Nickel ion doped modified sodium lithium titanate material and preparation method thereof, negative plate and battery
Through nickel ion doping modified sodium titanate lithium material, combined with sol-gel method and spray-drying method, the problems of low conductivity and insufficient lithium ion migration and mobility of Na2Li2Ti6O14 material were solved, and excellent electrochemical performance and cycling stability were achieved. reduces the preparation cost.
Patent Information
- Application Number
- CN202410979896.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-05
AI Technical Summary
Na2Li2Ti6O14 material has problems with low intrinsic electron conductivity and insufficient migration and movement of lithium ions, which affects its performance in lithium-ion batteries.
Ni-ion-doped modified sodium titanate lithium material, low-priced Ni2+ ions are used to replace high-priced Ti4+ ions, and nickel-ion-doped modified sodium titanate lithium material is prepared by combining sol-gel method and spray-drying method to inhibit the material Grow grains and increase the speed of lithium ion deintercalation.
It significantly improves the electrochemical performance and cyclic stability of the material, improves the conductivity and rate performance of lithium-ion batteries, and reduces the production cost and complexity.
Smart Images

Figure CN118899431A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application belong to the technical field of negative electrode materials for lithium-ion batteries, and in particular to a nickel-ion-doped modified sodium lithium titanate material and a preparation method thereof, a negative electrode sheet, and a battery. Background Art
[0002] With the development of human society, issues related to energy and the environment have attracted widespread attention, and the demand for green energy has increased day by day, becoming an urgent need of today's society. As an important power source, lithium-ion batteries have been used in portable devices, electric vehicles, and large-scale energy storage grids. It is well known that the safety and electrochemical performance of lithium-ion batteries (LIBs) are the two main criteria for practical applications. Although carbon-based materials were initially used as anodes, they were replaced by other anode materials due to their limited capacity and efficiency and safety hazards. Later, in the effort to find a safe and reliable anode material, spinel Li was discovered. 4 Ti 5 O 12 And other titanium-based materials.
[0003] With Li 4 Ti 5 O 12 In comparison, the introduction of Na leads to a much lower potential platform (1.25V vslito / Li), which will help increase the slot voltage and thus increase the energy density of the full battery. 2 Li 2 Ti 6 O 14 is a twisted TiO shared by edges and corners 6 The octahedral embedded network is constructed to provide ion tunnels along the b axis. This arrangement is suitable for the insertion, diffusion and storage of lithium ions b. In addition, based on the total reduction of Ti4t to Ti3t in the structure, it can provide 281.6 mAh.g -1 However, Na 2 Li 2 Ti 6 O 14 There are still problems of poor conductivity and limited diffusion kinetics. Summary of the invention
[0004] In view of this, the present invention provides a nickel ion-doped modified sodium lithium titanate material and a preparation method thereof, a negative electrode sheet and a battery to solve the problem of Na 2 Li 2 Ti 6 O 14 Low intrinsic electronic conductivity and low lithium ion migration power problems are solved by this application through low-cost Ni 2+ Ions replace high-valent Ti in the form of substitutional doping4+ ions, inhibiting the growth of material grains, which is beneficial to the rapid deintercalation of lithium ions. By combining the sol-gel method with the spray drying method, nickel ions are doped through the improved sol-gel method, and the modified sodium lithium titanate material prepared has excellent electrochemical properties and extremely good cycle stability.
[0005] In a first aspect, an embodiment of the present application provides a nickel ion-doped modified sodium lithium titanate material, wherein the chemical formula of the nickel ion-doped modified sodium lithium titanate material is: Na 2 Ni x Li 2 Ti 6-x O 14 , where the value range of x is 0≤x≤0.30.
[0006] In some embodiments, which may include the above embodiments, the value of x is 0.05, 0.075, 0.1, 0.125 or 0.15.
