Double-doped positive electrode active material, aqueous solution sodium ion battery and electronic device
By using the double-doped positive electrode active material Na3V2-x-yAlxFey(PO4)3 of Al and Fe double-doped sodium vanadium phosphate in aqueous sodium ion batteries, the Na-Zn ions in Zn‖Na3V2(PO4)3 battery is solved by using Na-Zn ions in Zn‖Na3V2(PO4)3 battery with double-doped sodium vanadium phosphate in aqueous sodium ion batteries. The problem of co-embedding reactions improves the cycle stability and voltage retention rate of the battery, achieving higher energy density and commercialization prospects.
Patent Information
- Application Number
- CN202410938752.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-14
- Publication Date
- 2024-11-05
AI Technical Summary
The co-embedding reaction of Na-Zn ions in the existing Zn‖Na3V2(PO4)3 aqueous sodium ion battery leads to irreversible generation of Zn3(PO4)2(H2O)4, resulting in a significant attenuation of battery performance, and the energy density of traditional aqueous sodium ion battery Far less than lithium-ion batteries and sodium-ion batteries.
Using Al and Fe double-doped positive electrode active material Na3V2-x-yAlxFey(PO4)3, the aqueous sodium ion battery is combined with aqueous sodium ion battery. The design includes specific electrolyte and diaphragm combinations.
It significantly improves the working life and power output stability of aqueous sodium ion batteries, has better cycle stability and higher voltage retention rate, broadens the application field and has good commercial prospects.
Smart Images

Figure CN118899387A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrochemical energy storage, and in particular to a dual-doped positive electrode active material, an aqueous sodium ion battery and an electronic device. Background Art
[0002] Guided by the energy revolution and the dual-carbon strategic goals, State Grid Corporation of China continues to give priority to, vigorously and orderly develop renewable energy power generation technologies with solar energy and wind energy as the main body. However, new energy sources such as wind and solar power have the characteristics of intermittency, randomness and volatility. With their large-scale and high-proportion access, their consumption in the power grid has become a problem that needs to be solved urgently. Energy storage technology, as an important regulatory resource for the new power system, is an important support for building a coordinated interactive ecology of source-grid-load-storage. New energy storage represented by electrochemical energy storage has the characteristics of precise control, rapid response and flexible layout, and has become the leader in the new energy storage installation of the current power system. The energy storage system has a large installed capacity, which puts forward high requirements on the reliability, safety and economy of electrochemical energy storage technology. The lithium-ion batteries and sodium-ion batteries currently developed all use organic solvents as electrolytes, which have great safety hazards. Recently, dozens of fire accidents in energy storage power stations in South Korea and fire and explosion accidents in energy storage power stations in Fengtai District, Beijing have continuously warned the large-scale application of electrochemical energy storage technology.
[0003] Aqueous sodium ion batteries have the advantages of good safety, high theoretical specific capacity, and low cost, and are expected to meet the requirements of large-scale energy storage systems. However, traditional aqueous sodium ion batteries use inorganic hosts that can intercalate and deintercalate sodium ions as positive and negative electrode materials. Their rigid structure limits the amount of sodium ions that can be intercalated and deintercalated. In addition, the electrochemical window of aqueous sodium ion batteries is narrow, making the energy density of aqueous sodium ion batteries far less than that of lithium ion batteries and sodium ion batteries. The Zn negative electrode can undergo redox reactions in aqueous sodium ion batteries, and its theoretical specific capacity is high. Aqueous sodium ion batteries based on Zn negative electrodes are expected to further improve their energy density. Vanadium-based polyanion materials represented by Na3V2(PO4)3 have a stable open large framework structure. Aqueous sodium ion batteries with Zn‖Na3V2(PO4)3 as the positive electrode and Zn as the negative electrode should theoretically have a high operating voltage and a long cycle life. In our recent research, we found that the co-intercalation reaction of Na-Zn ions occurred in the sodium ion battery of Zn‖Na3V2(PO4)3 aqueous solution, resulting in the irreversible formation of Zn3(PO4)2(H2O)4 and a significant degradation of battery performance.
