Method for representing modification residual degree of SBS modified asphalt polymer based on cross-mechanical behavior of static mechanical mechanics-dynamic rheology
Through the cross-mechanical behavior characterization method of static mechanical mechanics and dynamic rheology, combined with gray correlation analysis, the problem of difficult to distinguish and repair SBS-modified asphalt is solved, and the modification of SBS-modified asphalt polymers is achieved Accurate characterization of degree and recovery of material properties.
Patent Information
- Application Number
- CN202411166036.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art is difficult to effectively distinguish and repair SBS modified asphalt of different aging degrees, resulting in the repair and regeneration of the same structure being unable to achieve good results, affecting the recovery of the high temperature and elastic properties of the material.
Using a cross-mechanical behavior characterization method based on static mechanical mechanics-dynamic rheology, the comprehensive toughness index CTI and recovery rate R value were extracted through low-temperature stress-strain test and multiple stress creep recovery test, and combined with gray correlation analysis, polymerization was determined. The residue level of the substance is modified, and it provides repair solutions for different aging degrees.
This method can clarify the physically meaningful comprehensive toughness index CTI, reduce time and material consumption, find critical parameters that distinguish the degree of modification residue of aged SBS modified asphalt polymer, improve the recovery rate of high temperature and elastic properties of the material, and achieve different Accurate characterization and repair of aging degree.
Smart Images

Figure CN118896839A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for characterizing the residual degree of polymer modification of SBS modified asphalt. Background Art
[0002] Asphalt is widely used in roads and pavements due to its low cost, relatively easy application, and good mechanical properties under load conditions. In order to solve the problem that ordinary asphalt pavements are prone to rutting, potholes, cracks, and spalling, the road performance of asphalt pavements has dropped sharply and the service life has been seriously shortened, SBS modified asphalt was used to pave pavements internationally in the 1990s. SBS modified asphalt is made by adding SBS modifier to asphalt through high-speed shearing and stirring at a certain temperature. SBS is a triblock copolymer composed of styrene-butadiene-styrene (styrene-butadiene-styrene, SBS) segments. With the extension of service time, the modifier SBS, like the asphalt matrix, will also be affected by the external environment and naturally age, resulting in the deterioration of the road performance of the pavement paved with its modified asphalt. As a result, after a certain service life, the severely damaged pavement needs to be repaired or rebuilt to restore the service performance of the pavement, which will generate a large amount of waste SBS modified asphalt mixture. Research on the recycling technology of waste SBS modified asphalt mixture is an important issue facing my country's highway industry.
[0003] The polymer gives SBS modified asphalt unique mechanical properties and rheological properties. The addition of polymer SBS to asphalt gives it a very unique toughness performance compared to the base asphalt. This can be seen from the linearity of the curve in the stress-strain experiment at low temperature. The stress-strain curve has a strain strengthening stage, and a large fracture strain and a second peak appear in the curve. In the rheological experiment, it reflects more excellent high temperature performance and unique elastic recovery performance.
[0004] In actual engineering, the regeneration of aged asphalt cannot clearly distinguish between base asphalt and SBS modified asphalt. Commercial regeneration agents, aromatic oils, waste engine oils, vegetable oils and asphalt mastics are often used to regenerate aged asphalt mastics in modified asphalt. This regeneration process is mainly considered to be physical blending, which only supplements the light components lost due to aging, and can improve the fatigue resistance and low-temperature crack resistance of the material. However, due to the neglect of repairing the broken polymer network, the high temperature, elasticity and other properties of the material cannot be quickly restored. The current road service situation is very complicated. The aging degree of different SBS modified asphalt pavements is not the same. For slightly and severely aged SBS modified asphalt, due to the differences in the depolymerization and decrosslinking behavior of its polymer components, the residual effect of the polymer in the aged asphalt is not the same. Structural repair and regeneration of all aged SBS modified asphalts cannot achieve good results in regenerating SBS modified asphalt. In order to solve this problem, it is necessary to analyze and characterize the residual degree of polymer modification of SBS modified asphalt after aging. Summary of the invention
[0005] The present invention aims to solve the technical problem that the same structural repair and regeneration of SBS modified asphalt with different aging degrees cannot achieve good results in regenerating SBS modified asphalt, and to provide a method for characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanics-dynamic rheology.