[0007] The second aspect of the embodiment of the present application also provides a method for preparing the above-mentioned nickel ion-doped modified sodium lithium titanate material, comprising the following steps:
[0008] Step 1, dissolving the titanium source in the first solvent and stirring evenly to obtain solution A;
[0009] Step 2: dissolving the nickel source, lithium source, sodium source and complexing agent in a second solvent, performing ultrasonic vibration and stirring to obtain a solution B;
[0010] Step 3, mixing the solution A and the solution B to obtain a solution C;
[0011] Step 4: spray drying the solution C to obtain a precursor gel D;
[0012] Step 5: Grinding the precursor gel D to obtain precursor powder E;
[0013] Step six: calcining the precursor powder E to obtain a modified sodium lithium titanate material doped with nickel ions.
[0014] In some embodiments that may include the above embodiments, the following steps are specifically included:
[0015] Step 1, weigh a titanium source and dissolve it in 10-20 mL of ethanol, and heat and stir it in a constant temperature stirrer at 60-80° C. for 20-30 min to obtain solution A;
[0016] Step 2, weighing a nickel source, a lithium source and a sodium source according to the stoichiometric ratio of the chemical molecular formula of the nickel ion-doped modified sodium lithium titanate material, wherein the lithium source needs to be in excess of 10%, and the nickel source is weighed at 5wt%, 7.5%, 10wt%, 12.5wt%, and 15wt% by mass percentage, and weighing a certain amount of complexing agent and dissolving it in a mixed liquid of 10ml of ethanol and 10ml of plasma water, performing ultrasonic oscillation, and mixing and stirring evenly on a constant temperature stirrer for 2h to obtain a solution B;
[0017] Step 3, slowly adding the solution B dropwise into the solution A to mix, while the solution A is vigorously stirred for 2 hours to obtain a solution C;
[0018] Step 4, spray drying the solution C in a spray dryer to obtain a precursor gel D;
[0019] Step 5, grinding the precursor gel D for 20-30 minutes to obtain a precursor powder E;
[0020] Step 6: calcining the precursor powder E in a tube furnace under argon atmosphere to obtain a nickel ion-doped modified sodium lithium titanate material.
[0021] It should be noted that the 10% excess of lithium source is to compensate for the loss of lithium caused by high-temperature sintering. Spray drying after gelation can reduce the particle size and obtain more evenly distributed particles or powders, making the electrochemical properties of the doped material more stable after sintering.
[0022] In some embodiments that may include the above embodiments, in step 1, the complexing agent is citric acid, and the molar ratio of the sodium source, the lithium source and the citric acid is 1:1:1.
[0023] In some embodiments that may include the above embodiments, in step 4, the inlet temperature of the spray drying instrument is 140° C., the outlet temperature is 80° C., and the peristaltic pump speed is 130 rpm.
[0024] In some embodiments that may include the above embodiments, in step six, the calcination temperature is 600-800° C., preferably, the calcination temperature is 700° C.; the calcination time is 10 h, and the heating rate is 3-5° C. / min.
[0025] In some embodiments that may include the above embodiments, the nickel source is one or more of nickel hydroxide, nickel acetate, and nickel nitrate; the lithium source is one or more of lithium acetate, lithium carbonate, and lithium hydroxide; the sodium source is one or more of sodium acetate, sodium chloride, and sodium carbonate; and the titanium source is tetrabutyl titanate and / or titanium dioxide.
[0026] The third aspect of the embodiment of the present application further provides a negative electrode sheet, which contains the above-mentioned nickel ion-doped modified sodium lithium titanate material or the nickel ion-doped modified sodium lithium titanate material prepared by the above-mentioned method.
[0027] A fourth aspect of an embodiment of the present application further provides a battery, which includes the above-mentioned negative electrode sheet, and also includes a battery casing, a positive electrode sheet, a separator and an electrolyte.
[0028] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0029] 1. The nickel ion-doped modified sodium titanate lithium negative electrode material prepared by the method of the present application utilizes the principle that the radius of nickel ions and titanium ions are close. 2+ Substitution of Ti in the sodium lithium titanate lattice by substitutional doping 4+ Without destroying the crystal structure, the grain size of sodium lithium titanate is reduced, thereby increasing the ionic conductivity of sodium lithium titanate. On the one hand, it can improve the conductivity of sodium lithium titanate and the structural stability of the material. On the other hand, as a negative electrode material for lithium batteries, it exhibits excellent cycle stability and rate capability.
