Light metal article with ceramic texture and manufacturing method thereof
Through anodizing and grinding and polishing technology, the ceramic texture appearance is formed for light metal objects, which solves the shortcomings of ceramic texture and high gloss in the existing technology, and achieves diverse color changes and corrosion resistance improvement.
Patent Information
- Application Number
- CN202311790991.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-02
- Filing Date
- 2023-12-22
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art cannot effectively provide light metal objects with ceramic texture appearance and high gloss, while meeting diverse color needs, and insufficient corrosion resistance.
Porous ceramic layer is formed by anodizing treatment, and a protective layer is formed on it. It is ground and polished with sandpaper. The glossiness of 60° is not less than 90GU and the surface roughness Ra is less than 0.1. Combined with dye filling and electrical pore sealing technology, multiple results are achieved. Color variation and ceramic texture.
It realizes the ceramic texture and high gloss of light metal objects, while improving its diversity and corrosion resistance, achieving a unique surface decorative effect.
Smart Images

Figure CN118895541A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a surface-treated light metal object and a manufacturing method thereof, in particular to a light metal object with a ceramic texture and a manufacturing method thereof. Background Art
[0002] Light metal generally refers to a density less than 5g / cm 3 Metal. Today's portable electronic products are increasingly trending towards thinner and lighter designs. Light metals have become a popular material for portable electronic device housings and mechanical parts due to their excellent physical and mechanical properties. Objects made of light metals are usually treated on the surface, such as sandblasting, polishing, anodizing (Anodic oxidation) or micro-arc oxidation (Micro-arcoxidation, MAO), to meet the product's appearance diversity and functionality.
[0003] CN 101591799B discloses a surface polishing method for a magnesium alloy, which can improve the surface gloss of the magnesium alloy material, but no film layer is generated on the surface of the magnesium alloy material, resulting in poor corrosion resistance.
[0004] CN 1392295A discloses that a silver-grey smooth film layer with beautiful appearance is formed on the surface of magnesium or magnesium alloy by anodic oxidation treatment, but it cannot meet various color requirements for product appearance.
[0005] CN 101311326A discloses that a black oxide film layer is formed on the surface of a light metal by micro-arc oxidation treatment, but the black oxide film layer cannot change the color effect of the light metal surface, nor can it change the gloss of the light metal surface.
[0006] CN 107190301A forms an oxide film on the surface of titanium or titanium alloy by anodizing, and changes the color of the film by operating voltage and current. However, it is difficult to control the thickness of the film under such operation, and the color stability is not high. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a method for manufacturing a light metal object with a ceramic texture in view of the shortcomings of the prior art, wherein the outer surface of the light metal object is ceramicized and has a high gloss through anodizing, surface coating, grinding and polishing. The present invention also provides a light metal object with a ceramic texture obtained by the method.
[0008] In order to solve the above-mentioned technical problems, one of the technical solutions adopted by the present invention is to provide a method for manufacturing a light metal object with a ceramic texture, which includes: providing a light metal object; forming an anodized layer on the outer surface of the light metal object, the anodized layer having a plurality of openings extending toward the outer surface of the light metal object; forming a protective layer on the anodized layer; and grinding the protective layer with sandpaper so that the 60° glossiness of the surface of the protective layer is not less than 90GU and the surface roughness Ra is less than 0.1, and the number of the sandpaper is between P500 and P10000.
[0009] In an embodiment of the present invention, in the step of grinding the protective layer, the number of the sandpaper is P2000.
[0010] In an embodiment of the present invention, in the step of grinding the protective layer, the thickness of the protective layer is reduced to 20% to 80% of the original thickness.
[0011] In an embodiment of the present invention, between the step of forming the anodized layer and the step of forming the protective layer, the method further includes: filling at least one dye into the plurality of openings of the anodized layer. Furthermore, in the step of forming the protective layer, a portion of the protective layer is filled into the plurality of openings of the anodized layer to seal the plurality of openings.