[0006] The method of the present invention for characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology is carried out in the following steps:
[0007] First, prepare SBS modified asphalt and the corresponding base asphalt, and then prepare samples of SBS modified asphalt and base asphalt for different aging times;
[0008] Second, the SBS modified asphalt samples with different aging times obtained in the first test were subjected to stress-strain tests at 4°C to obtain the corresponding stress-strain curves, analyze the curve line shape, extract characteristic parameters, define the comprehensive toughness index CTI (Comprehensive Toughness Index CTI), and calculate the CTI values of the SBS modified asphalt with different aging times; the calculation formula of the CTI is as follows:
[0009]
[0010] Where:
[0011] CTI is the comprehensive toughness index, which comprehensively reflects the energy absorption capacity, ductility and strength index of the material and is dimensionless;
[0012] T eIt is the toughness area in the stress-strain curve. The toughness area represents the area of the part of the stress-strain curve caused by the ductility of the material, and the unit is MPa;
[0013] ε B Fracture strain, the strain value corresponding to the material when it breaks, reflects the ductility of the material, dimensionless; obtained through the stress-strain curve;
[0014] σ max is the maximum stress, which refers to the maximum stress value that the material bears during the stretching process, σ max is Y and σ B The larger value in MPa; Y is the yield strength, σ B is the fracture strength; obtained through stress-strain curve;
[0015] 3. The SBS modified asphalt samples with different aging times obtained in the first test and the corresponding matrix asphalt were subjected to a multiple stress creep recovery test (MSCR) respectively. The loading process was cycled 10 times at 3.2 kPa, and each cycle included 1 s creep and 9 s recovery. The recovery rate R value of the SBS modified asphalt with different aging times and the recovery rate R value of the matrix asphalt were calculated. The recovery rate R value of the SBS modified asphalt with different aging times was subtracted from the recovery rate R value of the matrix asphalt to obtain the recovery rate R value of the SBS modified asphalt with different aging times after eliminating the mechanical error.
[0016] 4. Fitting the CTI values of the SBS modified asphalt with different aging times obtained in step 2 with an S-shaped curve to obtain two inflection points, which correspond to two CTI values C1 and C2, respectively, where C1<C2;
[0017] The recovery rate R value of the SBS modified asphalt at different aging times after eliminating the mechanical error obtained in step 3 is fitted with an S-shaped curve to obtain two inflection points, which correspond to two R values R1 and R2, respectively, where R1<R2;
[0018] The criterion for judging the high degree of polymer modification residue is: CTI>C2;
[0019] The judgment criteria for the medium degree of polymer modification residue are: C1<CTI≤C2 and R1<the recovery rate R value of SBS modified asphalt at different aging times after eliminating mechanical error≤R2. If the two conditions cannot be met at the same time, it is classified as a low degree of polymer modification residue.
[0020] Another criterion for judging the low degree of polymer modification residue is: CTI≤C1.
[0021] The present invention provides a method for analyzing the residual degree of polymer modification of SBS modified asphalt by synergistically combining low-temperature stress-strain curve and high-temperature multiple stress creep recovery test. Based on low-temperature toughness and high-temperature viscoelasticity tests, according to parameter extraction definition and grey correlation analysis, a method for characterizing the residual degree of polymer modification of aged SBS modified asphalt is determined.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention uses the low-temperature stress-strain curve to extract the comprehensive toughness index CTI, which has a clear physical meaning and can reduce most of the time and material consumption compared with other tests;
[0024] 2. The present invention adopts a transmechanical behavior characterization method of obtaining CTI value by static mechanical mechanics and recovery rate R value by dynamic shear mechanics to find the critical parameters for distinguishing the residual degree of polymer modification of aged SBS modified asphalt. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a characteristic parameter diagram of the asphalt stress-strain double peak curve in step 2 of the present invention;
[0026] Figure 2 The stress-strain curves of SBS modified asphalt with different aging degrees in Test 1;
[0027] Figure 3 This is the stress-strain curve of 70# matrix asphalt with different aging degrees in Test 1;
[0028] Figure 4 This is the CTI value variation curve of SBS modified asphalt with different aging degrees in Test 1;
[0029] Figure 5 This is the result of the SBS modified asphalt viscosity-shear rate curve fitting in Test 1;
[0030] Figure 6 This is the viscosity-shear rate curve fitting result of 70# matrix asphalt in test 1;
[0031] Figure 7 This is the ZSV data diagram of asphalt with different aging degrees in Test 1;
[0032] Figure 8 This is the relative zero shear viscosity change curve of asphalt with different aging degrees in Test 1;
[0033] Fig. 9 This is the S-shaped curve diagram of the CTI value fitting in Experiment 1;
[0034] Fig.10This is the S-shaped curve fitting of the recovery rate R value at 3.2KPa in Experiment 1. DETAILED DESCRIPTION
