Solid, liquid and gas separation method in polycarbosilane melt spinning process
By designing solid, liquid and gas separation devices during the melt spinning process of polycarbonsilane, the problems of molecular weight distribution control and state separation are solved, the purification and gas purification of liquid polycarbonsilane are realized, and the preparation quality of SiC fibers is improved. .
Patent Information
- Application Number
- CN202410921099.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
AI Technical Summary
During the melt spinning process of polycarbonsilane, it is difficult to detect and control the molecular weight distribution of PCS, resulting in the lack of obvious separation of solid, liquid and gas. Liquid polycarbonsilane is easy to volatilize and flammable, and it is difficult to handle solid, liquid and gas in the same furnace. , affects fiber performance.
A solid, liquid and gas separation device including melting tanks, piggy tanks and gas recovery tanks was designed. Through step-by-step vacuum treatment and nitrogen filling, the molecular weight control and state separation of PCS are realized to ensure the condensation of liquid polycarbonsilane and Gas recovery.
It effectively improves the softening point and spinning properties of PCS, realizes the purification of liquid polycarbosilane and gas purification, reduces resource waste, and improves the preparation quality of SiC fibers.
Smart Images

Figure CN118895577A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polycarbosilane preparation, and particularly relates to a method for separating solid, liquid and gas in a polycarbosilane melt spinning process. Background Art
[0002] At present, the preparation method of silicon carbide (SiC) fiber is mainly the organic precursor polycarbosilane (PCS) conversion method. This method generally includes the synthesis of organic precursor polycarbosilane (PCS), melt spinning, infusibility treatment and high temperature sintering (high temperature inorganicization) and other processes. Among them, the synthesis of polycarbosilane (PCS) precursor is the basis of all research work. The composition, structure and performance of PCS directly affect the spinnability and infusibility reaction activity of PCS, thereby affecting the composition, structure and performance of the final SiC fiber. As a precursor polymer, PCS needs to have a high melting point and good spinnability to meet the requirements of subsequent processes.
[0003] Spinnability refers to the deformation ability of a fluid under stable stretching operation, that is, the ability of a liquid to form continuous slender filaments under stretching. It can be seen that the spinnability of PCS is restricted by its rheological properties, and according to the Mark-Houwink-Sakurada empirical formula, the melt viscosity and molecular weight have the following relationship: [η] = KM°, where [η]---melt characteristic viscosity; M--viscosity average molecular weight; K, α--constants, related to the molecular form. It can be seen that the melt viscosity is restricted by the molecular weight, that is, the spinnability of PCS is restricted by the molecular weight.
[0004] Studies have shown that PCS with high molecular weight has high ceramic yield and less volatile matter during sintering, thus forming fewer defects. Therefore, the high molecular weight part of PCS is beneficial to fiber strength.
[0005] The low molecular weight part acts as a plasticizer in the spinning process, which is beneficial to improving spinnability. In the synthesis process of PCS, it was found that as the reaction conditions were strengthened, the softening point of PCS increased, the molecular weight increased, the molecular weight distribution gradually widened, and the spinnability gradually decreased. It can be seen that the spinnability of PCS is also related to the molecular weight distribution. related.
[0006] It can be seen that PCS with lower molecular weight has better spinnability, but if the molecular weight is too high and the branching degree is too large, the spinnability of PCS will decrease. Therefore, it is of great significance to study the relationship between the softening point molecular weight and its distribution of PCS and melt spinnability, and to increase the high molecular weight part as much as possible while ensuring spinnability, for the preparation of high-performance SiC fibers.
[0007] In addition, the traditional melt spinning of polycarbosilane precursor is to load the precursor powder into the spinning cylinder, place it in a vacuum degassing furnace, heat it to the specified degassing temperature under vacuum and keep it warm for 3 hours. That is, the traditional vacuum degassing treatment of the precursor is to degas directly in a furnace (such as Figure 2 There are the following problems:
[0008] 1. It is difficult to observe or detect the molecular weight distribution of PCS in the molten state;
[0009] 2. The corresponding solid, liquid and gas separation is not obvious or insufficient, and there is no corresponding basis for judgment;
[0010] 3. Liquid polycarbosilane (LPCS) is separated. These low molecular weight liquid polycarbosilane (LPCS) have low boiling points and high vapor pressures, and are very volatile at room temperature. They are easy to burn when encountering static electricity or high temperatures, and are a volatile and flammable liquid. The existing disposal method is to seal them in containers and transport them to hazardous chemical disposal companies for harmless treatment.