[0012] In an embodiment of the present invention, the anodizing treatment is performed in an electrolyte having a pH value of 8-13 and a temperature in a range of 5° C. to 40° C. Furthermore, the electrolyte contains an oxidant, a pH regulator, and a film-forming agent.
[0013] In an embodiment of the present invention, the oxidant is selected from the group consisting of sodium nitrate, potassium nitrate, potassium permanganate and potassium dichromate, the pH adjuster is selected from the group consisting of sodium hydroxide, potassium hydroxide, lithium hydroxide and magnesium hydroxide, and the film-forming agent is selected from the group consisting of sodium silicate, aluminum hydroxide, diammonium phosphate, sodium hexametaphosphate and trisodium phosphate.
[0014] In an embodiment of the present invention, the anodizing treatment is a pulsed anodizing treatment, which includes a voltage ramp-up stage and a voltage constant voltage stage following the voltage ramp-up stage, wherein the operating voltage of the voltage ramp-up stage is increased from an initial voltage to a target voltage, and the operating voltage of the voltage constant voltage stage is maintained at the target voltage.
[0015] In an embodiment of the present invention, the conditions of the pulsed anodizing treatment include: the initial voltage is 0V and the target voltage is 50V to 600V, the pulse frequency is 500Hz to 2000Hz, and the duty cycle is 1% to 50%. In addition, the duration of the voltage ramp-up phase is 1 minute to 10 minutes, and the duration of the voltage constant phase is 5 minutes to 60 minutes, which is more than twice the duration of the voltage ramp-up phase.
[0016] In an embodiment of the present invention, the protective layer is formed by a resin composition, the resin composition comprises an acrylic resin and a solid powder, the solid powder is a powder of a metal, a non-metal or its oxide, and the solid content of the resin composition is 3% to 30%. In addition, the protective layer is formed by electric sealing, and the implementation conditions of the electric sealing include: an operating voltage of 1V to 150V, and a duration of 30 seconds to 10 minutes.
[0017] In an embodiment of the present invention, the step of forming the protective layer further comprises: baking the resin composition under the following conditions: a baking temperature of 100° C. to 200° C., and a baking time of 15 minutes to 60 minutes.
[0018] In order to solve the above technical problems, another technical solution adopted by the present invention is to provide a light metal object with a ceramic texture, which includes a light metal object, an anodized layer and a protective layer. The anodized layer is formed on the outer surface of the light metal object and has a plurality of openings extending toward the outer surface of the light metal object. The protective layer is formed on the anodized layer to seal the plurality of openings. The 60° glossiness of the surface of the protective layer is not less than 90GU and the surface roughness Ra is less than 0.1.
[0019] One of the beneficial effects of the present invention is that the method for making a light metal object with a ceramic texture of the present invention, by means of "forming an anodized layer on the outer surface of the light metal object", "forming a protective layer on the anodized layer" and "grinding the protective layer with sandpaper with a number between P500 and P10000 so that the 60° glossiness of the surface of the protective layer is not less than 90GU and the surface roughness Ra is less than 0.1", allows the light metal object to have a variety of color changes and a ceramic texture appearance, thereby obtaining a unique surface decoration effect.
[0020] In order to further understand the features and technical contents of the present invention, please refer to the following detailed description and drawings of the present invention. However, the drawings provided are only for reference and description and are not intended to limit the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1It is a flow chart of a method for manufacturing a light metal object with ceramic texture according to an embodiment of the present invention.
[0022] Figure 2 Another flow chart of the method for manufacturing a light metal object with ceramic texture according to an embodiment of the present invention.
[0023] Figure 3 It is a schematic diagram of the processing stages of anodizing treatment used in the method for manufacturing a light metal object with ceramic texture according to an embodiment of the present invention.
[0024] Figure 4 It is a partial schematic diagram of a part of the structure of a light metal object with ceramic texture according to an embodiment of the present invention.
[0025] Figure 5 It is a partial schematic diagram of a complete structure of a light metal object with ceramic texture according to an embodiment of the present invention.