[0035] Specific implementation method 1: This implementation method is a method for characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology, which is specifically carried out in the following steps:
[0036] First, prepare SBS modified asphalt and the corresponding base asphalt, and then prepare samples of SBS modified asphalt and base asphalt for different aging times;
[0037] Second, the SBS modified asphalt samples with different aging times obtained in the first test were subjected to stress-strain tests at 4°C to obtain the corresponding stress-strain curves, analyze the curve line shape, extract characteristic parameters, define the comprehensive toughness index CTI (Comprehensive Toughness Index CTI), and calculate the CTI values of the SBS modified asphalt with different aging times; the calculation formula of the CTI is as follows:
[0038]
[0039] Where:
[0040] CTI is the comprehensive toughness index, which comprehensively reflects the energy absorption capacity, ductility and strength index of the material and is dimensionless;
[0041] T e is the toughness area in the stress-strain curve. The toughness area represents the area of the part of the stress-strain curve caused by the ductility of the material, and the unit is MPa; the curve integral T e Indicates the toughness and fracture resistance of the material;
[0042] ε B Fracture strain, the strain value corresponding to the material when it breaks, reflects the ductility of the material, dimensionless; obtained through the stress-strain curve;
[0043] σ max is the maximum stress, which refers to the maximum stress value that the material bears during the stretching process, σ max is Y and σ B The larger value in MPa; Y is the yield strength, σ B is the fracture strength; obtained through stress-strain curve;
[0044] 3. The SBS modified asphalt samples with different aging times obtained in the first test and the corresponding matrix asphalt were subjected to a multiple stress creep recovery test (MSCR) respectively. The loading process was cycled 10 times at 3.2 kPa, and each cycle included 1 s creep and 9 s recovery. The recovery rate R value of the SBS modified asphalt with different aging times and the recovery rate R value of the matrix asphalt were calculated. The recovery rate R value of the SBS modified asphalt with different aging times was subtracted from the recovery rate R value of the matrix asphalt to obtain the recovery rate R value of the SBS modified asphalt with different aging times after eliminating the mechanical error.
[0045] 4. Fitting the CTI values of the SBS modified asphalt with different aging times obtained in step 2 with an S-shaped curve to obtain two inflection points, which correspond to two CTI values C1 and C2, respectively, where C1<C2;
[0046] The recovery rate R value of the SBS modified asphalt at different aging times after eliminating the mechanical error obtained in step 3 is fitted with an S-shaped curve to obtain two inflection points, which correspond to two R values R1 and R2, respectively, where R1<R2;
[0047] The criterion for judging the high degree of polymer modification residue is: CTI>C2;
[0048] The judgment criteria for the medium degree of polymer modification residue are: C1<CTI≤C2 and R1<the recovery rate R value of SBS modified asphalt at different aging times after eliminating mechanical error≤R2. If the two conditions cannot be met at the same time, it is classified as a low degree of polymer modification residue.
[0049] Another criterion for judging the low degree of polymer modification residue is: CTI≤C1.
[0050] Specific embodiment 2: This embodiment is different from the specific embodiment 1 in that: the method for preparing SBS modified asphalt in step 1 is:
[0051] First, put the matrix asphalt into an oven and bake it to 135°C for use; weigh SBS and add it to the matrix asphalt, quickly stir it with a glass rod until the distribution of SBS in the asphalt is relatively uniform, and then put the sample into the oven for swelling for 15 minutes, and the temperature of this process is 135°C; after the swelling is completed, heat the asphalt to 180°C, and sink the head of the high-speed shearing machine into the asphalt, and adjust the head height so that the asphalt covers the upper surface of the head, and then start shearing at a rate of 5000r / min for 30min, during which time the asphalt is slowly stirred with a glass rod to fully shear the SBS; stir the sheared asphalt, sink the mixer blade into the asphalt at 180°C, and adjust the head height so that the asphalt covers the upper surface of the head; then stir at a rate of 500r / min for 1h, then add the stabilizer elemental sulfur, and continue to stir at a rate of 500r / min for 1h at 180°C to obtain SBS modified asphalt. The rest is the same as the specific implementation method one.
[0052] Specific implementation method 3: This implementation method is different from the specific implementation method 2 in that the base asphalt is 70# base asphalt or 90# base asphalt. Other aspects are the same as the specific implementation method 2.
[0053] Specific implementation method 4: This implementation method is different from the specific implementation method 2 in that the SBS described is a linear SBS 1301. The rest is the same as the specific implementation method 2.
[0054] Specific implementation method 5: This implementation method is different from specific implementation method 4 in that the SBS modified asphalt contains 5% SBS by mass. The rest is the same as specific implementation method 4.
[0055] Specific implementation method 6: This implementation method is different from the specific implementation method 2 in that the mass of the stabilizer elemental sulfur is 0.15% of the mass of the base asphalt. The rest is the same as the specific implementation method 2.