[0004] In view of the technical defects of the current Zn‖Na3V2(PO4)3 aqueous solution sodium ion battery, it is necessary to improve it. Summary of the invention
[0005] In order to solve the problems in the above-mentioned prior art, the present invention provides a dual-doped positive electrode active material of Al and Fe dual-doped sodium vanadium phosphate. Compared with the existing sodium vanadium phosphate and other vanadium-based polyanion compound positive electrode materials, it not only has better cycle stability but also has higher voltage retention rate. The aqueous solution sodium ion battery based on the dual-doped positive electrode active material has a long working life and stable power output.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides a dual-doped positive electrode active material, the chemical formula of the dual-doped positive electrode active material is Na3V 2-x-y Al x Fe y (PO4)3,0 <x≤0.3,0<y≤0.3。
[0007] An aqueous sodium ion battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises the dual-doped positive electrode active material.
[0008] Further, the solvent of the electrolyte is water, and the solute of the electrolyte includes sodium salt and zinc salt, that is, the electrolyte is an aqueous solution containing sodium salt and zinc salt;
[0009] The sodium salt includes one or more of sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium perchlorate, sodium sulfate, sodium nitrate, sodium phosphate, sodium carbonate, and sodium oxalate;
[0010] The zinc salt includes one or more of zinc nitrate, zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate, zinc bis(trifluoromethylsulfonyl)imide, zinc p-hydroxybenzenesulfonate, and zinc perfluoro-2-ethoxyethanesulfonate.
[0011] Furthermore, the diaphragm includes one of non-woven fabric, glass fiber or porous PP / PE diaphragm.
[0012] Furthermore, the positive electrode further comprises a positive electrode current collector, a positive electrode conductive agent and a positive electrode adhesive, and the dual-doped positive electrode active material, the positive electrode conductive agent and the positive electrode adhesive are mixed and bonded to the positive electrode current collector to form the positive electrode;
[0013] The negative electrode comprises a negative electrode active material, a negative electrode current collector, a negative electrode conductive agent and a negative electrode adhesive. The negative electrode active material, the negative electrode conductive agent and the negative electrode adhesive are mixed and bonded to the negative electrode current collector to form the negative electrode.
[0014] Furthermore, the mass ratio of the dual-doped positive electrode active material, the positive electrode conductive agent, and the positive electrode binder is (7-9.5): (0.3-2): (0.2-1);
[0015] The mass ratio of the negative electrode active material, the negative electrode conductive agent and the negative electrode binder is (7-9.5): (0.3-2): (0.2-1).
[0016] Furthermore, the positive electrode conductive agent includes one or more of graphite, carbon black, carbon nanotubes, and graphene;
[0017] The negative electrode conductive agent includes one or more of graphite, carbon black, carbon nanotubes, and graphene.
[0018] Furthermore, the positive electrode binder includes one or more of polytetrafluoroethylene, polyacrylic acid, sodium alginate, polyvinyl alcohol, sodium carboxymethyl cellulose, and styrene-butadiene latex;
[0019] The negative electrode binder includes one or more of polytetrafluoroethylene, polyacrylic acid, sodium alginate, polyvinyl alcohol, sodium carboxymethyl cellulose, and styrene-butadiene latex.
[0020] Further, the positive electrode current collector comprises one of a foil or mesh of titanium, copper, stainless steel, or nickel;
[0021] The negative electrode current collector includes one of a foil or a mesh of titanium, copper, stainless steel, and nickel.
[0022] An electronic device comprises the aqueous sodium ion battery.
[0023] The beneficial effects of the present invention are:
[0024] 1. The chemical formula of the dual-doped positive electrode active material of the present invention is Na3V 2-x-y Al x Fe y (PO4)3, which is Al and Fe doped sodium vanadium phosphate, which has better cycle stability and higher voltage retention rate than existing sodium vanadium phosphate and other vanadium-based polyanion compound positive electrode materials;
[0025] 2. The present invention uses a dual-doped vanadium-based polyanion compound Na3V 2-x-y Al x Fe y (PO4)3 is used in aqueous sodium ion batteries, broadening its application areas;
[0026] 3. The aqueous sodium ion battery of the present invention has the characteristics of long service life and stable power output, and has good commercial prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The dual-doped positive electrode active material Na3V prepared in Example 1 of the present invention 1.4 Al 0.3 Fe 0.3XRD pattern of (PO4)3;
[0028] Figure 2 The aqueous sodium ion battery Zn||Na3V prepared in Example 1 of the present invention 1.4 Al 0.3 Fe 0.3 The charge and discharge curve of (PO4)3;
[0029] Figure 3 The dual-doped positive electrode active material Na3V prepared in Example 2 of the present invention 1.8 Al 0.1 Fe 0.1 XRD pattern of (PO4)3 after 200 charge and discharge cycles;
[0030] Figure 4 The aqueous sodium ion battery Zn||Na3V prepared in Example 2 of the present invention 1.8 Al 0.1 Fe 0.1 Cycling curve of (PO4)3 at 5C current density.
