Figure 8 The microscopic images of the DNA nanoflower-shaped composite structure before and after storage of Example 3 of the present application are shown;

[0033] Fig. 9 The microscopic images of the DNA nanomesh composite structure before and after storage of Comparative Example 1 of the present application are shown;

[0034] Fig.10 The microscopic images of the DNA nanoflower-shaped composite structure before and after storage of Comparative Example 2 of the present application are shown;

[0035] Fig.11 A schematic diagram of the first DNA circular template in Example 1 of the present application is shown;

[0036] Fig.12 A schematic diagram of a second DNA circular template in Example 1 of the present application is shown;

[0037] Fig.13 A schematic diagram of the third DNA circular template of Example 1 of the present application is shown. DETAILED DESCRIPTION

[0038] In order to make the application purpose, technical solution and beneficial technical effect of the present application clearer, the present application is further described in detail in conjunction with the embodiments below. It should be understood that the embodiments described in this specification are only for explaining the present application, not for limiting the present application.

[0039] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0040] In the description of the present application, it should be noted that, unless otherwise specified, “above” and “below” are inclusive of the number, and the “multiple” in “one or more” means two or more than two.

[0041] The above application content of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0042] Biomedical tissue engineering has brought new treatment strategies for many diseases, among which designing materials with biological functions and excellent performance is an important task of tissue engineering. In the past few decades, DNA nanomaterials have become one of the most widely used molecular building blocks in engineered self-assembly materials and are widely used in biological and medical fields, such as cell recruitment, organoid construction, protein capture and signal detection.

[0043] DNA nanomaterials can fold hundreds of short DNA oligonucleotides and long single-stranded DNA into various nanoscale two-dimensional or three-dimensional structures by adjusting DNA molecules to achieve different functions. DNA nanomaterials are prepared based on the principle of base pairing and have high biocompatibility and programmability. DNA nanomaterials have been widely used in biological and medical fields, such as cell recruitment, organoid construction, protein capture and signal detection.

[0044] Materials used in biomedical tissue engineering need to take into account both biocompatibility and functionality. Compared with other materials, nucleic acids have higher biocompatibility and programmability, but it is difficult to construct DNA nanomaterials with specific nanostructures that meet the requirements. The synthesis of DNA materials with two-dimensional structures is relatively simple, but it is not enough to meet the requirements for material performance. DNA materials can be divided into two-dimensional DNA materials and three-dimensional DNA materials. Two-dimensional materials include DNA aptamers and DNA nanonets. Three-dimensional DNA materials include DNA tetrahedrons and DNA supramolecular hydrogels. However, the functions of two-dimensional DNA materials are single and cannot adapt to the complex microenvironment in the body. The construction of three-dimensional materials relies on heavy metal ions and has poor biocompatibility. Moreover, the preparation process of three-dimensional DNA materials is complicated, the stability is poor, and they cannot be stored for a long time.

[0045] Currently, DNA origami and DNA cross-linked networks are important methods for constructing DNA materials. DNA origami is a technology that can fold long DNA chains into 3D nanomaterials of various shapes, such as DNA nanoflowers. DNA nanoflowers have been used for cell imaging and targeted drug delivery. DNA cross-linked networks can be used to create gel-like materials for biomedical applications. The materials prepared by this method can be used to capture bone marrow mesenchymal stem cells (BMSCs) and specific T cells. However, the preparation of DNA nanoflowers usually relies on heavy metal ions, such as Co and Mn ions, to form DNA-inorganic hybrid superstructures. This method is complex, unstable and difficult to control. In addition, heavy metal ions may cause cytotoxicity due to their participation and residues, thus limiting the medical application of nanoflowers. DNA cross-linked networks are highly disordered and have a short shelf life because their structure relies entirely on non-covalent bonds. Therefore, a method that can overcome these shortcomings is needed to achieve the preparation of DNA three-dimensional materials.