[0011] 4. It is difficult to carry out subsequent treatment and processing of solid, liquid and gas in the same furnace. If the escaped small molecules are not separated, it will affect the subsequent melt spinning.
[0012] In view of this, the inventor of this case conducted in-depth research, which resulted in the creation of this case. Summary of the invention
[0013] The object of the present invention is to provide a method for separating solid, liquid and gas in the melt spinning process of polycarbosilane having a higher melting point (softening point) and better spinnability.
[0014] In order to achieve the above object, the technical solution of the present invention is:
[0015] A method for separating solid, liquid and gas in a polycarbosilane melt spinning process is based on a solid, liquid and gas separation device in a polycarbosilane melt spinning process.
[0016] The solid, liquid and gas separation device in the polycarbosilane melt spinning process comprises a melting tank, a storage tank and a gas recovery tank, wherein the melting tank, the storage tank and the gas recovery tank are connected in sequence through a connecting switch;
[0017] The present invention provides a method for separating solid, liquid and gas in a polycarbosilane melt spinning process, comprising the following steps:
[0018] Step S1: adding PCS into the melting tank, and confirming that the connection switch between the melting tank and the storage tank, and the connection switch between the storage tank and the gas recovery tank are both in an open state;
[0019] Step S2: After the PCS is left to stand for at least one hour, the interior of the melting tank, the storage tank and the gas recovery tank is vacuumed for the first time, and then filled with nitrogen, followed by a second vacuuming and then filled with nitrogen. The vacuuming time for each time is at least half an hour, until the pressure of the melting tank, the storage tank and the gas recovery tank reaches -0.06Mpa to -0.08Mpa;
[0020] Step S3: After the second vacuuming is completed, the connection switch between the melting tank and the storage tank is closed;
[0021] Step S4: continuously evacuating the melting tank and setting target temperature values of the melting tank and the spinneret assembly according to process requirements;
[0022] When the melting tank and the spinning assembly are heated, when the temperature of the melting tank rises to the temperature at the bottom of the tank reaching the set temperature, the temperature is kept for half an hour, and then the vacuum pump of the melting tank is turned off, and the connection switch between the melting tank and the storage tank is turned on (at this time, the pressure difference on both sides must be consistent);
[0023] Step S5: When the temperature of the bottom of the melting tank reaches another set temperature, the PCS in the melting tank is stirred, and after confirming that the temperature of each part in the melting tank reaches the set process temperature, the PCS is kept warm and allowed to stand for degassing, and the escaped small molecule PCS is condensed in the storage tank and becomes liquid, and is stored in the storage tank. A liquid scale is provided inside the storage tank, and the escaped gas enters the gas recovery tank for recovery or storage;
[0024] Step S6: When the small molecules to be removed meet the production demand, nitrogen is filled into the melting tank, and the nitrogen brought into the floating substances in the melting tank is brought into the storage tank, and the small molecule PCS is condensed and liquefied in the storage tank and stored inside the storage tank, and the remaining gas enters the gas recovery tank along with the nitrogen;
[0025] Then the chamber pressures of the melting tank, the storage tank and the gas recovery tank are monitored. After the chambers of the melting tank, the storage tank and the gas recovery tank reach normal pressure, the connecting switch between the melting tank and the storage tank, and the connecting switch between the storage tank and the gas recovery tank are closed to make the melting tank, the storage tank and the gas recovery tank independently spaced; then, nitrogen is continuously filled into the melting tank until the positive pressure reaches 0.06Mpa~0.08Mpa, and then the melt spinning step is carried out, and then the corresponding liquid polycarbosilane in the storage tank can be purified and recovered; the gas in the gas recovery tank can be treated as exhaust gas from the gas discharge port.
