Uranium ore acid method agitation leaching method

By using column devices to oxidize ferrous in the lean liquid in the uranium ore acid stirring leaching process, the problem of frequent addition of oxidants in the existing process is solved, and the reduction of reagent consumption and the improvement of uranium ore leaching efficiency is achieved.

CN118895429APending Publication Date: 2024-11-05BEIJING RESEARCH INSTITUTE OF CHEMICAL ENGINEERING AND METALLURGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310494439.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing uranium ore acid stirring leaching process requires frequent addition of oxidants, resulting in high reagent consumption and increasing production costs.

Method used

By using a tandem column device in the stir leaching process, the ferrous in the recovered lean liquid is oxidized to trivalent iron and used to oxidize tetravalent uranium, the need for additional oxidizing agents is avoided.

Benefits of technology

The cyclic oxidation of ferrous in the lean liquid is achieved, which reduces the reagent consumption during the leaching process and improves the leaching efficiency and economicality of uranium ore.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of uranium ore processing, in particular to a uranium ore acid method agitation leaching method. The uranium ore acid method agitation leaching method comprises the following steps that 1, uranium ore suitable for acid method leaching is crushed and ground; 2, the ground ore and the extracting solution are mixed, the liquid-solid ratio of ore pulp is adjusted, and then sulfuric acid is added for a reaction; 3, the ore pulp is subjected to solid-liquid separation, and uranium is recycled from lixivium through an ion exchange method; and 4, the barren solution obtained in the step 3 enters one or more column type devices connected in series and stays in the column type devices for a certain time, and the outflowing solution enters the subsequent agitation leaching process. According to the method, an oxidizing agent does not need to be added during leaching, and the leaching reagent consumption can be effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of uranium ore processing, in particular to a method for acid-based stirring leaching of uranium ore. Background Art

[0002] In order to effectively improve the leaching rate of uranium ore, an oxidant is usually added to the stirring leaching to oxidize the difficult-to-leach tetravalent uranium in the ore into hexavalent uranium. In the acid stirring leaching, the commonly used oxidants are mainly pyrolusite, sodium chlorate, etc. The existing stirring leaching process is to add an oxidant when the uranium ore is ground or leached, and the leaching liquid is obtained after adsorption or extraction of uranium. Most of the lean liquid is directly returned to the next leaching. The oxidant used in leaching cannot be recycled, and additional addition is required for each stirring leaching. The cost of purchasing oxidants for mining companies each year accounts for a certain proportion of the production cost. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for acid-based stirring leaching of uranium ore, which does not require the addition of an oxidant during leaching and can effectively reduce the consumption of leaching reagents.

[0004] The present invention provides a method for acid-based stirring leaching of uranium ore, comprising the following steps:

[0005] Step 1: crushing and grinding the uranium ore suitable for acid leaching;

[0006] Step 2: Mix the ground ore with the extract, adjust the liquid-solid ratio of the slurry, and then add sulfuric acid to react;

[0007] Step 3: Separate the ore pulp into solid and liquid, and use ion exchange method to recover uranium from the leaching solution;

[0008] Step 4: The barren solution obtained in step 3 enters one or more column devices connected in series, stays in the column device for a certain period of time, and the outflowing solution enters the subsequent stirring leaching process.

[0009] Preferably, the ore grinding particle size is -32 mesh to -200 mesh.

[0010] Preferably, the liquid-to-solid ratio of the slurry is 0.5:1 to 5:1.

[0011] Preferably, the concentration of the sulfuric acid is 5 g / L to 100 g / L.

[0012] Preferably, the reaction temperature is 20°C to 90°C, and the reaction time is 0.5h to 4h.

[0013] Preferably, the column device is filled with waste residue or other forms of solid carriers.

[0014] Preferably, the column device contains a biological agent.

[0015] Preferably, the biological agent is a mixed autotrophic microorganism that can oxidize ferrous iron.

[0016] Preferably, the residence time of the lean solution is 2 h to 10 h.

[0017] Compared with the prior art, in the method for acid-based stirring leaching of uranium ore of the present invention, the barren solution obtained after uranium is recovered from the leaching solution is not directly returned to the leaching process, but stays in one or more column devices connected in series for a certain period of time, and the ferrous iron in the barren solution is oxidized into ferric iron before being returned to the leaching process. The ferric iron can oxidize tetravalent uranium. The method can effectively realize the cyclic oxidation of ferrous iron in the barren solution, and no additional oxidant needs to be added during stirring leaching, which can effectively reduce the consumption of leaching reagents. DETAILED DESCRIPTION

[0018] In order to further understand the present invention, the embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the present invention.