[0026] Figure 6 It is a partial schematic diagram of another complete structure of the light metal object with ceramic texture according to an embodiment of the present invention. DETAILED DESCRIPTION
[0027] The following is an explanation of the implementation methods of the "light metal object with ceramic texture and its manufacturing method" disclosed in the present invention through specific embodiments. Those skilled in the art can understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can be implemented or applied through other different specific embodiments, and the details in this specification can also be modified and changed in various ways based on different viewpoints and applications without departing from the concept of the present invention. In addition, the drawings of the present invention are only simple schematic illustrations and are not depicted according to actual dimensions. It is stated in advance. The following embodiments will further explain the relevant technical contents of the present invention in detail, but the disclosed contents are not intended to limit the scope of protection of the present invention. In addition, the term "or" used in this article may include any one or more combinations of the associated listed items depending on the actual situation.
[0028] Unless otherwise defined, the terms used herein have the same meanings as those generally understood by those skilled in the art. The materials involved in each embodiment are commercially available or prepared according to the prior art unless otherwise specified. The process methods involved in each embodiment are the process methods commonly used in the art unless otherwise specified.
[0029] It should be understood that although the steps in the method flow chart are described in a specific order in this article, this does not require or imply that the steps must be performed in this specific order, or that all steps must be performed to achieve the desired result. Optionally, multiple steps can be combined into one step for execution, or one step can be decomposed into multiple steps for execution.
[0030] See also Figure 1 As shown, an embodiment of the present invention provides a method for making a light metal object with a ceramic texture, which mainly includes: step S100, providing a light metal object; step S102, forming an anodized layer on the outer surface of the light metal object; step S104, forming a protective layer on the anodized layer; and step S106, grinding the protective layer using sandpaper with a number between P500 and P10000. Specifically, the technical solution in the embodiment of the present invention is to ceramicize the outer surface of the light metal object and have a high gloss through anodizing, surface coating, grinding and polishing.
[0031] Cooperate Figure 4 and Figure 5 As shown, after the above steps are completed, a light metal object Z with a ceramic texture can be obtained, which includes a light metal object 1, an anodized layer 2 and a protective layer 3. The light metal object 1 has an outer surface 100, and the anodized layer 2 is formed on the outer surface 100 of the light metal object 1 and has a plurality of openings 200, wherein the plurality of openings 200 are formed on the anodized layer 2 in a manner extending toward the outer surface 100 of the light metal object 1. The protective layer 3 is formed on the anodized layer 2 and seals the plurality of openings 200, and in addition, the 60° glossiness of the surface 300 of the protective layer 3 is not less than 90GU and the surface roughness Ra is less than 0.1μm.
[0032] Hereinafter, each step of the method for manufacturing the light metal object with ceramic texture of the present invention will be described in detail.
[0033] In step S100, the light metal object 1 may be made of aluminum, magnesium, titanium or alloys thereof. In addition, the light metal object 1 may be formed in a variety of ways, such as die casting, extrusion, forging and cutting, to have a shape (such as a thin sheet) required for practical applications, so that it can be used as an appearance part of an electronic product such as a housing.
[0034] In step S102, the anodized layer 2 is a crystalline porous ceramic layer formed by anodizing. During the execution process, the light metal object 1 is used as an anode and immersed in an alkaline electrolyte, and the cathode is made of corrosion-resistant material such as stainless steel. Under specific operating conditions, a well-adhered anodized layer 2 is formed on the entire outer surface 100 of the light metal object 1. In an embodiment of the present invention, the alkaline electrolyte contains an oxidant, a pH adjuster and a film-forming agent, and the pH value of the alkaline electrolyte is 8-13 and the temperature is in the range of 5°C to 40°C. In addition, the thickness of the anodized layer 2 is in the range of 3μm to 50μm, the appearance is uniform white or gray, and the surface roughness Ra is less than 1.0μm.