[0046] Method for preparing DNA three-dimensional nanomaterials

[0047] In a first aspect, the present invention provides a method for preparing a three-dimensional DNA nanomaterial, comprising:

[0048] S100. Providing a DNA circular template, including: a first circular DNA template, a second circular DNA template, and a third circular DNA template, wherein the first circular DNA template, the second circular DNA template, and the third circular DNA template respectively include: a plurality of first base sequence segments distributed at intervals and a plurality of second base sequence segments distributed at intervals, and the first base sequence segment and / or the second base sequence segment in the first circular DNA template can match at least part of the base sequence segments in the second circular DNA template and the third circular DNA template respectively;

[0049] S200. According to the DNA circular template, react under the action of DNA polymerase to obtain a long single-stranded DNA whose bases are at least partially complementary to the DNA circular template, wherein the long single-stranded DNA includes a first single-stranded DNA, a second single-stranded DNA, and a third single-stranded DNA; the first single-stranded DNA, the second single-stranded DNA, and the third single-stranded DNA respectively contain: a plurality of first binding sites distributed at intervals and a plurality of second binding sites distributed at intervals; the first binding site and / or the second binding site in the first single-stranded DNA can respectively bind to at least a portion of the bases of the second single-stranded DNA and the third single-stranded DNA in a complementary manner;

[0050] S300. Cool a mixture comprising a first DNA single strand, a second DNA single strand and a third DNA single strand from 90-97°C to 25-37°C at a rate of 2-4°C / min and react, so that at least a portion of the first binding site and at least a portion of the second binding site bind to the binding sites in the corresponding DNA single strand, the second DNA single strand and the third DNA single strand, and under the action of DNA topoisomerase, obtain a DNA three-dimensional nanomaterial.

[0051] According to the embodiment of the present application, the first DNA single strand, the second DNA single strand and the third DNA single strand are synthesized by a DNA circular template, and the above DNA single strands are interspersed with binding sites, which can be combined with other DNAs to synthesize a DNA three-dimensional nanomaterial with certain cross-linking nodes. Under the action of DNA topoisomerase, with the corresponding reaction conditions, the DNA three-dimensional nanomaterial with certain cross-linking nodes undergoes further conformational changes or supercoils, making the structure of the DNA three-dimensional nanomaterial more stable, convenient for later purification, storage and use, avoiding the instability of the structure of the DNA three-dimensional nanomaterial in the related art, which can only be used and prepared.

[0052] According to an embodiment of the present application, at least part of the bases in the first DNA single strand are complementary to the bases of the first circular DNA template, at least part of the bases in the second DNA single strand are complementary to the bases of the second circular DNA template, and at least part of the bases in the third DNA single strand are complementary to the bases of the third circular DNA template.

[0053] The method of the present application utilizes the spontaneous polymerization and divergence properties of long single-stranded DNA in solution, and achieves stable preparation of different nano-conformations by precisely controlling the action of DNA topoisomerase under reaction conditions.

[0054] According to an embodiment of the present application, the DNA polymerase may include BST DNA polymerase and Phi29 DNA polymerase. BST DNA polymerase, a part of Bacillus stearothermophilus DNA polymerase, is derived from E. coli strain. It is obtained by multiple purification and separation after expression in Escherichia coli using genetic recombination technology. The enzyme has 5′→3′ DNA polymerase activity, but does not have 5′→3′ exonuclease activity. Phi29 DNA polymerase is derived from Bacillus subtilis bacteriophage Phi29. The enzyme has excellent chain displacement and continuous synthesis properties, can continuously synthesize DNA fragments of up to 70,000 bases, and has 3'→5' exonuclease proofreading activity.

[0055] In some embodiments, in S100, in the first circular DNA template, the second circular DNA template, and the third circular DNA template, the base spacing between the first base sequence segment and the second base sequence segment is 10bp, which can be 5-20bp. In some embodiments, in S100, in the first circular DNA template, the second circular DNA template, and the third circular DNA template, the base spacing between the first base sequence segments is 50bp, which can be 20-100bp. In some embodiments, in S100, in the first circular DNA template, the second circular DNA template, and the third circular DNA template, the base spacing between the second base sequence segments is 100bp, which can be 100-500bp.

[0056] According to the embodiments of the present application, by controlling the base distance between the first base sequence segment and the second base sequence segment, the distance between the first binding site and the second binding site between the subsequent long DNA single strands can be regulated, which helps to make the DNA three-dimensional nanomaterial bind within a specific distance, which is beneficial to improving the stability of the DNA three-dimensional nanomaterial.

[0057] In some embodiments, in S200, the first binding site and the second binding site respectively include a base sequence. In any one of the first DNA single strand, the second DNA single strand and the third DNA single strand, the distance between the first binding site and the second binding site is 10bp, which can be optionally 5-20bp. In any one of the first DNA single strand, the second DNA single strand and the third DNA single strand, the distance between the first binding sites is 500bp, which can be optionally 20-100bp. In some embodiments, the spacing between the first binding site and the second binding site is 100bp, which can be optionally 100-500bp.