[0031] Figure 5 It is a charge and discharge curve diagram of the aqueous sodium ion battery Zn|Na3V2(PO4)3 prepared in Comparative Example 1 of the present invention;
[0032] Figure 6 This is the XRD diagram of the positive electrode active material Na3V2(PO4)3 prepared in Comparative Example 1 of the present invention after 200 cycles of charge and discharge;
[0033] Figure 7 The aqueous sodium ion battery Zn||Na3V prepared in Comparative Example 2 of the present invention 1.7 Al 0.3 The charge and discharge curve of (PO4)3;
[0034] Figure 8 The positive electrode active material Na3V prepared in Comparative Example 2 of the present invention 1.7 Al 0.3 XRD pattern of (PO4)3 after 200 charge and discharge cycles;
[0035] Fig. 9 The aqueous sodium ion battery Zn|Na3V prepared in Comparative Example 3 of the present invention 1.7 Fe 0.3 The charge and discharge curve of (PO4)3;
[0036] Fig.10 The positive electrode active material Na3V prepared in Comparative Example 3 of the present invention 1.7 Fe 0.3XRD pattern of (PO4)3 after 200 charge and discharge cycles. DETAILED DESCRIPTION
[0037] In order to clearly illustrate the technical features of this solution, this solution is described below through a specific implementation method.
[0038] The embodiment of the present invention provides a dual-doped positive electrode active material, the chemical formula of the dual-doped positive electrode active material is Na3V 2-x-y Al x Fe y (PO4)3,0 <x≤0.3,0<y≤0.3。
[0039] Based on the same inventive concept, the present invention also provides an aqueous sodium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, and in addition also comprising a shell, wherein the positive electrode comprises the above-mentioned dual-doped positive electrode active material.
[0040] The positive electrode also includes a positive electrode current collector, a positive electrode conductive agent and a positive electrode adhesive. The dual-doped positive electrode active material, the positive electrode conductive agent and the positive electrode adhesive are mixed and bonded to the positive electrode current collector to form a positive electrode.
[0041] The negative electrode includes a negative electrode active material, a negative electrode current collector, a negative electrode conductor and a negative electrode binder. The negative electrode active material, the negative electrode conductor and the negative electrode binder are mixed and bonded to the negative electrode current collector to form the negative electrode. Preferably, the negative electrode active material includes zinc or a zinc alloy.
[0042] The separator includes one of non-woven fabric, glass fiber or porous PP / PE separator.
[0043] The solvent of the electrolyte is water, and the solute of the electrolyte includes sodium salt and zinc salt;
[0044] Sodium salts include one or more of sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium perchlorate, sodium sulfate, sodium nitrate, sodium phosphate, sodium carbonate, and sodium oxalate;
[0045] The zinc salt includes one or more of zinc nitrate, zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate, zinc bis(trifluoromethylsulfonyl)imide, zinc p-hydroxybenzenesulfonate, and zinc perfluoro-2-ethoxyethanesulfonate.
[0046] The positive electrode conductive agent and the negative electrode conductive agent both include one or more of graphite, carbon black, carbon nanotubes, and graphene;
[0047] The positive electrode adhesive and the negative electrode adhesive both include one or more of polytetrafluoroethylene, polyacrylic acid, sodium alginate, polyvinyl alcohol, sodium carboxymethyl cellulose, and styrene-butadiene latex;
[0048] The positive electrode current collector and the negative electrode current collector both include one of the foils or meshes of titanium, copper, stainless steel, and nickel;
[0049] The mass ratio of the dual-doped positive electrode active material, the positive electrode conductive agent, and the positive electrode binder is (7-9.5): (0.3-2): (0.2-1);
[0050] The mass ratio of the negative electrode active material, the negative electrode conductive agent and the negative electrode binder is (7-9.5): (0.3-2): (0.2-1).