[0035] The oxidant may be selected from the group consisting of sodium nitrate, potassium nitrate, potassium permanganate and potassium dichromate, the pH regulator may be selected from the group consisting of sodium hydroxide, potassium hydroxide, lithium hydroxide and magnesium hydroxide, and the film-forming agent may be selected from the group consisting of sodium silicate, aluminum hydroxide, ammonium dihydrogen phosphate, sodium hexametaphosphate and trisodium phosphate. Furthermore, the contents of the oxidant, pH regulator and film-forming agent may be reasonably adjusted according to the performance requirements of the electrolyte. However, the present invention is not limited to the above examples.
[0036] Preferably, with Figure 3 As shown, the anodizing treatment of step S102 is a pulse anodizing treatment, which may include a voltage rise stage M1 and a voltage constant voltage stage M2 following the voltage rise stage M1, wherein the operating voltage of the voltage rise stage M1 is increased from 0V to the target voltage Vt, and the operating voltage of the voltage constant voltage stage M2 is maintained at the target voltage Vt. Further, the operating conditions of the pulse anodizing treatment include: the initial voltage is 0V and the target voltage Vt is 50V to 600V, the pulse frequency is 500Hz to 2000Hz, and the duty cycle is 1% to 50%. In addition, the duration of the voltage rise stage M1 is 1 minute to 10 minutes, and the duration of the voltage constant voltage stage M2 is 5 minutes to 60 minutes, which is more than twice the duration of the voltage rise stage M1. Under such operation, the surface smoothness and compactness of the anodized layer 2 can be improved by controlling the nucleation rate, growth rate and dissolution rate of magnesium oxide, and a plurality of openings 200 are regularly arranged and evenly distributed on the anodized layer 2. Furthermore, compared with general anodizing treatment, the anodizing treatment of the present invention is also beneficial for reducing power consumption and improving production efficiency.
[0037] In an embodiment of the present invention, the target voltage Vt of the pulsed anodizing treatment may be 50V, 100V, 150V, 200V, 250V, 300V, 350V, 400V, 450V, 500V, 550V or 600V; the pulse frequency may be 500Hz, 600Hz, 700Hz, 800Hz, 900Hz, 1000Hz, 1100Hz, 1200Hz, 1300Hz, 1400Hz, 1500Hz, 1600Hz, 1700Hz, 1800Hz, 1900Hz or 2000Hz; the duty cycle may be 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%.
[0038] In addition Figure 2 As shown, the method for making a light metal object with a ceramic texture of the present invention may also include a pretreatment step, that is, pretreatment of the light metal object 1 before anodizing (step S101). It should be noted that the means of pretreatment vary with different purposes; for example, the means of pretreatment may include degreasing, decarburization, alkali washing, acid washing or any combination thereof to remove defects, dirt, natural oxide film, etc. on the outer surface 100 of the light metal object 1; or, the means of pretreatment may include polishing, sandblasting or a combination of the two to produce a special surface effect.
[0039] In step S104, the protective layer 3 is formed by electric sealing. During the execution process, the light metal object 1 is immersed in the resin composition, and the resin component is migrated to the light metal object 1 by an external electric field, so as to be deposited on the anodized layer 2 to form a uniform coating. Further, the protective layer 3 is formed by a resin composition, which comprises an acrylic resin and a solid powder, and may further comprise a colorant as required. The solid content of the resin composition is 3% to 30%, so that the performance requirements such as gloss, hardness, and weather resistance can be met. The solid powder may be a powder of a metal, a non-metal or its oxide. Specific examples of solid powders include: powders of aluminum oxide, titanium oxide, silicon dioxide, iron oxide, tin oxide, and powders of aluminum, gold, silver, and iron. The implementation conditions of electric sealing may include: an operating voltage of 1V to 150V, and a duration of 30 seconds to 10 minutes. Then, the coating film attached to the anodized layer 2 can be cured into the protective layer 3 by baking, and the baking conditions include: a baking temperature of 100° C. to 200° C. and a baking time of 15 minutes to 60 minutes. In addition, a portion of the protective layer 3 is filled in the plurality of openings 200 of the anodized layer 2 to seal the plurality of openings 200.