[0058] According to an embodiment of the present application, controlling the distance between the first binding site and the second binding site within the above range or controlling the distance between the first binding sites or controlling the base sequence length of the first binding site and the second binding site within the above range helps to make the DNA three-dimensional nanomaterial have stable connection gaps or stable connection sites, which helps to improve the stability of the DNA three-dimensional nanomaterial.

[0059] In some optional embodiments, in S100, the method for preparing a DNA circular template includes:

[0060] Providing a first single-stranded DNA raw material and a second single-stranded DNA raw material respectively, wherein the first single-stranded DNA raw material and the second single-stranded DNA raw material respectively include at least one first base sequence segment and at least one second base sequence segment distributed at intervals;

[0061] The first DNA raw material single strand, the second DNA raw material single strand and the base sequence connecting segment are mixed, and a DNA circular template is prepared under the action of T4 2DNA ligase.

[0062] In some embodiments, in S100, the first DNA single-stranded raw material and the second DNA single-stranded raw material can be short DNA chains. The base length range of the first DNA single-stranded raw material and the second DNA single-stranded raw material (Loop portion) can be 20-200bp. The first DNA single-stranded raw material and the second DNA single-stranded raw material can be obtained through Shanghai Sangon Company. The length range of the base of the base sequence connecting segment (linker portion) can be 10-100bp. A DNA circular template of a predetermined length can be synthesized. The use of the above raw materials to obtain a DNA circular template is conducive to obtaining a designed long single-stranded DNA and reducing the cost of obtaining a long single-stranded DNA.

[0063] In some optional embodiments, in S200, preparing a long single-stranded DNA having at least a portion of bases complementary to the DNA circular template with the help of a primer according to the DNA circular template comprises:

[0064] The DNA circular template is amplified and reacted under the action of BST DNA polymerase to achieve rolling circle replication. The reaction temperature is 52-62° C. and the reaction time is 24-48 hours to obtain a long single-stranded DNA with at least some bases complementary to the DNA circular template.

[0065] According to the embodiments of the present application, the long single-stranded DNA prepared by the above method has binding sites, which helps to improve the stability of the DNA three-dimensional nanomaterial.

[0066] In some embodiments, in S200, in any one of the first DNA strand, the second DNA strand, and the third DNA strand, the first binding site and the second binding site are different. Between the first circular DNA template, the second circular DNA template, and the third circular DNA template, the spacing between the first binding site and the second binding site may be the same.

[0067] In some embodiments, in S300, the three long chains of DNA are cooled from 90-97°C to 25-37°C at a rate of 2-4°C / min and reacted. The optional cooling rate can be 2°C / min, 3°C / min and 4°C / min. The target stability of cooling can be any value or a range of its composition among 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, and finally the morphology is stabilized with DNA topoisomerase. Under the above reaction conditions, the sites in the first DNA single strand, the second DNA single strand and the third DNA single strand can be more effectively combined, and the combined DNA material can be supercoiled, thereby improving the stability of the DNA three-dimensional nanomaterial.

[0068] In some embodiments, in S300, the ratio of the total mass of the first DNA single strand, the second DNA single strand, and the third DNA single strand to the mass of the DNA topoisomerase is 1:(1-10). The molar ratio of the above substances within the above range is conducive to achieving supercoiling of DNA three-dimensional nanomaterials and improving their stability.

[0069] In some optional embodiments, in S300, the first DNA single strand, the second DNA single strand and the third DNA single strand that form the DNA nanomesh composite structure are relatively long and have more binding sites (including the first binding site and the second binding site). The binding sites are rigid and have more binding sites. The long DNA single strands are rigid and not prone to curling, so it is easy to generate a DNA nanomesh composite structure. The binding of the binding sites and the cooperation of DNA topoisomerase improve the stability of the structure, making it easier to maintain and preserve.

[0070] In some optional embodiments, in S300, the first DNA single strand, the second DNA single strand and the third DNA single strand of the structurally stable DNA nanoflower-shaped composite structure are shorter in length, have fewer binding sites (including the first binding site and the second binding site), the binding sites are rigid, and the long DNA single strands are prone to curling, thereby easily generating a DNA nanoflower-shaped composite structure. Moreover, under the binding of the binding sites and the coordinated action of DNA topoisomerase, the stability of the structure is improved, making it easier to maintain and preserve.