[0026] Furthermore, a vacuum pump, an air intake system, a heating coil, a pressure sensor and a temperature sensor are arranged on one side wall of the melting tank, and the heating coil is evenly distributed along the outer wall of the tank furnace; an exhaust valve is arranged on the other side wall of the melting tank, a feeding port and a stirring motor are arranged on the top of the melting tank, and a discharge port is arranged on the bottom of the melting tank;
[0027] An air intake system and a pressure sensor are provided on one side wall of the storage tank, an exhaust valve is provided on the other side wall of the storage tank, a vacuum pump is provided on the top of the storage tank, a liquid discharge port is provided on the bottom of the storage tank, and the liquid scale is vertically provided inside the storage tank, with the bottom end of the liquid scale located at the bottom of the storage tank;
[0028] An air intake system and a pressure sensor are arranged on the side wall of the gas recovery tank, a vacuum pump is arranged on the top of the gas recovery tank, and a gas discharge port is arranged on the bottom of the gas recovery tank.
[0029] Furthermore, the number of the temperature sensors of the melting tank is six, which are correspondingly arranged at the upper part, the middle part and the lower part of the two side walls inside the tank furnace.
[0030] Furthermore, the connection switch between the melting tank and the storage tank is a high temperature resistant electric hard-sealed gate valve; the connection switch between the storage tank and the gas recovery tank is a high temperature resistant electric hard-sealed gate valve.
[0031] Furthermore, the liquid scale is a transparent scale.
[0032] Furthermore, in step S1, the exhaust valve of the melting tank is opened, it is confirmed that the melting tank is at normal pressure, and then the exhaust valve of the melting tank is closed.
[0033] Further, in step S2, after standing for at least one hour, the vacuum pump of the melting tank, the vacuum pump of the storage tank and the vacuum pump of the gas recovery tank are started, and the first vacuuming is performed and nitrogen is filled in, and then the second vacuuming is performed and nitrogen is filled in; the nitrogen pressure reaches -0.05MPa, and then the vacuum pump of the melting tank, the vacuum pump of the storage tank and the vacuum pump of the gas recovery tank are turned off.
[0034] Further, in step S4, when setting the target temperature values of the melting tank and the spinneret assembly, the thermal polymerization adopts a stepwise heating method, and the heating process is as follows: heating to 100°C and keeping warm for 0.5h, heating to 150°C and keeping warm for 0.5h, heating to 190°C and keeping warm for 0.5h, heating to 250°C and keeping warm for 0.5h, heating to 300°C and keeping warm for 0.5h, heating to 350°C and keeping warm for 0.5h, heating to 380°C and keeping warm for 6h;
[0035] When the melting tank and the spinning assembly are heated, when the temperature of the melting tank rises to 190° C. or higher at the bottom of the melting tank, the temperature is maintained for half an hour.
[0036] Furthermore, in step S5, when the temperature at the bottom of the melting tank reaches above 290°C, stirring is started at a speed of 1min / 5r. After stirring for 2 hours, stirring is stopped. After confirming that the temperature of each part has reached the set process temperature, insulation and standing for degassing are started.
[0037] The present invention provides a method for separating solid, liquid and gas in a polycarbosilane melt spinning process, which has the following beneficial properties:
[0038] 1. A solid, liquid and gas separation device in the process of polycarbosilane melt spinning is divided into three areas: solid stirring preheating area, liquid recovery area, and gas recovery tank. The three areas are directly connected through a connecting switch. The three areas can be merged when necessary and separated according to actual production needs to achieve solid-liquid-gas separation in the melt spinning process and better control the molecular weight distribution of the product. This equipment has low investment and simple operation, can effectively achieve separation, and greatly improve product quality.
[0039] 2. A corresponding liquid scale is set in the liquid recovery area to observe the amount of PCS input and the amount of overflowed small molecule liquid PCS according to the factory inspection data of PCS input, calculate the corresponding vacuum degassing degree, and control the molecular weight range of PCS input;
[0040] 3. The present invention can separate liquid polycarbosilane (LPCS), which can be used for subsequent composite material preparation after purification.