[0040] See also Figure 2 And cooperate Figure 4 and Figure 6As shown, the method for making a light metal object with a ceramic texture of the present invention may also include: between the step of forming the anodized layer 2 (step S102) and the step of forming the protective layer 3 (step S104), a step of dyeing the light metal object 1 (step S103). During the execution process, the light metal object 1 is immersed in a dye, so that the color component 4 in the dye, such as an organic pigment, is deposited on the anodized layer 2 and at least partially penetrates into the multiple openings 200; after completion, a water washing process can be performed as needed to remove the color component 4 that is not in the opening 200. It is worth noting that the present invention controls the configuration and arrangement distribution of the multiple openings 200 on the anodized layer 2 through the set pulse voltage operation stage, including the voltage slow rise stage M1 and the voltage constant voltage stage M2, which can achieve the effect of easy and more uniform dyeing. In addition, in the presence of the protective layer 3, the color component 4 can be stably maintained in the multiple openings 200 of the anodized layer 2 for a long time, so that the light metal object 1 has a variety of color changes.
[0041] In step S106, the protective layer 3 is ground and polished using sandpaper with a number between P500 and P10000, preferably sandpaper with a number of P2000, so that the 60° glossiness of the surface 300 of the protective layer 3 is not less than 90GU and the surface roughness Ra is less than 0.1μm. Therefore, the glossiness of the outer surface 100 of the light metal object 1 can be increased while achieving ceramicization. In an embodiment of the present invention, the sandpaper used for grinding and polishing may contain abrasive particles of the following materials: garnet, corundum, aluminum oxide, silicon oxide, zinc oxide and / or chromium oxide. After grinding and polishing, the thickness of the protective layer 3 is reduced to 20% to 80% of the original.
[0042] The method for making the light metal object with ceramic texture of the present invention will be further described in the following specific examples, but the specific examples are only used as examples and should not be construed as limiting the implementation methods of the present invention.
[0043] Specific example 1
[0044] The object of AZ91D magnesium alloy is immersed in an electrolyte with a pH of 12, the temperature of the electrolyte is 10°C, which contains potassium pernitrate (as an oxidant), potassium hydroxide (as a pH adjuster) and sodium silicate (as a film-forming agent), and pulse anodizing treatment is carried out under the following conditions: the target voltage of the voltage ramp-up stage is 200V, the pulse frequency is 1000Hz, the duty cycle is 7%, the voltage ramp-up stage lasts for 5 minutes, and the voltage constant stage lasts for 20 minutes. After completion, an anodized layer with a thickness of 20μm is formed. The anodized object is immersed in a red dye for dyeing for 15 minutes to obtain an object with a red appearance. The object with a red appearance is immersed in a resin composition comprising acrylic resin and alumina powder (total solid content is 12%), and the holes are sealed at a voltage of 20V for 5 minutes, and then baked at 180°C for 30 minutes. After completion, sandpaper containing silicon oxide (No. P2000) was used for grinding and polishing to obtain a 10 μm thick red high-gloss ceramic-textured object with a 60° glossiness of 95GU and a surface roughness Ra of 0.08 μm.
[0045] Specific example 2
[0046] The object of AZ31B magnesium alloy is immersed in an electrolyte with a pH of 13, the temperature of the electrolyte is 20°C, and it contains potassium permanganate (as an oxidant), sodium hydroxide (as a pH adjuster) and a combination of sodium hexametaphosphate and trisodium phosphate (as a film-forming agent), and pulse anodizing treatment is carried out under the following conditions: the target voltage of the voltage ramp-up stage is 250V, the pulse frequency is 800Hz, the duty cycle is 5%, the voltage ramp-up stage lasts for 3 minutes, and the voltage constant stage lasts for 30 minutes. After completion, an anodized layer with a thickness of 30μm is formed. The anodized object is immersed in a resin composition containing acrylic resin and silica powder (total solid content is 16%), and the holes are sealed at a voltage of 30V for 3 minutes, and then baked at 160°C for 60 minutes. After completion, the surface was ground and polished using sandpaper containing aluminum oxide (No. P7000) to obtain a 20 μm thick white high-gloss ceramic object with a 60° glossiness of 100 GU and a surface roughness Ra of 0.05 μm.