[0056] Specific implementation method 7: This implementation method is different from specific implementation method 2 in that: the method for preparing SBS modified asphalt samples for different aging times in step 1 is: placing the SBS modified asphalt in a thin film oven at 163°C for short-term aging for 5 hours; after aging, the asphalt is taken out and placed in a pressure aging instrument, the temperature is maintained at 100±0.5°C, the pressure is controlled at 2.1±0.1MPa, and long-term pressure aging is performed for different times, and the long-term pressure aging time is 10h, 20h, 30h and 40h respectively. The rest is the same as specific implementation method 2.
[0057] Specific embodiment 8: This embodiment differs from specific embodiment 1 in that the stress-strain test in step 2 is conducted using an asphalt ductility tester, with a tensile rate of 50 mm / min and a test temperature of 4° C. The rest is the same as the specific embodiment.
[0058] Specific implementation method 9: This implementation method is different from specific implementation method 8 in that: in step 2, the step of analyzing the curve line shape and extracting characteristic parameters includes: dividing the stress-strain curve into different regions: elastic deformation region, yield point, strain softening stage, cold drawing stage, strain hardening stage and fracture point. The rest is the same as specific implementation method 8.
[0059] Specific embodiment 10: This embodiment is different from specific embodiment 9 in that: the yield strength σ is extracted at the yield point Y and yield strain ε Y ; Extract the fracture strength σ at the fracture point B and the fracture strain ε B . The rest is the same as the ninth embodiment.
[0060] The present invention is verified by the following tests:
[0061] Test 1: This test is a method based on static mechanical mechanics-dynamic rheology to characterize the residual degree of polymer modification of SBS modified asphalt. It is carried out in the following steps:
[0062] 1. This test uses 70# base asphalt and SBS modified asphalt (ID) to make the performance of the aged SBS modified asphalt equivalent to that of the 70# base asphalt. SBS modified asphalt (ID) was prepared using 70# base asphalt, linear SBS1301 and stabilizer. The SBS modifier is YH-791H (SBS1301-1) modifier from Sinopec Hunan Chemical Co., Ltd. Commercially available elemental sulfur is added as a stabilizer to the SBS modified asphalt to achieve chemical cross-linking. In actual engineering applications, SBS modified asphalt usually contains a SBS content of 5% by mass. Therefore, in order to meet actual conditions, a SBS content of 5% by mass was still used in this test. SBS modified asphalt was prepared using a high-speed emulsifying shearing machine and a mechanical agitator. High-speed shearing can make SBS modification and swelling reach the optimal particle size, while mechanical stirring can ensure uniform dispersion and prevent segregation. The specific steps of the preparation process of SBS modified asphalt are as follows:
[0063] 1) First, place 70# matrix asphalt in an oven and bake it to 135°C for later use. Then, weigh a certain amount of matrix asphalt (700g) and keep the temperature at 135°C.
[0064] 2) Weigh a certain amount of SBS and add it to the prepared matrix asphalt. Stir it quickly with a glass rod until the SBS is evenly distributed in the asphalt. Then put the sample into an oven to swell for about 15 minutes. The temperature during this process is still around 135°C. The mass of SBS is 5% of the mass of the matrix asphalt.
[0065] 3) After the swelling is completed, the asphalt is heated to 180°C, and the head of the high-speed shearing machine is sunk into the asphalt, and the head height is adjusted so that the asphalt covers the upper surface of the head; then shearing is started at a rate of 5000r / min for 30min, during which the asphalt is slowly stirred with a glass rod to fully shear the SBS;
[0066] 4) Stirring the sheared asphalt, sinking the mixer blades into the asphalt at 180°C, and adjusting the head height so that the asphalt covers the upper surface of the head. Then stirring at a rate of 500r / min for 1h, and then adding a corresponding proportion of stabilizer elemental sulfur, and continuing to stir at 180°C at a rate of 500r / min for 1h to obtain SBS modified asphalt (O); the mass of the stabilizer elemental sulfur is 0.15% of the mass of the base asphalt;
[0067] 2. Preparation method of asphalt with different aging degrees: The SBS modified asphalt prepared above is placed in a thin film oven at 163°C for short-term aging for 5 hours (TFOT). After aging, the asphalt is collected and placed in a pressure aging instrument. The temperature is maintained at 100±0.5°C and the pressure is controlled at 2.1±0.1MPa. Long-term pressure aging PAV with gradient time is performed. The PAV aging time is set to 10h, 20h, 30h and 40h. The aged SBS modified asphalt samples are abbreviated as: TFOT, SBS10P, SBS20P, SBS 30P and SBS 40P, and the original sample (unaged SBS modified asphalt) is abbreviated as: O.