[0030] 2. The method of the present application innovatively adopts a method combining a sol-gel method and a spray drying method, which can improve the conductivity of the modified sodium lithium titanate negative electrode material doped with nickel ions in the present application as an electrode material for lithium ion batteries. The spray drying after the sol-gel method will obtain particles or powders with more uniform distribution, thereby making the electrochemical performance of the modified sodium lithium titanate material doped with nickel ions after sintering more stable.
[0031] 3. The preparation method adopted in this application is simple, fast and uses inexpensive raw materials. First, low-cost and easily available starting raw materials are selected, and a uniform particle powder is obtained by combining the spray drying method. The precursor powder is then calcined in a tubular furnace in an argon atmosphere to obtain the product. This synthesis method does not require expensive raw materials, equipment or complex synthesis conditions, which greatly reduces the complexity and cost of the preparation process and has practical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0033] Figure 1 XRD spectra of the nickel ion-doped modified sodium lithium titanate materials of Examples 1-5 of the present application;
[0034] Figure 2 This is a magnification diagram of the pure sodium lithium titanate material of Comparative Example 1 of the present application;
[0035] Figure 3 This is a long cycle diagram of the pure sodium lithium titanate material of Comparative Example 1 of the present application;
[0036] Figure 4 This is a rate performance diagram of the nickel ion-doped modified sodium lithium titanate material of Example 5 of the present application;
[0037] Figure 5 This is a long cycle diagram of the nickel ion-doped modified sodium lithium titanate material of Example 5 of the present application. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0039] The experimental methods in the following examples without specifying specific conditions are usually measured according to national standards; if there is no corresponding national standard, it is carried out according to the general international standards or the standard requirements known in the art. Unless otherwise specified, all parts are by weight and all percentages are by weight.
[0040] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0041] Example 1
[0042] The method for modifying the sodium lithium titanate material doped with nickel ions in this embodiment specifically comprises the following steps:
[0043] First, weigh 5 mmol of tetrabutyl titanate and slowly drop it into 15 ml of ethanol, heat and stir at 60°C constant temperature stirrer for 20 min to obtain solution A;
[0044] Then weigh 5mmol sodium acetate, 5mmol lithium acetate, 5mmol citric acid, and 5wt% nickel acetate, dissolve in a mixed liquid of 10mL ionized water and 10ml ethanol, stir evenly in a beaker, ultrasonicate in an ultrasonic cleaner for 1h, and mix evenly on a constant temperature stirrer for 2h to obtain solution B;
[0045] Solution B was slowly dripped into solution A, during which solution A needed to be vigorously stirred. After the above solution was stirred for 2 h to mix evenly, it was spray dried using a spray dryer (the inlet temperature of the spray dryer was 140 °C, the outlet temperature was 80 °C, and the peristaltic pump speed was 130 rpm). After grinding in a mortar for 30 min, it was calcined at 700 °C in a tube furnace under an argon atmosphere for 10 h, with a heating rate of 4 °C / min, to obtain nickel-doped modified Na 2 Ni 0.05 Li 2 Ti 5.95 O 14 Electrode material: NLTO@5%Ni.