[0071] In some optional embodiments, in S300, the molar ratio of the first DNA single strand, the second DNA single strand and the third DNA single strand is 1:(0.1-50):(0.1-50). It can be optionally 1:1:1. Controlling the molar ratio of the first DNA single strand, the second DNA single strand and the third DNA single strand within the above range is conducive to preparing a DNA three-dimensional nanomaterial with a higher ratio while saving raw materials.

[0072] In some optional embodiments, in S300, the DNA three-dimensional nanomaterial includes one or more of a DNA nanoflower-shaped composite structure or a DNA nanogrid composite structure.

[0073] In some optional embodiments, in S300, a mixture comprising a first DNA single strand, a second DNA single strand and a third DNA single strand is cooled and reacted from 90-97°C to 25-37°C at a rate of 2-4°C / min under the action of DNA topoisomerase and metal ions, so that at least part of the first binding site and at least part of the second binding site are combined with the binding sites in the corresponding DNA single strand, the second DNA single strand and the third DNA single strand to obtain a DNA nanoflower-shaped composite structure, wherein the metal ions include one or more of magnesium ions, calcium ions, potassium ions and sodium ions.

[0074] According to an embodiment of the present application, the mixture of the above raw materials is cooled from 90-97°C to 25-37°C at a rate of 2-4°C / min and reacted under the action of DNA topoisomerase and metal ions, so that the first DNA single strand, the second DNA single strand and the third DNA single strand can achieve site binding and spontaneous conformational change, thereby making the DNA nanoflower-shaped composite structure have a stable structure.

[0075] In some embodiments, in S300, a mixture comprising a first DNA single strand, a second DNA single strand and a third DNA single strand is cooled from 90-97°C to 25-37°C at a rate of 2-4°C / min under the action of DNA topoisomerase and reacted so that at least part of the first binding site and at least part of the second binding site are combined with the binding sites in the corresponding DNA single strand, the second DNA single strand and the third DNA single strand to obtain a DNA nanogrid composite structure. According to an embodiment of the present application, during the preparation process, the polymerization of the first DNA single strand, the second DNA single strand and the third DNA single strand itself is less dependent on the bonding effect of metal ions, and metal ions may not be used, so that the prepared nanomaterial has simple preparation and high storage stability.

[0076] In some embodiments, in S300, a mixture comprising a first DNA strand, a second DNA strand, and a third DNA strand is cooled from 90-97°C to 25-37°C at a rate of 2-4°C / min and reacted so that at least part of the first binding site and at least part of the second binding site are combined with the binding sites in the corresponding DNA strands, the second DNA strand, and the third DNA strand to obtain a DNA three-dimensional nanomaterial comprising a DNA nanoflower-shaped composite structure and a DNA nanogrid composite structure. According to an embodiment of the present application, during the preparation process, the polymerization of the first DNA strand, the second DNA strand, and the third DNA strand itself is less dependent on the bonding effect of metal ions, and metal ions and DNA topoisomerases may not be used to obtain a DNA three-dimensional nanomaterial comprising a DNA nanoflower-shaped composite structure and a DNA nanogrid composite structure.

[0077] In some optional embodiments, in S300, the volume of the DNA nanoflower-shaped composite structure is 0.0001-100 cubic microns; optionally ≥20 cubic microns; optionally, the DNA nanoflower-shaped composite structure has a spherical particle appearance and has stacked petal-shaped sheets inside.

[0078] In some optional embodiments, the diameter of the DNA nanoflower-shaped composite structure is 200-5000 nm.

[0079] In some optional embodiments, the area of ​​the DNA nanomesh composite structure on the projection surface is 100 μm 2 -1mm 2 ; Optionally, the DNA nanomesh composite structure has a grid layered appearance.

[0080] The DNA long chain synthesized by the rolling circle amplification method of the present application and the DNA long single chain can be cross-linked to form a nanomesh precursor and a nanoflower precursor. Under the action of topoisomerase, the nanomesh precursor is fixed as a DNA nanomesh composite structure. Under the action of light metal ions and DNA topoisomerase, the nanoflower precursor is converted into a DNA nanoflower-shaped composite structure with a topological structure. After freeze-drying, the DNA three-dimensional nanomaterial can be stored in a low-temperature dry environment for more than six months, has the characteristics of low cost and wide application, and solves the defect that the existing DNA three-dimensional material needs to be ready-to-use.

[0081] DNA 3D nanomaterials

[0082] In a second aspect, an embodiment of the present application provides a DNA three-dimensional nanomaterial prepared by the method of the first aspect.

[0083] According to an embodiment of the present application, the DNA three-dimensional nanomaterial includes one or more of a DNA nanoflower-shaped composite structure or a DNA nanogrid composite structure.