[0051] Based on the same inventive concept, the present invention also provides an electronic device, including the above-mentioned aqueous sodium ion battery. Specifically, the electronic device can be an electronic device that uses an aqueous sodium ion battery as an operating power source to perform various functions; the electronic device can also be an electronic terminal device such as a communication base station, a car starter, and a rural energy storage power supply; the electronic device can also be an electric tool that uses an aqueous sodium ion battery as a driving power source to move parts; the electronic device also includes an electric vehicle that relies on an aqueous sodium ion battery as a driving power source, and can be a car equipped with other driving sources in addition to the aqueous sodium ion battery.
[0052] The following describes the dual-doped Na3V 2-x-y Al x Fe y Superiority of (PO4)3 cathode and its application in aqueous sodium-ion batteries.
[0053] Comparative Example 1
[0054] A positive electrode active material, whose chemical formula is Na3V2(PO4)3, and the preparation method of the positive electrode active material is:
[0055] NaH2PO4, V2O5 and citric acid are used as raw materials; among them, NaH2PO4 is both a sodium source and a phosphorus source, V2O5 is a vanadium source, and citric acid is a carbon source.
[0056] 4.6803 g NaH2PO4·2H2O, 3.6376 g V2O5, and 1.0507 g citric acid monohydrate were added to 200 mL water, dispersed under magnetic stirring for 0.5 h to form a suspension, the suspension was transferred to a sand mill and ground for 3 h, and then spray-dried at an air inlet rate of 80%, an air inlet temperature of 180° C., and a feed rate of 0.5% to obtain a precursor;
[0057] Then the above precursor is placed in an argon atmosphere and calcined at 750°C for 6 hours to obtain Na3V2(PO4)3.
[0058] Furthermore, an aqueous sodium ion battery is provided, comprising:
[0059] Positive electrode, the preparation method of the positive electrode is as follows: weigh Na3V2(PO4)3 positive electrode active material, positive electrode conductive agent, and positive electrode binder in a weight ratio of 80:10:10, wherein the positive electrode conductive agent is conductive carbon black SP, and the positive electrode binder is 60% by weight PTFE emulsion; firstly grind the Na3V2(PO4)3 positive electrode active material and conductive carbon black SP in an agate mortar evenly to obtain a powder material for standby use; then take the positive electrode binder PTFE emulsion and put it in a beaker, add isopropyl alcohol to break the emulsion, then add the ground powder material, slurry mix and dry under an infrared lamp, and finally roll it into a film on a double-roller machine, put the film into a vacuum oven at 100°C for more than 6 hours, and press it on a stainless steel mesh to obtain the positive electrode;
[0060] Negative electrode: use zinc sheet as negative electrode. Take zinc sheet with thickness of 0.1-1mm, polish it with sandpaper, rinse it with ethanol, dry it, cut it and set it aside.
[0061] Electrolyte, electrolyte is 10 mol·L -1 of sodium bis(fluorosulfonyl)imide aqueous solution and 2 mol·L -1 A mixed solution of ZnSO4 aqueous solution.
[0062] Diaphragm, the diaphragm is glass fiber.
[0063] The positive electrode, the negative electrode, the electrolyte and the separator are assembled into an aqueous sodium ion battery.
[0064] Comparative Example 2
[0065] A positive electrode active material with the chemical formula Na3V 1.7 Al 0.3 (PO4)3, the preparation method of the positive electrode active material is:
[0066] NaH2PO4, V2O5, Al(NO3)3 and citric acid are used as raw materials; among them, NaH2PO4 is both a sodium source and a phosphorus source, V2O5 is a vanadium source, Al(NO3)3 is an aluminum source, and citric acid is a carbon source.
[0067] 4.6803 g NaH2PO4·2H2O, 3.0920 g V2O5, 0.639 g Al(NO3)3, and 1.0507 g citric acid monohydrate were added to 200 mL water, dispersed under magnetic stirring for 0.5 h to form a suspension, the suspension was transferred to a sand mill and ground for 3 h, and then spray-dried at an air inlet rate of 80%, an air inlet temperature of 180°C, and a feed rate of 0.5% to obtain a precursor;
[0068] Then the precursor was placed in an argon atmosphere and calcined at 750 °C for 6 h to obtain Na3V 1.7 Al 0.3 (PO4)3.