[0068] 3. The static mechanical mechanics test and analysis method specifically includes the following steps: using the SYD-4508G-1 asphalt ductility tester of Shanghai Changji Geological Instrument Co., Ltd., which is designed in accordance with the requirements of the industry standard NB / SH / T 0814 "Asphalt Material Force Ductility Test Method" of the People's Republic of China, and is suitable for determining the maximum tensile value and elongation deformation value at maximum tensile force of asphalt, modified asphalt and emulsified asphalt residues;
[0069] (1) With reference to the AASHTO T 300 specification, a force-ductility instrument was used, the test temperature was 4°C ± 0.5°C, the tensile speed was 5 cm / min (± 5.0%), and the low-temperature stress-strain curves of SBS modified asphalt and 70# base asphalt with different aging degrees were obtained;
[0070] (2) According to the polymer yield and fracture theory, the stress-strain curve is divided into different regions: elastic deformation region, yield point, strain softening stage, cold drawing stage, strain hardening stage and fracture point (e.g. Figure 1 );
[0071] (3) Extract the yield strength (σ) at the yield point Y) and yield strain (ε Y ); extract the fracture strength (σ B ) and fracture strain (ε B ); Curve integral T e Indicates the toughness and fracture resistance of the material;
[0072] (4) For the bimodal curve, the comprehensive toughness index (CTI) is defined and calculated as follows:
[0073]
[0074] Where:
[0075] CTI - Comprehensive Toughness Index, a comprehensive index of the energy absorption capacity, ductility and strength of the material, dimensionless;
[0076] T e ——Toughness area, which refers to the area of the stress-strain curve caused by the ductility of the material, MPa;
[0077] ε B ——Fracture strain, the strain value corresponding to the material when it breaks, reflects the ductility of the material, dimensionless;
[0078] σ max ——Maximum stress refers to the maximum stress value that the material withstands during the stretching process, σ max =max(σ Y , σ B )MPa.
[0079] Figure 1 The characteristic parameters extracted from the stress-strain curve are plotted. Figure 2 is the stress-strain curve of SBS modified asphalt under different aging degrees, Figure 3 The stress-strain curves of 70# matrix asphalt at different aging degrees.
[0080] The characteristic parameters of the corresponding stress-strain curves of SBS modified asphalt and base asphalt with different aging degrees are extracted, and the comprehensive toughness index CTI value is calculated as follows:
[0081] Table 1. Extraction and calculation results of bimodal curve parameters
[0082]
[0083] Note: SBS 40P has no double peaks, T e is 0, so CTI is 0; the matrix asphalt has no double peak curve, T e is 0, so CTI is 0.
[0084] It can be seen that with the increase of aging degree, the yield strength σ Y , yield strain ε Y , fracture strength σ B The overall trend is upward, but the distinction between the original sample (SBS O) and the short-term aged sample (SBS TFOT) of SBS modified asphalt is not high. e The overall trend is downward, and the distinction between the original sample and short-term aging is the same as above. Fracture strain ε B It decreases with the increase of aging degree. In order to describe the energy absorption capacity, ductility and strength index of SBS modified asphalt, the comprehensive toughness index CTI is defined, which includes the toughness area T e and the fracture strain ε B The product of , which combines the energy absorption capacity and ductility of the material, is normalized and divided by the maximum stress, ignoring the dependence on strength, which better reflects the toughness of the material and can fully and accurately reflect the toughness characteristics of the material. The CTI value change curve of SBS modified asphalt with different aging degrees is drawn as follows Figure 4 .Depend on Figure 4 It was found that the CTI values of the original asphalt (O) and short-term aged (TFOT) asphalt samples did not fluctuate much, which was reflected in the change of SBS. During the short-term aging process, SBS will be affected by high temperature, and some SBS will crack, but most of the SBS and cross-linked structures are not destroyed, and the unique toughness given to SBS modified asphalt by the polymer is still largely retained. After entering the long-term aging, it was observed that the CTI index of SBS10P was 4.788, which was 67.8% lower than that of the unaged SBS modified asphalt. This is because under long-term pressure aging, the polymer undergoes oxidation reaction to generate carbonyl and hydroxyl grade groups, the polymer body will degrade, and the cross-linked structure formed by SBS in the modified asphalt will be destroyed. These factors will significantly affect the superior performance of SBS modified asphalt, and the corresponding change in the index is a sharp decrease in the CTI index.
[0085] 4. The steady-state shear test analysis method specifically includes the following steps:
[0086] (1) According to EN 15325, the test temperature is 60°C and the shear frequency range is 10 -3 s -1 -10 3 s -1 Under the conditions, steady-state shear tests were carried out on SBS modified asphalt with different aging degrees and 70# base asphalt, and a curve with the abscissa being the shear rate and the ordinate being the viscosity was obtained.