[0084] Taking advantage of the spontaneous stretching and curling properties of DNA three-dimensional nanomaterials, DNA three-dimensional nanomaterials can present the form of nanonets or nanospheres under different experimental conditions. The DNA nanogrid composite structure can be used as a nano DNA aptamer, DNA nanolayer, recruit stem cells, and enhance the effect of aptamers. It can be used for targeted recruitment of stem cells. The DNA nanoflower-shaped composite structure can be used in imaging, targeted drug delivery, cell uptake, etc. The DNA flower-shaped composite structure can carry fluorescent molecules and can carry a large number of fluorescent molecules into cells in a short time.

[0085] DNA three-dimensional nanomaterials have the following uses:

[0086] 1) Tissue engineering repair. The material can be attached to tissue engineering repair materials to enhance the attachment and migration ability of stem cells and to implant stem cells in a fixed location.

[0087] 2) Improve the delivery efficiency of live cell fluorescent dyes. It can be used for specific nucleic acid live cell dyes. It can greatly improve the delivery efficiency of small fluorescent molecules.

[0088] 3) Delivery of small molecule drugs: Active small molecules can be loaded to deliver them into cells, increasing the effective concentration in cells.

[0089] Example

[0090] The following examples more specifically describe the disclosure of the present application, which are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations are possible within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0091] Example 1

[0092] 1. Design of DNA nanostructures.

[0093] (https: / / sulcgroup.github.io / oxdna-viewer / #) and NUPACK

[0094] (https: / / www.nupack.org) simulated the design of DNA material raw materials, and obtained several sets of first DNA single-stranded raw materials and second DNA single-stranded raw materials through Shanghai Sangon, such as Loop1.1, Loop1.2, Loop2.1, Loop2.2, Loop3.1, Loop3.2. And based on the first DNA single-stranded raw materials and the second DNA single-stranded raw materials, base sequence linkers were designed, such as Linker1.1, Linker1.2, Linker2.1, Linker2.2, Linker3.1 and Linker3.2.

[0095] 2. Synthesis of circular DNA template: Cool the mixture of Loop1.1, Loop1.2, Linker1.1, and Linker1.2 in each group of four DNA short chains from 95°C to 37°C at a rate of 2°C per 2 minutes, and react at 37°C for 10 minutes. Add T4 DNA ligase and react at 16°C for 10 hours. Prepare the first DNA circular template, such as Fig.11 shown.

[0096] The mixture of four DNA short chains, Loop2.1, Loop2.2, Linker2.1, and Linker2.2 in each group, was cooled from 95°C to 37°C at a rate of 2°C per 2 minutes and reacted at 37°C for 10 minutes. T4 DNA ligase was added and the reaction was carried out at 16°C for 10 hours to prepare the second DNA circular template, as shown in FIG. Fig.12 shown.

[0097] The mixture of four DNA short chains, Loop3.1, Loop3.2, Linker3.1 and Linker3.2 in each group, was cooled from 95°C to 37°C at a rate of 2°C per 2 minutes and reacted at 37°C for 10 minutes. T4 DNA ligase was added and the reaction was carried out at 16°C for 10 hours to prepare the third DNA circular template, as shown in FIG. Fig.13 shown.

[0098] Table 1 Related base sequences.

[0099]

[0100]

[0101] 3. Preparation of long single-stranded DNA: Various circular DNA templates are reacted with their corresponding primers (Primer1, Primer2 and Primer3) and dNTp under the action of BST DNA polymerase at 62°C for 24-48 hours for PCR amplification to obtain long single-stranded DNA, including the first DNA single strand, the second DNA single strand and the third DNA single strand.

[0102] Example 2

[0103] The difference between this embodiment and embodiment 1 is that the first DNA single-stranded raw material and the second DNA single-stranded raw material are different, Loop1.1, Loop1.2, Loop2.1, Loop2.2, Loop3.1, Loop3.2. And based on the first DNA single-stranded raw material and the second DNA single-stranded raw material, base sequence linkers are designed, such as Linker1.1, Linker1.2, Linker2.1, Linker2.2, Linker3.1 and Linker3.2. The above sequences are shown in Table 2.