[0019] The embodiment of the present invention discloses a method for acid-based stirring leaching of uranium ore, comprising the following steps:

[0020] Step 1: crushing and grinding the uranium ore suitable for acid leaching;

[0021] The ore grinding particle size is -32 mesh to -200 mesh.

[0022] Step 2: Mix the ground ore with the extract, adjust the liquid-solid ratio of the slurry, and then add sulfuric acid to react;

[0023] The liquid-to-solid ratio of the slurry is 0.5:1 to 5:1.

[0024] The concentration of the sulfuric acid is 5 g / L to 100 g / L.

[0025] The reaction temperature is 20° C. to 90° C., and the reaction time is 0.5 h to 4 h.

[0026] Step 3: Separate the ore pulp into solid and liquid, and use ion exchange method to recover uranium from the leaching solution;

[0027] Step 4: The barren solution obtained in step 3 enters one or more column devices connected in series, stays in the column device for a certain period of time, and the outflowing solution enters the subsequent stirring leaching process.

[0028] The column device is filled with waste residue or other forms of solid carriers.

[0029] The column device also includes a biological agent.

[0030] The biological agent is a mixed autotrophic microorganism that can oxidize ferrous iron.

[0031] The residence time of the lean solution is 2 hours to 10 hours.

[0032] After passing through the column device, the redox potential of the outflowing solution is greater than 450mv.

[0033] The invention of this patent is that the barren solution obtained after the uranium is recovered from the leaching solution is not directly returned to the leaching, but stays in one or more column devices in series for a certain period of time before returning to the leaching. This method oxidizes the ferrous iron in the barren solution into ferric iron and then returns it to the leaching. The ferric iron can oxidize tetravalent uranium. This method can effectively realize the cyclic oxidation of ferrous iron in the barren solution.

[0034] In order to further understand the present invention, the method for acid-based stirring leaching of uranium ore provided by the present invention is described in detail below in conjunction with embodiments, and the protection scope of the present invention is not limited by the following embodiments.

[0035] Example 1

[0036] The uranium grade of a certain uranium mine is 0.105%, the tetravalent uranium content accounts for 75.2% of the total uranium, and the iron content in the ore is 2.78%.

[0037] The method of the present invention for treating the uranium ore comprises the following process steps:

[0038] (1) crushing and grinding the uranium ore to a particle size of -100 mesh;

[0039] (2) 100 g of the ore ground to a certain particle size in step (1) was added to a reaction vessel, the slurry liquid-to-solid ratio was adjusted to 1:1, sulfuric acid was added, the amount of sulfuric acid was 8%, and the reaction was carried out at 60° C. for 4 h; the solution used to adjust the slurry liquid-to-solid ratio was the solution of the lean solution obtained after the last stirred leaching solution after uranium recovery was retained in a column device filled with biological agents for 6 h;

[0040] (3) After step (2) is completed, the ore pulp is subjected to solid-liquid separation, the obtained leaching solution is used to recover uranium by ion exchange, and the leaching tailings are dried and analyzed for uranium content.

[0041] Test results: After adopting the process of the present invention, without adding an external oxidant, the uranium content of the leached tailings is 0.012%, and the uranium leaching rate of the slag is 88.6%.

[0042] Example 2

[0043] The uranium grade of a certain uranium mine is 0.105%, the tetravalent uranium content accounts for 75.2% of the total uranium, and the iron content in the ore is 2.78%.

[0044] The method of the present invention for treating the uranium ore comprises the following process steps:

[0045] (1) crushing and grinding the uranium ore to a particle size of -100 mesh;

[0046] (2) 2000 g of the ore ground to a certain particle size in step (1) was added to a reaction vessel, the slurry liquid-to-solid ratio was adjusted to 1:1, sulfuric acid was added, the amount of sulfuric acid was 8%, and the reaction was carried out at 60° C. for 4 h; the solution used to adjust the slurry liquid-to-solid ratio was the solution of the lean solution obtained after the uranium was recovered from the last stirred leaching solution after it was left in a column device filled with biological agents for 6 h;

[0047] (3) After step (2) is completed, the ore pulp is subjected to solid-liquid separation, the obtained leaching solution is used to recover uranium by ion exchange, and the leaching tailings are dried and analyzed for uranium content;

[0048] Experimental results: After adopting the process of the present invention, under the condition of no external oxidant, the uranium content of the leached tailings is 0.013%, and the uranium leaching rate of the slag is 87.6%.