[0046] Example 2
[0047] The method for modifying the sodium lithium titanate material doped with nickel ions in this embodiment specifically comprises the following steps:
[0048] First, weigh 5 mmol of tetrabutyl titanate and slowly drop it into 15 ml of ethanol, heat and stir at 60°C constant temperature stirrer for 20 min to obtain solution A;
[0049] Then weigh 5mmol sodium acetate, 5mmol lithium acetate, 5mmol citric acid, and 7.5wt% nickel acetate, dissolve in a mixed liquid of 10mL ionized water and 10ml ethanol, stir evenly in a beaker, ultrasonicate in an ultrasonic cleaner for 1h, and mix evenly on a constant temperature stirrer for 2h to obtain solution B;
[0050] Solution B was slowly dripped into solution A, during which solution A needed to be vigorously stirred. After the above solution was stirred for 2 h to mix evenly, it was spray dried using a spray dryer (the inlet temperature of the spray dryer was 140 °C, the outlet temperature was 80 °C, and the peristaltic pump speed was 130 rpm). After grinding in a mortar for 30 min, it was calcined at 700 °C in a tube furnace under an argon atmosphere for 10 h, with a heating rate of 4 °C / min, to obtain nickel-doped modified Na 2 Ni 0.75 Li 2 Ti 5.25 O 14 Electrode material: NLTO@7.5%Ni.
[0051] Example 3
[0052] The method for modifying the sodium lithium titanate material doped with nickel ions in this embodiment specifically comprises the following steps:
[0053] First, weigh 5 mmol of tetrabutyl titanate and slowly drop it into 15 ml of ethanol, heat and stir at 60°C constant temperature stirrer for 20 min to obtain solution A;
[0054] Then weigh 5mmol sodium acetate, 5mmol lithium acetate, 5mmol citric acid, and 10wt% nickel acetate, dissolve in a mixed liquid of 10mL ionized water and 10ml ethanol, stir evenly in a beaker, ultrasonicate in an ultrasonic cleaner for 1h, and mix evenly on a constant temperature stirrer for 2h to obtain solution B;
[0055] Solution B was slowly dripped into solution A, during which solution A needed to be vigorously stirred. After the above solution was stirred for 2 h to mix evenly, it was spray dried using a spray dryer (the inlet temperature of the spray dryer was 140 °C, the outlet temperature was 80 °C, and the peristaltic pump speed was 130 rpm). After grinding in a mortar for 30 min, it was calcined at 700 °C in a tube furnace under an argon atmosphere for 10 h, with a heating rate of 4 °C / min, to obtain nickel-doped modified Na 2 Ni 0.1 Li 2 Ti 5.9 O 14 Electrode material: NLTO@10%Ni.
[0056] Example 4
[0057] The method for modifying the sodium lithium titanate material doped with nickel ions in this embodiment specifically comprises the following steps:
[0058] First, weigh 5 mmol of tetrabutyl titanate and slowly drop it into 15 ml of ethanol, heat and stir at 60°C constant temperature stirrer for 20 min to obtain solution A;
[0059] Then weigh 5mmol sodium acetate, 5mmol lithium acetate, 5mmol citric acid, and 12.5wt% nickel acetate, dissolve in a mixed liquid of 10mL ionized water and 10ml ethanol, stir evenly in a beaker, ultrasonicate in an ultrasonic cleaner for 1h, and mix evenly on a constant temperature stirrer for 2h to obtain solution B;
[0060] Solution B was slowly dripped into solution A, during which solution A needed to be vigorously stirred. After the above solution was stirred for 2 h to mix evenly, it was spray dried using a spray dryer (the inlet temperature of the spray dryer was 140 °C, the outlet temperature was 80 °C, and the peristaltic pump speed was 130 rpm). After grinding in a mortar for 30 min, it was calcined at 700 °C in a tube furnace under an argon atmosphere for 10 h, with a heating rate of 4 °C / min, to obtain nickel-doped modified Na 2 Ni 0.125 Li 2 Ti 5.875 O 14 Electrode material: NLTO@12.5%Ni.