[0041] 4. Liquid (storage tank) and gas (gas recovery tank) are equipped with their own discharge ports, which can be recycled separately;
[0042] 5. The newly added storage tank can make the removed small molecules escape and cool down, the liquid enters the storage tank, and the gas enters the gas recovery tank;
[0043] 6. Liquid polycarbosilane and gas filtration and purification treatment are realized, effectively reducing resource waste.
[0044] 7. In order to obtain PCS with a higher softening point and good spinnability, its molecular weight distribution must be controlled so that its dispersion coefficient is about 1.8-2.2, the high molecular weight content is about 10%-30%, and the low and medium molecular weight content is about 80%. Through the patent of this invention, PCS with a higher softening point, a smaller dispersion coefficient, and good spinnability can be obtained as a good precursor for preparing SiC fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1It is a schematic diagram of a solid, liquid and gas separation device in the polycarbosilane melt spinning process of the present invention;
[0046] Figure 2 Schematic diagram of degassing in a furnace during the melt spinning process of polycarbosilane in the background technology.
[0047] In the figure:
[0048] Melting tank a; storage tank b; gas recovery tank c; vacuum pump 1; feeding port 2; stirring motor 3; exhaust valve 4; air intake system 5; heating coil 6; pressure sensor 7; temperature sensor 8; feed port 9; gate valve 10; air intake system 11; pressure sensor 13; liquid feed port 14; liquid scale 15; exhaust valve 16; gate valve 17; air intake system 18; vacuum pump 19; pressure sensor 20. DETAILED DESCRIPTION
[0049] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.
[0050] The present invention provides a method for separating solid, liquid and gas in a polycarbosilane melt spinning process, based on a device for separating solid, liquid and gas in a polycarbosilane melt spinning process, such as Figure 1 As shown, it includes a melting tank a, a storage tank b and a gas recovery tank c, and the three tanks are connected in sequence through high-temperature resistant electric hard-sealed gate valves.
[0051] The melting tank a is a tank furnace structure and is used as a solid stirring preheating zone. A vacuum pump 1, an air intake system 5, a heating coil 6, a pressure sensor 7 and a temperature sensor 8 are provided on one side wall of the melting tank a. The heating coil 6 is evenly distributed along the outer wall of the tank furnace so that the PCS is heated evenly without direct contact with the PCS. There are six temperature sensors 8, which are correspondingly arranged at the upper, middle and lower parts of the two side walls inside the tank furnace to monitor the temperature inside the tank furnace. An exhaust valve 4 is provided on the other side wall of the melting tank a (the side opposite to the vacuum pump 1). A feeding port 2 and a stirring motor 3 are provided on the top of the melting tank a. A discharge port 9 is provided at the bottom of the melting tank a.
[0052] The vacuum pump 1 evacuates the inside of the melting tank. The feeding port 2 is used for feeding. The stirring motor 3 is used to stir the molten PCS during the vacuum degassing stage or the spinning stage to make the heating uniform. The exhaust valve 4 is used to exhaust gas and keep the pressure in the furnace consistent with the atmosphere when necessary. The air intake system 5 can be filled with inert gases such as nitrogen and argon as protective gas. The pressure sensor 7 monitors the pressure in the tank furnace in real time. The unloading port 9 is used to unload the PCS in the molten state.
[0053] Storage tank b is a tank furnace structure and is used as a liquid recovery area. An air intake system 11 and a pressure sensor 13 are provided on one side wall of storage tank b, and an exhaust valve 16 is provided on the other side wall of storage tank b. A vacuum pump 12 is provided on the top of storage tank b. A liquid discharge port 14 is provided at the bottom of storage tank b. A liquid scale 15 is vertically provided inside storage tank b, and the bottom end of the liquid scale 15 is located at the bottom of storage tank b. The liquid scale 15 is specifically a transparent scale.