[0104]

[0105]

[0106] Example 3 DNA nanogrid composite structure

[0107] The first single-stranded DNA, the second single-stranded DNA and the third single-stranded DNA of this embodiment are obtained according to the method of the above-mentioned embodiment 1 or embodiment 2, respectively, and the added amounts are as follows: 4nM circular DNA template, 20nM primer, 56nM dNTP and 4U BstDNA polymerase mixture are prepared. The reaction conditions are 62°C and 48 hours. The solutions containing the three DNA long chains are mixed in equal molar proportions. The mixture is cooled from 95°C to 37°C at a rate of 2°C per 2 minutes, and reacted at 37°C for 10 minutes to self-assemble the DNA long chains into a precursor DNA nanomesh without topological structure. By reacting with DNA topoisomerase at 37°C for 15 minutes, a nanomesh with a stable topological structure is obtained, that is, the DNA nanomesh composite structure of the present application. The schematic flow chart of the preparation method of this embodiment is shown in the figure. Figure 1 shown.

[0108] Purification and storage: Purification was performed by removing soluble impurities separately using 3 times the liquid volume of isopropanol. The mixture of isopropanol and DNA high-dimensional material was incubated at -20°C for 20 minutes, then centrifuged at 12000rpm for 5 minutes, the supernatant was removed, and then freeze-dried in a vacuum to obtain a powder of pure DNA high-dimensional material, which was then freeze-dried in a vacuum freeze dryer and stored in a dry low-temperature environment. After freezing, observation was performed using an electron microscope, as shown below. Figure 2 The microstructure shown.

[0109] Example 4 DNA nanoflower-shaped composite structure

[0110] The first DNA single strand, the second DNA single strand and the third DNA single strand of this embodiment are prepared according to the method of the above-mentioned embodiment 1 or embodiment 2, respectively, and the added amounts are as follows: 1nM circular DNA template, 5nM primer, 3.5nM dNTP and 1U BstDNA polymerase mixture are prepared. The reaction conditions are 62°C and last for 12 hours. Subsequently, the three DNA long chain solutions are mixed in equal molar ratios, and MgCl 2 The solution was added to a final concentration of 10 nM, and then cooled from 95°C to 37°C at a rate of 2°C per 2 minutes, and reacted at 37°C for 10 minutes to self-assemble the long DNA chains into pre-DNA nanoflowers without topological structures. By reacting with DNA topoisomerase I at 37°C for 15 minutes, a nanoflower with a stable topological structure, i.e., a DNA nanoflower-shaped composite structure of the embodiment of the present application, was obtained. The schematic flow diagram of the preparation method of this embodiment is shown in FIG. Figure 3 shown.

[0111] Purification and storage: Purification was performed by removing soluble impurities separately using 3 times the liquid volume of isopropanol. The mixture of isopropanol and DNA high-dimensional material was incubated at -20°C for 20 minutes, then centrifuged at 12000rpm for 5 minutes, the supernatant was removed, and then freeze-dried in a vacuum to obtain a powder of pure DNA high-dimensional material, which was then freeze-dried in a vacuum freeze dryer and stored in a dry low-temperature environment. After freezing, observation was performed using an electron microscope, as shown below. Figure 4 The microstructure shown.

[0112] Example 5 Dual-modal nanomaterials comprising a DNA nanoflower composite structure or a DNA nanogrid composite structure

[0113] The first DNA single strand, the second DNA single strand and the third DNA single strand of this embodiment are obtained according to the method of the above-mentioned embodiment 1 or embodiment 2, respectively, and the added amounts are as follows: 2nM circular DNA template, 10nM RCA primer, 14nM dNTP, 2U Bst enzyme mixture. The reaction conditions are 62°C for 24 hours (Figure S5b). Subsequently, the three DNA long chain solutions are mixed in equal molar ratios. The mixture is cooled from 95°C to 37°C at a rate of 2°C per 2 minutes, and maintained at 37°C for 10 minutes to obtain a dual-modal nanomaterial comprising a DNA nanoflower-shaped composite structure or a DNA nanomesh composite structure. The schematic flow chart of the preparation method of this embodiment is shown in the figure. Figure 5 shown.

[0114] Purification and storage: Purification was performed by removing soluble impurities separately using 3 times the liquid volume of isopropanol. The mixture of isopropanol and DNA high-dimensional material was incubated at -20°C for 20 minutes, then centrifuged at 12,000 rpm for 5 minutes, the supernatant was removed, and then freeze-dried in a vacuum to obtain a powder of pure DNA high-dimensional material, which was then freeze-dried in a vacuum freeze dryer and stored in a dry low-temperature environment. The prepared bimodal nanomaterial containing a DNA nanoflower-shaped composite structure or a DNA nanogrid composite structure was dissolved in an aqueous solution and observed using an electron microscope, as shown below. Figure 6 The microstructure shown.