[0061] Example 5
[0062] The method for modifying the sodium lithium titanate material doped with nickel ions in this embodiment specifically comprises the following steps:
[0063] First, weigh 5 mmol of tetrabutyl titanate and slowly drop it into 15 ml of ethanol, heat and stir at 60°C constant temperature stirrer for 20 min to obtain solution A;
[0064] Then weigh 5mmol sodium acetate, 5mmol lithium acetate, 5mmol citric acid, and 15wt% nickel acetate, dissolve in a mixed liquid of 10mL ionized water and 10ml ethanol, stir evenly in a beaker, ultrasonicate in an ultrasonic cleaner for 1h, and mix evenly on a constant temperature stirrer for 2h to obtain solution B;
[0065] Solution B was slowly dripped into solution A, during which solution A needed to be vigorously stirred. After the above solution was stirred for 2 h to mix evenly, it was spray dried using a spray dryer (the inlet temperature of the spray dryer was 140 °C, the outlet temperature was 80 °C, and the peristaltic pump speed was 130 rpm). After grinding in a mortar for 30 min, it was calcined at 700 °C in a tube furnace under an argon atmosphere for 10 h, with a heating rate of 4 °C / min, to obtain nickel-doped modified Na 2 Ni 0.15 Li 2 Ti 5.85 O 14 Electrode material: NLTO@15%Ni.
[0066] Example 6
[0067] The method for modifying the sodium lithium titanate material doped with nickel ions in this embodiment specifically comprises the following steps:
[0068] First, weigh 5 mmol of tetrabutyl titanate and slowly drop it into 15 ml of ethanol, heat and stir at 60°C constant temperature stirrer for 20 min to obtain solution A;
[0069] Then weigh 5mmol sodium acetate, 5mmol lithium acetate, 5mmol citric acid, and 15wt% nickel acetate, dissolve in a mixed liquid of 10mL ionized water and 10ml ethanol, stir evenly in a beaker, ultrasonicate in an ultrasonic cleaner for 1h, and mix evenly on a constant temperature stirrer for 2h to obtain solution B;
[0070] Solution B was slowly dripped into solution A, during which solution A needed to be vigorously stirred. After the above solution was stirred for 2 h to mix evenly, it was spray dried using a spray dryer (the inlet temperature of the spray dryer was 140 °C, the outlet temperature was 80 °C, and the peristaltic pump speed was 130 rpm). After grinding in a mortar for 30 min, it was calcined at 600 °C in a tube furnace under an argon atmosphere for 10 h, with a heating rate of 4 °C / min, to obtain nickel-doped modified Na 2 Ni0.15 Li 2 Ti 5.85 O 14 Electrode material.
[0071] Example 7
[0072] The method for modifying the sodium lithium titanate material doped with nickel ions in this embodiment specifically comprises the following steps:
[0073] First, weigh 5 mmol of tetrabutyl titanate and slowly drop it into 15 ml of ethanol, heat and stir at 60°C constant temperature stirrer for 20 min to obtain solution A;
[0074] Then weigh 5mmol sodium acetate, 5mmol lithium acetate, 5mmol citric acid, and 15wt% nickel acetate, dissolve in a mixed liquid of 10mL ionized water and 10ml ethanol, stir evenly in a beaker, ultrasonicate in an ultrasonic cleaner for 1h, and mix evenly on a constant temperature stirrer for 2h to obtain solution B;
[0075] Solution B was slowly dripped into solution A, during which solution A needed to be vigorously stirred. After the above solution was stirred for 2 h to mix evenly, it was spray dried using a spray dryer (the inlet temperature of the spray dryer was 140 ° C, the outlet temperature was 80 ° C, and the peristaltic pump speed was 130 rpm). After grinding in a mortar for 30 min, it was calcined in a tube furnace at 800 ° C for 10 h under an argon atmosphere, with a heating rate of 4 ° C / min, to obtain nickel-doped modified Na 2 Ni 0.15 Li 2 Ti 5.85 O 14 Electrode material.
[0076] Comparative Example 1
[0077] The method for modifying the sodium lithium titanate material doped with nickel ions in this comparative example specifically comprises the following steps:
[0078] First, weigh 5 mmol of tetrabutyl titanate and slowly drop it into 15 ml of ethanol, heat and stir at 60°C constant temperature stirrer for 20 min to obtain solution A;
[0079] Then weigh 5mmol of sodium acetate, 5mmol of lithium acetate, and 5mmol of citric acid, dissolve them in a mixed liquid of 10mL of ionized water and 10ml of ethanol, stir them evenly in a beaker, ultrasonicate them in an ultrasonic cleaner for 1h, and mix them evenly on a constant temperature stirrer for 2h to obtain solution B;
[0080] Solution B was slowly dripped into solution A, during which solution A needed to be vigorously stirred. After the above solution was stirred for 2 hours to mix evenly, it was spray dried using a spray dryer (the inlet temperature of the spray dryer was 140°C, the outlet temperature was 80°C, and the peristaltic pump speed was 130 rpm). After grinding in a mortar for 30 minutes, it was calcined at 700°C in a tube furnace under an argon atmosphere for 10 hours with a heating rate of 4°C / min to obtain a pure sample of Na 2 Li 2 Ti 6 O 14 Electrode material.