[0069] Furthermore, an aqueous sodium ion battery is provided, comprising:
[0070] The positive electrode is prepared by weighing Na3V 1.7 Al 0.3 (PO4)3 positive electrode active material, positive electrode conductive agent, positive electrode binder, wherein the positive electrode conductive agent is carbon nanotubes, and the positive electrode binder is sodium alginate; firstly, Na3V 1.7 Al 0.3 The (PO4)3 positive electrode active material and carbon nanotubes are evenly ground in an agate mortar to obtain a powder material for later use; then the positive electrode binder sodium alginate is slurried, dried, and finally rolled into a film on a double-roller machine, and the film is placed in a vacuum oven at 100°C for more than 6 hours and pressed on a stainless steel mesh to obtain a positive electrode;
[0071] Negative electrode: use zinc sheet as negative electrode. Take zinc sheet with thickness of 0.1-1mm, polish it with sandpaper, rinse it with ethanol, dry it, cut it and set it aside.
[0072] Electrolyte, electrolyte is 5 mol·L -1 Sodium perchlorate aqueous solution and 2 mol·L -1 A mixed solution of an aqueous solution of zinc trifluoromethanesulfonate.
[0073] Diaphragm, the diaphragm is non-woven fiber.
[0074] The positive electrode, the negative electrode, the electrolyte and the separator are assembled into an aqueous sodium ion battery.
[0075] Comparative Example 3
[0076] A positive electrode active material with the chemical formula Na3V 1.7 Fe 0.3 (PO4)3, the preparation method of the positive electrode active material is:
[0077] NaH2PO4, V2O5, Fe(NO3)3 and citric acid are used as raw materials; among them, NaH2PO4 is both a sodium source and a phosphorus source, V2O5 is a vanadium source, Fe(NO3)3 is an iron source, and citric acid is a carbon source.
[0078] 4.6803 g NaH2PO4·2H2O, 3.0920 g V2O5, 0.7256 g Fe(NO3)3, and 1.0507 g citric acid monohydrate were added to 200 mL water, dispersed for 0.5 h under magnetic stirring to form a suspension, the suspension was transferred to a sand mill and ground for 3 h, and then spray-dried at an air inlet rate of 80%, an air inlet temperature of 180°C, and a feed rate of 0.5% to obtain a precursor;
[0079] Then the precursor was placed in an argon atmosphere and calcined at 750 °C for 6 h to obtain Na3V 1.7 Fe 0.3 (PO4)3.
[0080] Furthermore, an aqueous sodium ion battery is provided, comprising:
[0081] The positive electrode is prepared by weighing Na3V 1.7 Fe 0.3 (PO4)3 positive electrode active material, positive electrode conductive agent, positive electrode binder, wherein the positive electrode conductive agent is graphite, and the positive electrode binder is polyacrylic acid; firstly, Na3V 1.7 Fe 0.3 The (PO4)3 positive electrode active material and graphite are evenly ground in an agate mortar to obtain a powder material for later use; then the positive electrode binder polyacrylic acid is slurried, dried, and finally rolled into a film on a double-roller machine, and the film is placed in a vacuum oven at 100°C for more than 6 hours and pressed on a copper mesh to obtain a positive electrode;
[0082] For the negative electrode, a zinc-indium alloy sheet is used as the negative electrode. A 0.1-1 mm thick alloy sheet is taken, polished with sandpaper, rinsed with ethanol, dried, cut and set aside;
[0083] Electrolyte, electrolyte is 10 mol·L -1 bis(trifluoromethanesulfonyl)imide aqueous solution and 2 mol·L -1 A mixed solution of an aqueous solution of zinc p-hydroxybenzenesulfonate.
[0084] Diaphragm: the diaphragm is a porous PP / PE film.
[0085] The positive electrode, the negative electrode, the electrolyte and the separator are assembled into an aqueous sodium ion battery.