[0087] (2) The Carreau model and the Cross model were used to fit the data curves obtained from the time-division aged SBS modified asphalt and 70# base asphalt, respectively, and the corresponding asphalt zero shear viscosity (ZSV) fitting curves were obtained as follows: Figure 5 and Figure 6 , zero shear viscosity data such as Figure 7 ;
[0088] The Cross model describes the stress-strain relationship of pseudo-plastic non-Newtonian fluid as follows:
[0089]
[0090] Where:
[0091] η——Asphalt viscosity, Pa·s;
[0092] η0——Viscosity in the first Newtonian region, i.e. zero shear viscosity ZSV, Pa·s;
[0093] η ∞ ——The viscosity in the second Newtonian region, i.e., the viscosity value when the shear rate is very large, Pa·s;
[0094] k is a material characteristic parameter with a time dimension, which affects the endpoint rate of the first Newtonian zone of the sample (i.e., the starting rate of non-Newtonian behavior). The reciprocal of the k value can be regarded as the transition shear rate of the sample from the first Newtonian zone platform to the shear thinning zone;
[0095] m——material characteristic parameter, time dimensionless. The larger the m value, the faster the sample viscosity decreases. When m=0, the sample is a Newtonian fluid.
[0096] Similar to the Cross model, the Carreau-Yasuda model is expressed as:
[0097]
[0098] Where:
[0099] η——Asphalt viscosity, Pa·s.
[0100] η0——Viscosity in the first Newtonian zone, that is, zero shear viscosity ZSV, Pa·s.
[0101] η ∞ ——Viscosity in the second Newtonian region, that is, the viscosity value when the shear rate is very large, Pa·s.
[0102] k is a material characteristic parameter that controls the shear rate at which the first Newtonian zone begins to decrease.
[0103] m——material characteristic parameter, time dimensionless. The larger the m value, the faster the sample viscosity decreases.
[0104] α——Controls the curvature of the turn from the first Newton zone to the shear thinning zone. When α=2, the formula is the Carreau model.
[0105] (3) Definition of relative zero shear viscosity (η r ) indicator, expressed as:
[0106]
[0107] Where:
[0108] η r ——Relative viscosity index of zero shear viscosity of SBS modified asphalt and base asphalt of the same grade;
[0109] η 0-SBS ——SBS modified asphalt ZSV, PA·s;
[0110] η 0-基质 ——Base asphalt ZSV, PA·s.
[0111] η r Data such as Figure 8 .
[0112] from Figure 7 By observing the ZSV data of the time-divided aged asphalt, it is found that with the increase of the aging degree, the ZSV value shows an upward trend. The overall ZSV of SBS modified asphalt is significantly greater than that of the base asphalt. Only focusing on the value of ZSV cannot determine the residual degree of polymer modification of SBS modified asphalt. Therefore, the relative viscosity index is used for analysis ( Figure 8 ), the index excludes the changes in the base asphalt caused by aging, and indicates the residual degree of the polymer modification effect at different aging stages. The larger the value, the more stable the chemical structure and cross-linking structure of the polymer in the SBS modified asphalt, and the lower the degree of damage; the lower the value, the weaker the unique modification effect of the polymer in the SBS modified asphalt. Figure 8 The curve showing the change of relative viscosity value with the aging stage. The trend of the curve is Figure 4 The change trend of the mechanical index CTI is very similar. At the SBS20P stage, the change of the value tends to be gentle, which may be due to the serious depolymerization and de-crosslinking behavior of the polymer.
[0113] 5. The multiple stress creep recovery (MSCR) test specifically includes the following steps:
[0114] (1) A multi-stress creep recovery (MSCR) test was conducted using a dynamic shear rheometer. Two stresses (0.1 kPa and 3.2 kPa) were used for the test. The loading process included 20 cycles (10 cycles at 0.1 kPa and 10 cycles at 3.2 kPa), and each cycle included 1 s of creep and 9 s of recovery (ASTM 2015c).
[0115] (2) According to the requirements of ASTM 2015c, the recovery rate R value and irreversible creep compliance Jnr of SBS modified asphalt with different aging degrees at 0.1 KPa and 3.2 KPa are calculated. The data are shown in Table 2.
[0116] Table 2 MSCR test results of asphalt at different aging degrees
[0117]
[0118] Since the elastic recovery of the matrix asphalt is almost zero, the measured recovery rate R value should come from the mechanical error. Therefore, the real recovery rate data is obtained by eliminating the mechanical error (subtraction) of the SBS modified asphalt recovery rate R value, as shown in Table 3, and then gray correlation analysis is performed.