[0047] Specific example 3
[0048] The object of 6063 aluminum alloy is immersed in an electrolyte with a pH of 11 and a temperature of 18°C. It contains sodium nitrate (as an oxidant), sodium hydroxide (as a pH adjuster) and aluminum hydroxide (as a film-forming agent), and pulse anodizing is carried out under the following conditions: the target voltage of the voltage ramp-up stage is 150V, the pulse frequency is 1200Hz, the duty cycle is 10%, the voltage ramp-up stage lasts for 3 minutes, and the voltage constant stage lasts for 10 minutes. After completion, an anodized layer with a thickness of 15μm is formed. The anodized object is immersed in a blue dye for dyeing for 30 minutes to obtain an object with a blue appearance. The object with a blue appearance is immersed in a resin composition comprising acrylic resin and titanium dioxide powder (total solid content is 10%), and is electrically sealed at a voltage of 100V for 3 minutes, and then baked at 200°C for 30 minutes. After completion, sandpaper containing aluminum oxide (No. P10000) was used for grinding and polishing to obtain a 9 μm thick blue high-gloss ceramic-textured object with a 60° glossiness of 92GU and a surface roughness Ra of 0.03 μm.
[0049] Specific example 4
[0050] The pure titanium object is immersed in an electrolyte with a pH of 13 and a temperature of 10°C. The electrolyte contains potassium nitrate (as an oxidant), lithium hydroxide (as a pH adjuster) and a combination of sodium silicate and sodium hexametaphosphate (as a film-forming agent), and pulse anodizing is performed under the following conditions: the target voltage of the voltage ramp-up phase is 120V, the pulse frequency is 1500Hz, the duty cycle is 8%, the voltage ramp-up phase lasts for 2 minutes, and the voltage constant phase lasts for 12 minutes. After completion, an anodized layer with a thickness of 10μm is formed. The anodized object is immersed in a resin composition containing acrylic resin and silver powder (total solid content is 14%), and the holes are sealed at a voltage of 25V for 10 minutes, and then baked at 170°C for 40 minutes. After completion, sandpaper containing diamond sand (No. P2000) was used for grinding and polishing to obtain a 4 μm thick gray high-gloss ceramic-textured object with a 60° glossiness of 90GU and a surface roughness Ra of 0.08 μm.
[0051] Advantageous Effects of Embodiments
[0052] One of the beneficial effects of the present invention is that the method for making a light metal object with a ceramic texture of the present invention, by means of "forming an anodized layer on the outer surface of the light metal object", "forming a protective layer on the anodized layer" and "grinding the protective layer with sandpaper with a number between P500 and P10000 so that the 60° glossiness of the surface of the protective layer is not less than 90GU and the surface roughness Ra is less than 0.1", allows the light metal object to have a variety of color changes and a ceramic texture appearance, thereby obtaining a unique surface decoration effect.
[0053] Furthermore, the anodizing treatment used in the method for making a light metal object with a ceramic texture of the present invention is a pulse anodizing treatment, which may include a voltage boosting stage and a voltage constant voltage stage following the voltage boosting stage. Under such operation, the surface smoothness and density of the anodized layer can be improved by controlling the nucleation rate, growth rate and dissolution rate of magnesium oxide, and multiple openings can be arranged regularly and evenly distributed on the anodized layer. Moreover, compared with the general anodizing treatment, the anodizing treatment of the present invention is also conducive to reducing power consumption and improving production efficiency.
[0054] Furthermore, the present invention controls the configuration and arrangement distribution of multiple openings on the anodized layer through the set pulse voltage operation stage, including the voltage ramp-up stage and the voltage constant stage, so as to achieve the effect of easier and more uniform dyeing.
[0055] The contents disclosed above are only preferred feasible embodiments of the present invention, and are not intended to limit the protection scope of the claims of the present invention. Therefore, all equivalent technical changes made using the contents of the present invention description and drawings are included in the protection scope of the claims of the present invention.