[0115] Comparative Example 1

[0116] The difference between this comparative example and Example 3 is that no DNA topoisomerase is used to participate in the reaction.

[0117] Comparative Example 2

[0118] The difference between this comparative example and Example 4 is that magnesium ions and DNA topoisomerase are not used to participate in the reaction.

[0119] Application Example 1 Directed Recruitment of Bone Marrow Mesenchymal Stem Cells

[0120] The 1nM probe containing Apt19s and the DNA nanomesh composite structure prepared in Example 3 were mixed at a mass concentration ratio of 1:6 to mount the aptamer on the mesh and assemble into a functionalized DNA nanomesh. The functionalized DNA nanomesh and equal concentrations of APT19s were fixed by UV to an area with a diameter of 1 cm in the center of the culture dish. Through light microscopy and crystal violet staining, it can be observed that there is obvious cell aggregation in the area where the functionalized DNA nanomesh is fixed, indicating that stem cells are recruited to the area where DNA is fixed and the recruitment effect of functionalized DNN is significantly higher than that of pure APT19s.

[0121] In addition, the DNA nanomesh composite structure prepared in Comparative Example 1 was prepared with a 1 nM probe containing Apt19s under the same experimental conditions. It can be observed that the cell recruitment effect is stronger than that of the pure APT19S group and smaller than that of the pure DNA nanomesh group, indicating that the pure DNA nanomesh has the strongest directional recruitment ability.

[0122] Application Example 2: Enhancement of Cellular Fluorescence Localization Probe Uptake

[0123] The DNA nanoflower composite structure prepared in Example 4 was mixed with 20 ng / μl of DNA fluorescent probe from Sangon and incubated at 25°C for 1 hour. The size of the positively charged DNA nanoflower particles carrying the DNA probe was 4313 nm. The cultured mixture was added to 1 ml of culture medium and acted on ATDC5 chondrogenic precursor cells from mice (concentration of 10 5 / L), using an imaging system with ultra-micro resolution to observe the effect. It can be observed that DNA nanoflowers can carry a large number of probes into cells within 30 minutes and show strong fluorescence signals.

[0124] In addition, the group using only 20 ng / μl DNA fluorescent probe had poor results.

[0125] In addition, the DNA nanoflower-shaped composite structure prepared in Comparative Example 2 was prepared with a 1 nM probe containing Apt19s under the same experimental conditions. It can be observed that the structure in Comparative Example 2 without topoisomerase and magnesium ion treatment has a much worse effect of entering cells than the nanoflower-shaped composite structure group in Example 3, indicating that the Example 3 group is the best form for carrying small molecule DNA into cells.

[0126] The possible reason is that there are a large number of DNA probe binding sites on the DNA nanoflower-shaped composite structure, which can carry a large number of DNA probes into cells at the same time. The experimental results observed by confocal fluorescence microscopy show that the DNA nanoflower-shaped composite structure in Example 4 is more stable than the structure in Comparative Example 2, resulting in the above-mentioned effect.

[0127] Experiments have shown that a DNA nanoflower concentration of 20 ng / μl is the optimal concentration for carrying probes into cells.

[0128] Test Section

[0129] Stability test: The DNA three-dimensional nanomaterials prepared in Examples 3-4 and Comparative Examples 1-2 were freeze-dried into powders, observed using an electron microscope, and then stored at room temperature for 6 months. They were then dissolved in water to make the concentration of the DNA three-dimensional nanomaterials in the water consistent. The DNA three-dimensional nanomaterials stored in the aqueous solution for 6 months were tested using a freeze-fracture electron microscope. The results shown in Table 3 were obtained. Figure 8-11 Pictures shown.

[0130] Table 3

[0131]

[0132] As can be seen from the figure, Figure 8-9The pictures of the three-dimensional DNA nanomaterials in Examples 3 and 4 are respectively the freeze-dried form before storage and the pictures of the three-dimensional DNA nanomaterials dissolved in water after storage. It can be seen from the pictures that the structure is stable, well preserved, and the original functional structure is maintained. Figure 10-11 The pictures of the DNA three-dimensional nanomaterials in comparative examples 1-2 without using DNA topoisomerase dissolved in water before and after storage at room temperature are shown in sequence. As can be seen from Table 3 and the figure, comparative examples 1-2 no longer have the original structure after being stored for 6 months, and have been degraded to a great extent. In this case, it needs to be used immediately after preparation and cannot be stored, while the DNA three-dimensional nanomaterials of Examples 3-4 have a stable structure after storage and can still be used.