[0119] Table 3 Recovery rate data of SBS modified asphalt after eliminating mechanical error
[0120]
[0121] 6. Grey correlation analysis specifically includes the following steps:
[0122] 1. Take CTI as the reference series and use the relative zero shear viscosity η r R and J obtained by removing mechanical errors from multiple asphalt creep experiments nr The indicators are used as comparative series for grey relational analysis;
[0123] 2. Make the data dimensionless. Since the purpose of this processing is to analyze the residual degree of SBS modification and compare it with the relevant data of unaged SBS modified asphalt, the initial value method is used for analysis;
[0124] 3. Calculate the grey correlation coefficient;
[0125] 4. Calculate the grey correlation degree. The calculation results are shown in Table 4.
[0126] Table 4 Correlation calculation results
[0127]
[0128] According to the correlation calculation results in Table 4, the gray correlation between the irrecoverable compliance parameter obtained by the MSCR test and the CTI value is 0.5764 and 0.5642, both below 0.6, indicating that its correlation with the low-temperature toughness parameter is very low. This parameter cannot be used as an identifiable indicator for determining the residual degree of polymer modification of SBS modified asphalt. r The grey correlation indexes of the recovery rate R value at 0.1KPa and 3.2KPa are 0.7287, 0.8184 and 0.8634 respectively, which show a strong correlation in numerical value. However, from the perspective of the difficulty of data acquisition, the acquisition of the relative zero shear viscosity index is relatively cumbersome and not suitable for engineering research. For this reason, the recovery rate R value at 3.2KPa with a higher grey correlation is selected as the identification index for determining the residual degree of polymer modification of SBS modified asphalt at the high temperature rheological mechanics level.
[0129] The CTI value (see Table 1) and the recovery rate R value at 3.2 KPa (see Table 3) were fitted with an S-shaped curve, as follows: Fig. 9 and Fig.10 As shown. Fig. 9 and Fig.10 It is concluded that the corresponding CTI values at the inflection points of the CTI fitting S-curve are 11.8 and 1.2 respectively; the corresponding values of the recovery rate R value at the inflection point of the fitting S-curve at 3.2KPa are 60% and 16.5% respectively. The inflection point of the S-curve represents the junction of the fast and slow changes in the value. By comparing the comprehensive toughness index CTI value and the recovery rate R value at 3.2KPa, since the gray correlation between the two is above 0.93 in the aging stage samples O, TFOT, 30P and 40P, the difference between the two is not obvious in these four stages, and only the CTI index is considered. The polymer modification residual degree (high) is divided as follows: CTI>11.8, corresponding to the O and TFOT vicinity in the aging stage; the polymer modification residual degree (medium): 1.2<CTI≤11.8 and 16.5%<3.2KPaR value≤60%, corresponding to the 10P and 20P vicinity in the aging stage, both of which must be met. If any of the conditions is not met, it is divided into the polymer modification residual degree (low); the polymer modification residual degree (low): CTI≤1.2, corresponding to the 30P and 40P vicinity in the aging stage.
[0130] The present invention adopts the grey correlation analysis method to analyze the correlation between the comprehensive toughness index CTI defined by the low temperature stress-strain curve and the relative zero shear viscosity defined by the steady-state shear test and the recovery rate and irrecoverable creep compliance parameters of the multiple stress repeated creep test (MSCR), and optimizes the identification index for determining the polymer modification residual performance of aged SBS modified asphalt. According to the index, the polymer modification residual is divided into three degrees. The invention provides a method for dividing the regeneration stage of SBS modified asphalt.
Claims
1. A method for characterizing the residual degree of polymer modification in SBS modified asphalt based on the cross-mechanical behavior of static mechanics-dynamic rheology, Features The method for characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanics-dynamic rheology is carried out in the following steps: First, prepare SBS modified asphalt and the corresponding base asphalt, and then prepare samples of SBS modified asphalt and base asphalt for different aging times; 2. The SBS modified asphalt samples with different aging times obtained in step 1 were subjected to stress-strain tests at 4°C to obtain corresponding stress-strain curves, analyze the curve line shape, extract characteristic parameters, define the comprehensive toughness index CTI, and calculate the CTI values of the SBS modified asphalt with different aging times; the calculation formula of the CTI is as follows: Where: CTI is the comprehensive toughness index, which comprehensively reflects the energy absorption capacity, ductility and strength index of the material and is dimensionless; T e is the toughness area in the stress-strain curve. The toughness area represents the area of the part of the stress-strain curve caused by the ductility of the material, and the unit is MPa; the curve integral T e Indicates the toughness and fracture resistance of the material; ε B Fracture strain, the strain value corresponding to the material when it breaks, reflects the ductility of the material, dimensionless; obtained through the stress-strain curve; σ max is the maximum stress, which refers to the maximum stress value that the material bears during the stretching process, σ max is Y and σ B The larger value in MPa; Y is the yield strength, σ B is the fracture strength; obtained through stress-strain curve; 3. Perform multiple stress creep recovery tests on the SBS modified asphalt samples with different aging times obtained in step 1 and the corresponding matrix asphalt, respectively. The loading process is cycled 10 times at 3.2 kPa, and each cycle includes 1 s creep and 9 s recovery. Calculate the recovery rate R value of the SBS modified asphalt with different aging times and the recovery rate R value of the matrix asphalt, and subtract the recovery rate R value of the matrix asphalt from the recovery rate R value of the SBS modified asphalt with different aging times to obtain the recovery rate R value of the SBS modified asphalt with different aging times after eliminating the mechanical error.