[0054] The air intake system 11 can be filled with inert gases such as nitrogen and argon to act as protective gas. The vacuum pump 12 can evacuate the interior of the storage tank b. The pressure sensor 13 monitors the pressure inside the storage tank b in real time. The liquid scale 15 recovers the small molecules in the liquid recovery area, and can monitor the volume of the small molecule liquid inside the storage tank b in real time. The small molecule content is calculated according to the relative molecular weight of the PCS put into the melting tank a furnace and the liquid amount (volume) measured by the liquid scale 15 inside the storage tank b. Specifically, under normal circumstances, the small molecules that escape from 100kg of PCS are about 160±40g. According to the factory inspection data of the PCS, the types and quantities of small molecules that may be contained in the PCS are understood. Through experimental or empirical data, the volatilization rate of these small molecules at specific temperatures and pressures is understood. Combined with the vacuum degree, temperature and time of the melting tank a, the degree of removal of small molecules is estimated. The liquid scale 15 shows that the amount or level of liquid in the storage tank b has stabilized, and there is no significant overflow of small molecule liquid. According to calculation or estimation, the removed small molecular weight has reached the expected target value or met the production standard.
[0055] The gas recovery tank c is used as a gas recovery tank. The side wall of the gas recovery tank c is provided with an air intake system 18 and a pressure sensor 20, the top of the gas recovery tank c is provided with a vacuum pump 19, and the bottom of the gas recovery tank c is provided with a gas discharge port. The air intake system 18 can be filled with inert gases such as nitrogen and argon as protective gas. The vacuum pump 19 can evacuate the interior of the gas recovery tank c. The pressure sensor 20 can monitor the pressure inside the gas recovery tank c in real time.
[0056] The melting tank a is connected to the storage tank b through the gate valve 10, and the storage tank b is connected to the gas recovery tank c through the gate valve 17. The gate valves 10 and 17 are high temperature resistant electric hard seal gate valves. Electric energy is used as power to connect the electric actuator to drive the valve to realize the opening and closing and regulating actions of the valve. Thus, the purpose of opening and closing or regulating the pipeline medium is achieved.
[0057] The control system of the device of the present invention adopts Omron PLC and MCGS touch screen control, and the entire system flow chart corresponds to the operation on the touch screen, including the start and stop of each vacuum pump, coil heating, stirring start and stop, and the operation, control and interlocking of each gate valve switch. Specifically, the corresponding control components of the vacuum pump start and stop, coil heating, stirring start and stop, and gate valve switch are electrically connected to the control system respectively to achieve corresponding control.
[0058] The present invention discloses a solid, liquid and gas separation device in the process of polycarbosilane melt spinning. The device is divided into three areas: a melting tank a, a storage tank b and a gas recovery tank c. The three areas are connected by a gate valve. Solid PCS is heated in the melting tank a and stirred for 1 min / (5-20 rpm) in a molten state for vacuum degassing. The escaped small molecules are condensed and converted into liquid PCS and stored in the storage tank. The gas can enter the next tank for recovery or storage.
[0059] It should be noted that, in the solid, liquid and gas separation device in the polycarbosilane melt spinning process of the present invention, before the separation operation is performed, the melting tank a, the storage tank b and the gas recovery tank c are interconnected (ie, the gate valve 10 and the gate valve 17 are both open).
[0060] The present invention provides a method for separating solid, liquid and gas in a polycarbosilane melt spinning process, comprising the following steps:
[0061] Step S1: Open the exhaust valve 4, confirm that the melting tank a is at normal pressure, and close the exhaust valve 4. Add PCS into the melting tank a of the spinning machine from the feeding port 2; and confirm that the connection switch between the melting tank and the storage tank, and the connection switch between the storage tank and the gas recovery tank are both in the open state;
[0062] Step S2: The PCS is allowed to stand for at least 1 hour. The standing period allows the PCS to better adapt to the temperature in the melting tank a and reduce potential problems caused by temperature fluctuations. The standing period can provide initial preparation time for subsequent reactions. This helps ensure that the reaction can proceed smoothly and effectively in the subsequent steps.
[0063] Then start vacuum pump 1, vacuum pump 12 and vacuum pump 19 to perform the first vacuuming and fill with nitrogen, then perform the second vacuuming and fill with nitrogen; each vacuuming time is at least half an hour, until the pressure of melting tank a, storage tank b and gas recovery tank c reaches -0.06Mpa to -0.08Mpa or above; the nitrogen pressure should reach -0.05MPa, and then turn off vacuum pump 1, vacuum pump 12 and vacuum pump 19;
[0064] Step S3: After the second vacuuming is completed, close the connection switch (gate valve 10) between the melting tank a and the storage tank b; record the time and pressure of the two vacuuming in step S2; (gate valve 17 is not closed) keep the storage tank b and the gas recovery tank c interconnected and the air pressure consistent.