[0086] Example 1
[0087] A dual-doped positive electrode active material with the chemical formula Na3V 1.4 Al 0.3 Fe 0.3 (PO4)3, the preparation method of the positive electrode active material is:
[0088] NaH2PO4, V2O5, Al(NO3)3, Fe(NO3)3 and citric acid are used as raw materials; among them, NaH2PO4 is both a sodium source and a phosphorus source, V2O5 is a vanadium source, Al(NO3)3 is an aluminum source, Fe(NO3)3 is an iron source, and citric acid is a carbon source.
[0089] 4.6803 g NaH2PO4·2H2O, 2.5463 g V2O5, 0.639 g Al(NO3)3, 0.7256 g Fe(NO3)3, and 1.0507 g citric acid monohydrate were added to 200 mL of water, dispersed for 0.5 h under magnetic stirring to form a suspension, the suspension was transferred to a sand mill and ground for 3 h, and then spray-dried at an air inlet rate of 80%, an air inlet temperature of 180°C, and a feed rate of 0.5% to obtain a precursor;
[0090] Then the precursor was placed in an argon atmosphere and calcined at 750 °C for 6 h to obtain Na3V 1.4 Al 0.3 Fe 0.3 (PO4)3.
[0091] Furthermore, an aqueous sodium ion battery is provided, comprising:
[0092] The positive electrode is prepared by weighing Na3V 1.4 Al 0.3 Fe 0.3 (PO4)3 dual-doped positive electrode active material, positive electrode conductive agent, positive electrode binder, wherein the positive electrode conductive agent is graphene, and the positive electrode binder is polyvinyl alcohol; firstly, Na3V 1.4 Al 0.3 Fe 0.3 The (PO4)3 dual-doped positive electrode active material and graphene are evenly ground in an agate mortar to obtain a powder material for later use; then the positive electrode binder polyvinyl alcohol is slurried, dried, and finally rolled into a film on a double-roller machine, and the film is placed in a vacuum oven at 100°C for more than 6 hours, and pressed on a stainless steel mesh to obtain a positive electrode;
[0093] For the negative electrode, a zinc-tin alloy sheet is used as the negative electrode. A 0.1-1 mm thick alloy sheet is taken, polished with sandpaper, rinsed with ethanol, dried, cut and set aside;
[0094] Electrolyte, electrolyte is 2 mol·L -1 of sodium sulfate aqueous solution and 4 mol·L -1 A mixed solution of an aqueous solution of zinc bis(trifluoromethylsulfonyl)imide.
[0095] Diaphragm: the diaphragm is a glass fiber membrane.
[0096] The positive electrode, the negative electrode, the electrolyte and the separator are assembled into an aqueous sodium ion battery.
[0097] Example 2
[0098] A dual-doped positive electrode active material with the chemical formula Na3V 1.8 Al 0.1 Fe 0.1 (PO4)3, the preparation method of the positive electrode active material is:
[0099] NaH2PO4, V2O5, Al(NO3)3, Fe(NO3)3 and citric acid are used as raw materials; among them, NaH2PO4 is both a sodium source and a phosphorus source, V2O5 is a vanadium source, Al(NO3)3 is an aluminum source, Fe(NO3)3 is an iron source, and citric acid is a carbon source.
[0100] 4.6803 g NaH2PO4·2H2O, 3.2738 g V2O5, 0.213 g Al(NO3)3, 0.2419 g Fe(NO3)3, and 1.0507 g citric acid monohydrate were added to 200 mL water, dispersed for 0.5 h under magnetic stirring to form a suspension, the suspension was transferred to a sand mill and ground for 3 h, and then spray-dried at an air inlet rate of 80%, an air inlet temperature of 180°C, and a feed rate of 0.5% to obtain a precursor;
[0101] Then the precursor was placed in an argon atmosphere and calcined at 750 °C for 6 h to obtain Na3V 1.8 Al 0.1 Fe 0.1 (PO4)3.