[0133] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A method for preparing DNA three-dimensional nanomaterials, It is characterized in that include: A DNA circular template is provided, comprising: a first circular DNA template, a second circular DNA template and a third circular DNA template, wherein the first circular DNA template, the second circular DNA template and the third circular DNA template respectively comprise: a plurality of first base sequence segments distributed at intervals and a plurality of second base sequence segments distributed at intervals, and the first base sequence segment and / or the second base sequence segment in the first circular DNA template can match at least part of the base sequence segments in the second circular DNA template and the third circular DNA template respectively; According to the DNA circular template, a reaction is carried out under the action of a DNA polymerase to obtain a long single-stranded DNA whose bases are at least partially complementary to the DNA circular template, wherein the long single-stranded DNA includes a first single-stranded DNA, a second single-stranded DNA and a third single-stranded DNA; the first single-stranded DNA, the second single-stranded DNA and the third single-stranded DNA respectively contain: a plurality of first binding sites distributed at intervals and a plurality of second binding sites distributed at intervals; the first binding site and / or the second binding site in the first single-stranded DNA can respectively bind to at least a portion of the bases of the second single-stranded DNA and the third single-stranded DNA in a complementary manner; A mixture comprising the first DNA single strand, the second DNA single strand and the third DNA single strand is cooled from 90-97°C to 25-37°C at a rate of 2-4°C / min and reacted so that at least part of the first binding site and at least part of the second binding site bind to the corresponding binding sites in the DNA single strand, the second DNA single strand and the third DNA single strand, and under the action of DNA topoisomerase, the DNA three-dimensional nanomaterial is obtained.

2. The method according to claim 1, It is characterized in that The method for preparing the DNA circular template comprises: Providing a first single-stranded DNA raw material and a second single-stranded DNA raw material respectively, wherein the first single-stranded DNA raw material and the second single-stranded DNA raw material respectively include at least one first base sequence segment and at least one second base sequence segment distributed at intervals; The first DNA raw material single strand, the second DNA raw material single strand and the base sequence connecting segment are mixed, and under the action of DNA ligase, the DNA circular template is obtained.

3. The method according to claim 2, It is characterized in that According to the DNA circular template, preparing a long single-stranded DNA having at least some bases complementary to the DNA circular template with the participation of a primer comprises: The DNA circular template is amplified and reacted under the action of Bst DNA polymerase to achieve rolling circle replication. The reaction temperature is 52-62° C. and the reaction time is 6-48 hours to obtain a long single-stranded DNA whose bases are at least partially complementary to the DNA circular template.

4. The method according to any one of claims 1 to 3, It is characterized in that The molar ratio of the first DNA single strand, the second DNA single strand and the third DNA single strand is 1:(0.1-50):(0.1-50).

5. The method according to claim 4, It is characterized in that The DNA three-dimensional nanomaterial includes one or more of a DNA nanoflower-shaped composite structure or a DNA nanogrid composite structure.

6. The method according to claim 5, It is characterized in that A mixture comprising the first DNA single strand, the second DNA single strand and the third DNA single strand is cooled from 90-97°C to 25-37°C at a rate of 2-4°C / min and reacted under the action of metal ions, so that at least part of the first binding site and at least part of the second binding site are combined with the corresponding binding sites in the DNA single strand, the second DNA single strand and the third DNA single strand to obtain the DNA nanoflower-shaped composite structure, under the action of DNA topoisomerase, wherein the metal ions include one or more of magnesium ions, calcium ions, potassium ions and sodium ions.

7. The construction method according to claim 5 or 6, It is characterized in that The volume of the DNA nanoflower-shaped composite structure is 0.0001-100 cubic microns; optionally, it can be ≥20 cubic microns; optionally, the DNA nanoflower-shaped composite structure has a spherical particle appearance and has stacked petal-shaped sheets inside.

8. The construction method according to claim 5 or 6, It is characterized in that The diameter of the DNA nanoflower-shaped composite structure is 200-5000nm.

9. The construction method according to claim 5, It is characterized in that The area of ​​the DNA nanogrid composite structure on the projection surface is 100 μm 2 -1mm 2 ; Optionally, the DNA nanomesh composite structure has a grid layered appearance.

10. A DNA three-dimensional nanomaterial, It is characterized in that Prepared by the method according to any one of claims 1 to 9.