[0065] Step S4: Turn on the vacuum pump 1 of the melting tank a, continuously evacuate the melting tank a, and set the target temperature values of the melting tank a and the spinneret assembly according to the process requirements. Specifically, the thermal polymerization adopts a stepwise heating method, and the heating process is as follows: heating to 100°C and keeping warm for 0.5h, heating to 150°C and keeping warm for 0.5h, heating to 190°C and keeping warm for 0.5h, heating to 250°C and keeping warm for 0.5h, heating to 300°C and keeping warm for 0.5h, heating to 350°C and keeping warm for 0.5h, and heating to 380°C and keeping warm for 6h.
[0066] When heating the melting tank a and the spinning assembly, when the temperature of the melting tank a rises to above 190°C at the bottom of the melting tank a, keep it warm for half an hour, first close the vacuum pump valve of the vacuum pump 1, then close the vacuum pump 1, and open the gate valve 10 to connect the melting tank a and the storage tank b;
[0067] Step S5: When the temperature at the bottom of the melting tank a reaches above 290°C, start stirring at a speed of 1min / 5r to ensure uniform heating. Stop stirring after 2 hours of stirring. After confirming that the temperature of each part reaches the set process temperature, start heat preservation and stand for degassing. The escaped small molecules are condensed in the storage tank b and become liquid and stored in the storage tank b. The gas can enter the next tank (gas recovery tank c) for recovery or storage.
[0068] At this time, according to the liquid scale 15 in the storage tank b, according to the factory inspection data of the PCS input, the amount of PCS input and the amount of small molecule liquid PCS overflowed can be observed, and the corresponding vacuum degassing degree (small molecule escape) can be calculated to control the molecular weight range of the PCS input. Specifically, the small molecules that escape from the normal 100kg PCS input are about 160±40g. According to the factory inspection data of the PCS input, understand the types and quantities of small molecules that may be contained in the PCS. Through experiments or empirical data, understand the volatilization rate of these small molecules at specific temperatures and pressures. Combined with the vacuum degree, temperature and time of the melting tank a, estimate the degree of removal of small molecules.
[0069] Step S6: When the small molecules to be removed meet the production demand, the types and quantities of small molecules that may be contained in PCS are understood based on the factory inspection data of the PCS. Through experimental or empirical data, the volatilization rate of these small molecules at specific temperature and pressure is understood. Combined with the vacuum degree, temperature and time of the melting tank a, the degree of removal of small molecules is estimated. The liquid scale 15 shows that the amount or liquid level of the liquid in the storage tank b has stabilized, and there is no significant overflow of small molecule liquid. According to calculation or estimation, the small molecular weight removed has reached the expected target value or meets the production standard.
[0070] At this time, nitrogen is slowly filled into the melting tank a. The nitrogen filled into the melting tank a will bring the floating substances (small molecules, etc.) in the melting tank a into the storage tank b. The small molecules will be condensed and liquefied in the storage tank b, and the remaining gases will enter the gas recovery tank c along with the nitrogen filled into the melting tank a. After the chamber pressures of the melting tank a, the storage tank b and the gas recovery tank c all reach normal pressure, the gate valves 10 and 17 are closed to make the three areas independently spaced. At this time, the melting tank a continues to be filled with nitrogen until the positive pressure reaches 0.06Mpa to 0.08Mpa, and then the melt spinning step is carried out; the corresponding liquid polycarbosilane (LPCS) in the storage tank b can be purified and recovered; the gas in the gas recovery tank can be treated as tail gas from the gas discharge port.
[0071] The present invention provides a method for separating solid, liquid and gas in a polycarbosilane melt spinning process, which has the following beneficial properties:
[0072] 1. A solid, liquid and gas separation device in the process of polycarbosilane melt spinning is divided into three areas: solid stirring preheating area, liquid recovery area and gas recovery tank. The three areas are directly connected through gate valves. The three areas can be merged when necessary and separated according to actual production needs to achieve solid-liquid-gas separation in the melt spinning process. This equipment has low investment and simple operation, can effectively achieve separation, and greatly improve product quality.