[0102] Furthermore, an aqueous sodium ion battery is provided, comprising:
[0103] The positive electrode is prepared by weighing Na3V 1.8 Al 0.1 Fe 0.1 (PO4)3 dual-doped positive electrode active material, positive electrode conductive agent, positive electrode binder, wherein the positive electrode conductive agent is carbon black, and the positive electrode binder is sodium carboxymethyl cellulose; firstly, Na3V 1.8 Al 0.1 Fe 0.1 The (PO4)3 dual-doped positive electrode active material and carbon black are evenly ground in an agate mortar to obtain a powder material for later use; then the positive electrode binder sodium carboxymethyl cellulose is slurried, dried, and finally rolled into a film on a double-roller machine, and the film is placed in a vacuum oven at 100°C for more than 6 hours and pressed on a titanium mesh to obtain a positive electrode;
[0104] For the negative electrode, a zinc-titanium alloy sheet is used as the negative electrode. A 0.1-1 mm thick alloy sheet is taken, polished with sandpaper, rinsed with ethanol, dried, cut and set aside;
[0105] Electrolyte, electrolyte is 1 mol·L -1 of sodium oxalate aqueous solution and 6 mol·L -1 A mixed solution of an aqueous solution of zinc perfluoro 2-ethoxyethane sulfonate.
[0106] Diaphragm: the diaphragm is a non-woven fiber membrane.
[0107] The positive electrode, the negative electrode, the electrolyte and the separator are assembled into an aqueous sodium ion battery.
[0108] Performance Testing
[0109] The charge and discharge curves of the aqueous sodium ion battery prepared in Comparative Example 1 and the XRD pattern of the positive electrode active material Na3V2(PO4)3 after 200 cycles of charge and discharge were tested. The results are as follows: Figure 5 , Figure 6 As shown, from Figures 5-6 It can be seen that after 200 cycles, the average discharge voltage of the mixed ion battery Zn‖Na3V2(PO4)3 increased from 1.37V (relative to Zn 2+ / Zn) dropped to 0.88V, and the capacity retention rate was only 52.0%; the characteristic peak belonging to Na3V2(PO4)3 gradually weakened, and a new phase of Zn3(PO4)2(H2O)4 appeared.
[0110] The aqueous sodium ion battery Zn|Na3V prepared in Comparative Example 2 was tested. 1.7 Al 0.3 The charge and discharge curves of (PO4)3 and the positive electrode active material Na3V after 200 charge and discharge cycles 1.7 Al 0.3 The XRD pattern of (PO4)3 is as follows Figure 7 , Figure 8 As shown, from Figures 7-8 It can be seen that after 200 cycles, the mixed ion battery Zn‖Na3V 1.7 Al 0.3 The average discharge voltage of (PO4)3 remained unchanged, and the capacity retention rate was 73%; it belongs to Na3V 1.7 Al 0.3 The characteristic peaks of (PO4)3 (same as Na3V2(PO4)3) can be well retained, but a small amount of new phase of Zn3(PO4)2(H2O)4 still appears.
[0111] The aqueous sodium ion battery Zn|Na3V prepared in Comparative Example 3 was tested. 1.7 Fe0.3 The charge and discharge curves of (PO4)3 and the positive electrode active material Na3V after 200 charge and discharge cycles 1.7 Fe 0.3 The XRD pattern of (PO4)3 is as follows Fig. 9 , Fig.10 As shown, from Figures 9-10 It can be seen that after 200 cycles, the mixed ion battery Zn‖Na3V 1.7 Fe 0.3 The average discharge voltage retention rate of (PO4)3 is lower than that of Zn‖Na3V 1.7 Al 0.3 (PO4)3, but better than Zn‖Na3V2(PO4)3; belongs to Na3V 1.7 Fe 0.3 The characteristic peaks of (PO4)3 (same as Na3V2(PO4)3) still exist, but a large number of new phases of Zn3(PO4)2(H2O)4 still appear.
[0112] The positive electrode active material Na3V prepared in Example 1 was tested 1.4 Al 0.3 Fe 0.3 XRD of (PO4)3 and aqueous sodium ion battery Zn‖Na3V 1.4 Al 0.3 Fe 0.3 (PO4)3 charge and discharge curve, the results are as follows Figure 1 , Figure 2 As shown, from Figures 1-2 It can be seen that Al-Fe doped Na3V 1.4 Al 0.3 Fe 0.3 The structure of (PO4)3 and Na3V2(PO4)3, Na3V 1.7 Al 0.3 (PO4)3 and Na3V 1.7 Fe 0.3 (PO4)3 is consistent. After 200 cycles, the mixed ion battery Zn‖Na3V 1.4 Al 0.3 Fe 0.3 The average discharge voltage of (PO4)3 remained unchanged, and the capacity retention rate was 77%.