[0081] XRD test
[0082] The materials prepared in Examples 1-5 were subjected to XRD testing. The test results are as follows: Figure 1 As shown. Figure 1 It can be seen that the main diffraction peak positions of nickel-doped sodium lithium titanate prepared with different doping ratios are consistent, and all the main diffraction peaks are basically consistent with the standard spectrum of sodium lithium titanate (PDF#52-0690), indicating that the target product was successfully synthesized.
[0083] Battery performance test
[0084] The product of Example 5 is used as an electrode material for lithium-ion batteries, and the specific production process is as follows:
[0085] (1) The material of Example 5 was mixed with the conductive agent Super P and PVDF in a mass ratio of 8:1:1, ground and mixed in a mortar, an appropriate amount of NMP was added and then coated on a copper foil, placed in a vacuum drying oven at 80° C. for 12 h, and rolled and cut into pieces to obtain a battery negative electrode sheet;
[0086] (2) Using lithium metal sheets as counter electrodes, a 2016-type button cell was made in a glove box filled with argon. The diaphragm used was Celgard 2250, and the electrolyte used was LiPF with a concentration of 1 M. 6 / EC:DEC (volume ratio 1:1), the prepared 2016 type button battery was tested on the blue power test system to test the electrochemical energy storage performance of the prepared lithium-ion battery;
[0087] (3) The charge and discharge range is 0.01-3V, and the charge and discharge rates are 0.1A / g, 0.2A / g, 0.3A / g, 0.5A / g, and 1A / g. The electrochemical energy storage performance of the prepared lithium-ion battery is tested, such as Figure 4 and Figure 5 shown.
[0088] Depend on Figure 4 It can be seen that the Na prepared in Example 5 2 Ni0.15 Li 2 Ti 5.85 O 14 The composite material has a discharge specific capacity of about 231.8mAh / g, 123mAh / g, 104.7mAh / g, 92.9mAh / g, and 80.7mAh / g at different charge and discharge current densities of 0.1A / g, 0.2A / g, 0.3A / g, 0.5A / g, and 1A / g, and a capacity retention rate of 95.11%, 98.29%, 99.61%, 99.11%, and 99.62%, respectively. This indicates that the material has good cycle performance and high coulombic efficiency.
[0089] Depend on Figure 5 It can be seen that the Na prepared in Example 5 2 Ni 0.15 Li 2 Ti 5.85 O 14 After the composite material was cycled 100 times at a current density of 100 mA / g, its specific capacity was still 200 mAh / g, and the capacity retention rate was about 99.92%, indicating that the material had good cycle performance and high coulombic efficiency.
[0090] The product of Comparative Example 1 is used as an electrode material for lithium-ion batteries, and the specific production process is as follows:
[0091] (1) The material of comparative example 1 was mixed with the conductive agent Super P and PVDF in a mass ratio of 8:1:1, ground and mixed in a mortar, an appropriate amount of NMP was added and then coated on a copper foil, placed in a vacuum drying oven at 80° C. for 12 h, and rolled and cut into pieces to obtain a battery negative electrode sheet;
[0092] (2) Using lithium metal sheets as counter electrodes, a 2016-type button cell was made in a glove box filled with argon. The diaphragm used was Celgard 2250, and the electrolyte used was LiPF with a concentration of 1 M. 6 / EC:DEC (volume ratio 1:1), the prepared 2016 type button battery was tested on the blue power test system to test the electrochemical energy storage performance of the prepared lithium-ion battery;
[0093] (3) The charge and discharge range is 0.01-3V, and the charge and discharge rates are 0.1A / g, 0.2A / g, 0.3A / g, and 0.5A / g. The electrochemical energy storage performance of the prepared lithium-ion battery is tested, such as Figure 2 and Figure 3 shown.