Claims
1. A method for manufacturing a light metal object with a ceramic texture, characterized in that: The method for manufacturing the light metal object with ceramic texture comprises: Provide light metal objects; forming an anodized layer on the outer surface of the light metal object, wherein the anodized layer has a plurality of openings extending toward the outer surface of the light metal object; forming a protective layer on the anodized layer; and The protective layer is ground using sandpaper so that the 60° glossiness of the surface of the protective layer is not less than 90GU and the surface roughness Ra is less than 0.1, wherein the number of the sandpaper is between P500 and P10000.
2. The method for manufacturing a light metal object with ceramic texture according to claim 1, characterized in that: In the step of grinding the protective layer, the number of the sandpaper is P2000.
3. The method for manufacturing a light metal object with ceramic texture according to claim 2, characterized in that: In the step of grinding the protective layer, the thickness of the protective layer is reduced to 20% to 80% of the original thickness.
4. The method for manufacturing a light metal object with ceramic texture according to claim 1, characterized in that: Between the step of forming the anodized layer and the step of forming the protective layer, it also includes: filling at least one dye into the multiple openings of the anodized layer; in the step of forming the protective layer, a portion of the protective layer is filled in the multiple openings of the anodized layer to seal the multiple openings.
5. The method for manufacturing a light metal object with ceramic texture according to claim 1 or 4, characterized in that: The anodizing treatment is carried out in an electrolyte having a pH value of 8-13 and a temperature in the range of 5° C. to 40° C.; the electrolyte contains an oxidant, a pH regulator and a film-forming agent.
6. The method for manufacturing a light metal object with ceramic texture according to claim 5, characterized in that: The oxidant is selected from the group consisting of sodium nitrate, potassium nitrate, potassium permanganate and potassium dichromate, the pH adjuster is selected from the group consisting of sodium hydroxide, potassium hydroxide, lithium hydroxide and magnesium hydroxide, and the film-forming agent is selected from the group consisting of sodium silicate, aluminum hydroxide, diammonium phosphate, sodium hexametaphosphate and trisodium phosphate.
7. The method for manufacturing a light metal object with ceramic texture according to claim 6, characterized in that: The anodizing treatment is a pulsed anodizing treatment, which includes a voltage ramp-up phase and a voltage constant voltage phase following the voltage ramp-up phase. The operating voltage in the voltage ramp-up phase is increased from an initial voltage to a target voltage, and the operating voltage in the voltage constant voltage phase is maintained at the target voltage.
8. The method for manufacturing a light metal object with ceramic texture according to claim 7, characterized in that: The conditions for the pulsed anodizing treatment include: the initial voltage is 0V and the target voltage is 50-600V, the pulse frequency is 500Hz to 2000Hz, and the duty cycle is 1% to 50%; the duration of the voltage ramp-up phase is 1 minute to 10 minutes, and the duration of the voltage constant phase is 5 minutes to 60 minutes, which is more than twice the duration of the voltage ramp-up phase.
9. The method for manufacturing a light metal object with ceramic texture according to claim 1 or 4, characterized in that: The protective layer is formed by a resin composition, which includes an acrylic resin and solid powder. The solid powder is a powder of metal, non-metal or its oxide, and the solid content of the resin composition is 3% to 30%. The protective layer is formed by electric sealing, and the implementation conditions of the electric sealing include: an operating voltage of 1V to 150V and a duration of 30 seconds to 10 minutes.
10. The method for manufacturing a light metal object with ceramic texture according to claim 9, characterized in that: The step of forming the protective layer further includes: baking the resin composition under the following conditions: a baking temperature of 100° C. to 200° C. and a baking time of 15 minutes to 60 minutes.
11. A light metal object with a ceramic texture, characterized in that: The light metal object with ceramic texture includes: Light metal objects; an anodized layer formed on an outer surface of the light metal object and having a plurality of openings extending toward the outer surface of the light metal object; and A protective layer is formed on the anodized layer to seal the plurality of openings; wherein the 60° glossiness of the surface of the protective layer is not less than 90GU and the surface roughness Ra is less than 0.1.