4. The CTI values of SBS modified asphalt with different aging times obtained in step 2 are fitted with an S-shaped curve to obtain two inflection points, which correspond to two CTI values C 1 and C 2 , where C 1 <C 2 ; The recovery rate R value of SBS modified asphalt with different aging time after eliminating mechanical error obtained in step 3 is fitted with an S-shaped curve to obtain two inflection points, which correspond to two R values R 1 and R 2 , where R 1 <R 2 ; The criterion for judging the high degree of polymer modification residue is: CTI>C 2 ; The judgment criteria for the moderate degree of polymer modification residue are: C 1 <CTI≤C 2 And R 1 <After eliminating mechanical error, the recovery rate R value of SBS modified asphalt at different aging times ≤ R 2 , if the two conditions cannot be met at the same time, it is classified as low degree of polymer modification residue; There is another criterion for judging the low degree of polymer modification residue: CTI≤C 1 .
2. According to claim 1, a method for characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology, Features The method for preparing SBS modified asphalt in step 1 is: First, put the base asphalt into an oven and bake it at 135°C for use; weigh SBS and add it to the base asphalt, quickly stir it with a glass rod until the distribution of SBS in the asphalt is relatively uniform, then put the sample into the oven for swelling for 15 minutes, and the temperature of this process is 135°C; after the swelling is completed, heat the asphalt to 180°C, sink the head of the high-speed shearing machine into the asphalt, and adjust the head height so that the asphalt covers the upper surface of the head, then start shearing at a rate of 5000r / min for 30min, during which time slowly stir the asphalt with a glass rod to fully shear the SBS; stir the sheared asphalt, sink the mixer blades into the asphalt at 180°C, and adjust the head height so that the asphalt covers the upper surface of the head; then stir at a rate of 500r / min for 1h, then add stabilizer elemental sulfur, and continue stirring at a rate of 500r / min for 1h at 180°C to obtain SBS modified asphalt.
3. A method for characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology according to claim 2, Features The matrix asphalt is 70# matrix asphalt or 90# matrix asphalt.
4. A method for characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology according to claim 2, Features The SBS is a linear SBS1301.
5. The method of characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology according to claim 2, Features SBS modified asphalt contains 5% SBS by mass.
6. A method for characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanics-dynamic rheology according to claim 2, Features The mass of the stabilizer elemental sulfur is 0.15% of the mass of the base asphalt.
7. The method of characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology according to claim 1, Features The method for preparing SBS modified asphalt samples for different aging times in step one is: placing the SBS modified asphalt in a thin film oven at 163°C for short-term aging for 5 hours; after aging, taking out the asphalt and placing it in a pressure aging instrument, maintaining the temperature at 100±0.5°C, and controlling the pressure at 2.1±0.1MPa, and performing long-term pressure aging for different times, and the long-term pressure aging times are 10h, 20h, 30h and 40h, respectively.
8. The method of characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology according to claim 1, Features The stress-strain test described in step 2 is carried out using an asphalt ductility tester with a tensile rate of 50 mm / min and a test temperature of 4°C.
9. The method of characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology according to claim 1, Features The step of analyzing the curve line shape and extracting characteristic parameters in step 2 includes: dividing the stress-strain curve into different regions: elastic deformation region, yield point, strain softening stage, cold drawing stage, strain hardening stage and fracture point.
10. A method for characterizing the residual degree of polymer modification of SBS modified asphalt based on the cross-mechanical behavior of static mechanical mechanics-dynamic rheology according to claim 9, Features Extract the yield strength σ at the yield point Y and yield strain ε Y ; Extract the fracture strength σ at the fracture point B and fracture strain ε B .