[0073] 2. A corresponding liquid scale 15 is set in the liquid recovery area to observe the amount of PCS input and the amount of overflowed small molecule liquid PCS according to the factory inspection data of PCS input, calculate the corresponding vacuum degassing degree, and control the molecular weight range of PCS input;
[0074] 3. The present invention can separate liquid polycarbosilane (LPCS), which can be used for subsequent composite material preparation after purification.
[0075] 4. Liquid (storage tank b) and gas (gas recovery tank c) are provided with respective discharge ports, and can be recycled and processed separately;
[0076] 5. The newly added storage tank b can make the removed small molecules escape and after cooling, the liquid enters the storage tank b and the gas enters the gas recovery tank c;
[0077] 6. Liquid polycarbosilane and gas filtration and purification treatment are realized, effectively reducing resource waste.
[0078] 7. In order to obtain PCS with a higher softening point and good spinnability, its molecular weight distribution must be controlled so that its dispersion coefficient is about 1.8-2.2, the high molecular weight content is about 10%-30%, and the low and medium molecular weight content is about 80%. The method of the present invention can synthesize PCS with a higher softening point, a smaller dispersion coefficient, and good spinnability, and is a good precursor for preparing SiC fibers.
[0079] The above embodiments and drawings do not limit the method of the present invention. Any appropriate changes or modifications made thereto by a person of ordinary skill in the art should be deemed to be within the patent scope of the present invention.
Claims
1. A method for separating solid, liquid and gas in a polycarbosilane melt spinning process, characterized in that: Based on a solid, liquid and gas separation device in the polycarbosilane melt spinning process, The solid, liquid and gas separation device in the polycarbosilane melt spinning process comprises a melting tank, a storage tank and a gas recovery tank, wherein the melting tank, the storage tank and the gas recovery tank are connected in sequence through a connecting switch; The present invention provides a method for separating solid, liquid and gas in a polycarbosilane melt spinning process, comprising the following steps: Step S1: adding PCS into the melting tank, and confirming that the connection switch between the melting tank and the storage tank, and the connection switch between the storage tank and the gas recovery tank are both in an open state; Step S2: After the PCS is left to stand for at least one hour, the interior of the melting tank, the storage tank and the gas recovery tank is vacuumed for the first time, and then filled with nitrogen, followed by a second vacuuming and then filled with nitrogen. The vacuuming time for each time is at least half an hour, until the pressure of the melting tank, the storage tank and the gas recovery tank reaches -0.06Mpa to -0.08Mpa; Step S3: After the second vacuuming is completed, the connection switch between the melting tank and the storage tank is closed; Step S4: continuously evacuating the melting tank and setting target temperature values of the melting tank and the spinneret assembly according to process requirements; When the melting tank and the spinning assembly are heated, when the temperature of the melting tank rises to the temperature at the bottom of the tank reaching the set temperature, the temperature is kept for half an hour, and then the vacuum pump of the melting tank is turned off, and the connection switch between the melting tank and the storage tank is turned on; Step S5: When the temperature of the bottom of the melting tank reaches another set temperature, the PCS in the melting tank is stirred, and after confirming that the temperature of each part in the melting tank reaches the set process temperature, the PCS is kept warm and allowed to stand for degassing, and the escaped small molecule PCS is condensed in the storage tank and becomes liquid, and is stored in the storage tank. A liquid scale is provided inside the storage tank, and the escaped gas enters the gas recovery tank for recovery or storage; Step S6: When the small molecules to be removed meet the production demand, nitrogen is filled into the melting tank, and the nitrogen brought into the floating substances in the melting tank is brought into the storage tank, and the small molecule PCS is condensed and liquefied in the storage tank and stored inside the storage tank, and the remaining gas enters the gas recovery tank along with the nitrogen; Then the chamber pressures of the melting tank, the storage tank and the gas recovery tank are monitored. After the chambers of the melting tank, the storage tank and the gas recovery tank reach normal pressure, the connecting switch between the melting tank and the storage tank, and the connecting switch between the storage tank and the gas recovery tank are closed to make the melting tank, the storage tank and the gas recovery tank independently spaced; then, nitrogen is continuously filled into the melting tank until the positive pressure reaches 0.06Mpa~0.08Mpa, and then the melt spinning step is carried out, and then the corresponding liquid polycarbosilane in the storage tank can be purified and recovered; the gas in the gas recovery tank can be treated as exhaust gas from the gas discharge port.