[0113] The aqueous sodium ion battery Zn||Na3V prepared in Test Example 2 1.8 Al 0.1 Fe 0.1 After 200 cycles of charge and discharge of (PO4)3, the positive electrode active material Na3V 1.8 Al 0.1 Fe 0.1The XRD pattern of (PO4)3 and the long-term cycle diagram of the battery are shown in the following figure. Figure 3 , Figure 4 As shown, from Figures 3-4 It can be seen that after 200 cycles, it belongs to Na3V 1.8 Al 0.1 Fe 0.1 The characteristic peaks of (PO4)3 (same as Na3V2(PO4)3) are well preserved, and no new phase appears; Zn‖Na3V 1.8 Al 0.1 Fe 0.1 The (PO4)3 hybrid ion battery has an initial energy density of 138.4Wh / kg at a current density of 5C, and an energy retention rate of 50% after 1000 cycles.
[0114] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A dual-doped positive electrode active material, characterized in that: The chemical formula of the dual-doped positive electrode active material is Na3V 2-x-y Al x Fe y (PO4)3,0 <x≤0.3,0<y≤0.3。 2. An aqueous sodium ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises the dual-doped positive electrode active material according to claim 1.
3. The aqueous sodium ion battery according to claim 2, characterized in that: The solvent of the electrolyte is water, and the solute of the electrolyte includes sodium salt and zinc salt; The sodium salt includes one or more of sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium perchlorate, sodium sulfate, sodium nitrate, sodium phosphate, sodium carbonate, and sodium oxalate; The zinc salt includes one or more of zinc nitrate, zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate, zinc bis(trifluoromethylsulfonyl)imide, zinc p-hydroxybenzenesulfonate, and zinc perfluoro-2-ethoxyethanesulfonate.
4. The aqueous sodium ion battery according to claim 2, characterized in that: The separator includes one of non-woven fabric, glass fiber or porous PP / PE separator.
5. The aqueous sodium ion battery according to claim 2, characterized in that: The positive electrode further comprises a positive electrode current collector, a positive electrode conductive agent and a positive electrode adhesive. The dual-doped positive electrode active material, the positive electrode conductive agent and the positive electrode adhesive are mixed and bonded to the positive electrode current collector to form the positive electrode. The negative electrode comprises a negative electrode active material, a negative electrode current collector, a negative electrode conductive agent and a negative electrode adhesive. The negative electrode active material, the negative electrode conductive agent and the negative electrode adhesive are mixed and bonded to the negative electrode current collector to form the negative electrode.
6. The aqueous sodium ion battery according to claim 5, characterized in that: The mass ratio of the dual-doped positive electrode active material, the positive electrode conductive agent, and the positive electrode binder is (7-9.5): (0.3-2): (0.2-1); The mass ratio of the negative electrode active material, the negative electrode conductive agent and the negative electrode binder is (7-9.5): (0.3-2): (0.2-1).
7. The aqueous sodium ion battery according to claim 5, characterized in that: The positive electrode conductive agent includes one or more of graphite, carbon black, carbon nanotubes, and graphene; The negative electrode conductive agent includes one or more of graphite, carbon black, carbon nanotubes, and graphene.
8. The aqueous sodium ion battery according to claim 5, characterized in that: The positive electrode binder includes one or more of polytetrafluoroethylene, polyacrylic acid, sodium alginate, polyvinyl alcohol, sodium carboxymethyl cellulose, and styrene-butadiene latex; The negative electrode binder includes one or more of polytetrafluoroethylene, polyacrylic acid, sodium alginate, polyvinyl alcohol, sodium carboxymethyl cellulose, and styrene-butadiene latex.
9. The aqueous sodium ion battery according to claim 5, characterized in that: The positive electrode current collector comprises one of a foil or a mesh of titanium, copper, stainless steel, or nickel; The negative electrode current collector includes one of a foil or a mesh of titanium, copper, stainless steel, and nickel.
10. An electronic device, characterized in that: An aqueous sodium ion battery comprising the aqueous solution according to any one of claims 3 to 9.