[0049] Example 3

[0050] The uranium grade of a certain uranium mine is 0.085%, the tetravalent uranium content accounts for 62.4% of the total uranium, and the iron content in the ore is 2.35%.

[0051] The method of the present invention for treating the uranium ore comprises the following process steps:

[0052] (1) crushing and grinding the uranium ore to a particle size of -100 mesh;

[0053] (2) 100 g of the ore ground to a certain particle size in step (1) was added to a reaction vessel, the slurry liquid-to-solid ratio was adjusted to 1:1, sulfuric acid was added, the amount of sulfuric acid was 6%, and the reaction was carried out at 60° C. for 4 h; the solution used to adjust the slurry liquid-to-solid ratio was the solution of the lean solution obtained after the last stirred leaching solution after uranium recovery was retained in a column device filled with biological agents for 6 h;

[0054] (3) After step (2) is completed, the ore pulp is subjected to solid-liquid separation, the obtained leaching solution is used to recover uranium by ion exchange, and the leaching tailings are dried and analyzed for uranium content;

[0055] Experimental results: After adopting the process of the present invention, under the condition of no external oxidant, the uranium content of the leached tailings is 0.010%, and the uranium leaching rate of the slag is 88.2%.

[0056] Comparative Example 1

[0057] The uranium grade of a certain uranium mine is 0.105%, the tetravalent uranium content accounts for 75.2% of the total uranium, and the iron content in the ore is 2.78%.

[0058] The existing leaching process for treating the uranium ore includes the following process steps:

[0059] (1) crushing and grinding the uranium ore to a particle size of -100 mesh;

[0060] (2) 100 g of the ore ground to a certain particle size in step (1) was added to a reaction vessel, the slurry liquid-to-solid ratio was adjusted to 1:1, sulfuric acid and oxidant pyrolusite were added, the amount of sulfuric acid was 8%, and the amount of pyrolusite was 2.0%, and the reaction was carried out at 60° C. for 4 h; the solution used to adjust the slurry liquid-to-solid ratio was the lean solution obtained after adsorption of the last stirred leaching solution;

[0061] (3) After step (2) is completed, the ore pulp is subjected to solid-liquid separation, the obtained leaching solution is used to recover uranium by ion exchange, and the leaching tailings are dried and analyzed for uranium content.

[0062] Test results: The uranium content of the leached tailings is 0.012%, and the uranium leaching rate based on the slag is 88.6%.

[0063] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0064] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for acid-based stirring leaching of uranium ore, It is characterized in that The following steps are involved: Step 1: crushing and grinding the uranium ore suitable for acid leaching; Step 2: Mix the ground ore with the extract, adjust the liquid-solid ratio of the slurry, and then add sulfuric acid to react; Step 3: Separate the ore pulp into solid and liquid, and use ion exchange method to recover uranium from the leaching solution; Step 4: The barren solution obtained in step 3 enters one or more column devices connected in series, stays in the column device for a certain period of time, and the outflowing solution enters the subsequent stirring leaching process.

2. The method for acid-based agitation leaching of uranium ore according to claim 1, It is characterized in that The ore grinding particle size is -32 mesh to -200 mesh.

3. The method for acid-based agitation leaching of uranium ore according to claim 1, It is characterized in that The liquid-to-solid ratio of the slurry is 0.5:1 to 5:

1.

4. The method for acid-based agitation leaching of uranium ore according to claim 1, It is characterized in that The concentration of the sulfuric acid is 5 g / L to 100 g / L.

5. The method for acid agitation leaching of uranium ore according to claim 1, It is characterized in that The reaction temperature is 20° C. to 90° C., and the reaction time is 0.5 h to 4 h.

6. The method for acid-based agitation leaching of uranium ore according to claim 1, It is characterized in that The column device is filled with waste residue or other forms of solid carriers.

7. The method for acid-based agitation leaching of uranium ore according to claim 6, It is characterized in that The column device contains a biological agent.

8. The method for acid-based agitation leaching of uranium ore according to claim 7, It is characterized in that The biological agent is a mixed autotrophic microorganism that can oxidize ferrous iron.

9. The method for acid-based agitation leaching of uranium ore according to claim 1, It is characterized in that The residence time of the lean solution is 2 hours to 10 hours.