2. The method for separating solid, liquid and gas in a polycarbosilane melt spinning process according to claim 1, characterized in that: A vacuum pump, an air intake system, a heating coil, a pressure sensor and a temperature sensor are arranged on one side wall of the melting tank, and the heating coils are evenly distributed along the outer wall of the tank furnace; an exhaust valve is arranged on the other side wall of the melting tank, a feeding port and a stirring motor are arranged on the top of the melting tank, and a discharge port is arranged on the bottom of the melting tank; An air intake system and a pressure sensor are provided on one side wall of the storage tank, an exhaust valve is provided on the other side wall of the storage tank, a vacuum pump is provided on the top of the storage tank, a liquid discharge port is provided on the bottom of the storage tank, and the liquid scale is vertically provided inside the storage tank, with the bottom end of the liquid scale located at the bottom of the storage tank; An air intake system and a pressure sensor are arranged on the side wall of the gas recovery tank, a vacuum pump is arranged on the top of the gas recovery tank, and a gas discharge port is arranged on the bottom of the gas recovery tank.
3. The method for separating solid, liquid and gas in a polycarbosilane melt spinning process according to claim 2, characterized in that: The number of the temperature sensors of the melting tank is six, which are correspondingly arranged at the upper part, the middle part and the lower part of the two side walls inside the tank furnace.
4. The method for separating solid, liquid and gas in a polycarbosilane melt spinning process according to claim 1, characterized in that: The connection switch between the melting tank and the storage tank is a high temperature resistant electric hard-sealed gate valve; the connection switch between the storage tank and the gas recovery tank is a high temperature resistant electric hard-sealed gate valve.
5. The method for separating solid, liquid and gas in a polycarbosilane melt spinning process according to claim 1, characterized in that: The liquid scale is a transparent scale.
6. The method for separating solid, liquid and gas in a polycarbosilane melt spinning process according to claim 2, characterized in that: In step S1, the exhaust valve of the melting tank is opened, and it is confirmed that the melting tank is at normal pressure, and then the exhaust valve of the melting tank is closed.
7. The method for separating solid, liquid and gas in a polycarbosilane melt spinning process according to claim 2, characterized in that: In step S2, after standing for at least one hour, the vacuum pump of the melting tank, the vacuum pump of the storage tank and the vacuum pump of the gas recovery tank are started, and the first vacuuming is performed and nitrogen is filled in, and then the second vacuuming is performed and nitrogen is filled in again; the nitrogen pressure reaches -0.05MPa, and then the vacuum pump of the melting tank, the vacuum pump of the storage tank and the vacuum pump of the gas recovery tank are turned off.
8. The method for separating solid, liquid and gas in a polycarbosilane melt spinning process according to claim 2, characterized in that: In step S4, when setting the target temperature values of the melting tank and the spinneret assembly, the thermal polymerization adopts a stepwise heating method, and the heating process is as follows: heating to 100°C and keeping warm for 0.5h, heating to 150°C and keeping warm for 0.5h, heating to 190°C and keeping warm for 0.5h, heating to 250°C and keeping warm for 0.5h, heating to 300°C and keeping warm for 0.5h, heating to 350°C and keeping warm for 0.5h, and heating to 380°C and keeping warm for 6h; When the melting tank and the spinning assembly are heated, when the temperature of the melting tank rises to 190° C. or higher at the bottom of the melting tank, the temperature is maintained for half an hour.
9. The method for separating solid, liquid and gas in a polycarbosilane melt spinning process according to claim 8, characterized in that: In step S5, when the temperature at the bottom of the melting tank reaches above 290°C, stirring is started at a speed of 1min / 5r. After stirring for 2 hours, stirring is stopped. After confirming that the temperature of each part has reached the set process temperature, insulation and static degassing are started.