[0094] Depend on Figure 2 It can be seen that the pure sample Na prepared in Comparative Example 1 2 Li2 Ti 6 O 14 The material has a discharge specific capacity of about 130.2 mAh / g, 89 mAh / g, 72.6 mAh / g, and 57.3 mAh / g at different charge and discharge current densities of 0.1 A / g, 0.2 A / g, 0.3 A / g, and 0.5 A / g, and a capacity retention rate of 78.75%, 95.55%, 95.82%, and 97.48%, respectively. Compared with Example 5, it can be seen that the material prepared in Example 5 has better rate performance and higher coulombic efficiency.
[0095] Depend on Figure 3 It can be seen that the pure sample Na prepared in Comparative Example 1 2 Li 2 Ti 6 O 14 After the material was cycled 100 times at a current density of 100 mA / g, its specific capacity was only 150.8 mAh / g, and the capacity retention rate was about 99.07%. Compared with Example 5, it can be seen that the material prepared in Example 5 has better cycle performance and higher coulombic efficiency.
[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A nickel ion-doped modified sodium lithium titanate material, characterized in that: The chemical formula of the nickel ion-doped modified sodium lithium titanate material is: Na2Ni x Li2Ti 6-x O 14 , where the value range of x is 0≤x≤0.
30.
2. The nickel ion-doped modified sodium lithium titanate material according to claim 1, characterized in that: The value of x is 0.05, 0.075, 0.1, 0.125 or 0.
15.
3. A method for preparing the nickel ion-doped modified sodium lithium titanate material according to claim 1 or 2, characterized in that: The steps include: Step 1, dissolving the titanium source in the first solvent and stirring evenly to obtain solution A; Step 2: dissolving the nickel source, lithium source, sodium source and complexing agent in a second solvent, performing ultrasonic vibration and stirring to obtain a solution B; Step 3, mixing the solution A and the solution B to obtain a solution C; Step 4: spray drying the solution C to obtain a precursor gel D; Step 5: Grinding the precursor gel D to obtain precursor powder E; Step six: calcining the precursor powder E to obtain a modified sodium lithium titanate material doped with nickel ions.
4. The method for modifying sodium lithium titanate material by nickel ion doping according to claim 3, characterized in that: The specific steps include: Step 1, weigh a titanium source and dissolve it in ethanol, heat and stir it in a constant temperature stirrer at 60-80° C. for 20-30 minutes to obtain solution A; Step 2, weighing a nickel source, a lithium source and a sodium source according to the stoichiometric ratio of the chemical molecular formula of the nickel ion-doped modified sodium lithium titanate material, wherein the lithium source needs to be in excess of 10%, and the nickel source is weighed at 5wt%, 7.5%, 10wt%, 12.5wt%, and 15wt% by mass percentage, and weighing a certain amount of a complexing agent and dissolving it in a mixed liquid of ethanol and plasma water, performing ultrasonic oscillation, and mixing and stirring uniformly on a constant temperature stirrer for 2h to obtain a solution B; Step 3, slowly adding the solution B dropwise into the solution A to mix, while the solution A is vigorously stirred for 2 hours to obtain a solution C; Step 4, spray drying the solution C in a spray dryer to obtain a precursor gel D; Step 5, grinding the precursor gel D for 20-30 minutes to obtain a precursor powder E; Step 6: calcining the precursor powder E in a tube furnace under argon atmosphere to obtain a nickel ion-doped modified sodium lithium titanate material.
5. The method for modifying the sodium lithium titanate material by nickel ion doping according to claim 4, characterized in that: In step 1, the complexing agent is citric acid, and the molar ratio of the sodium source, the lithium source and the citric acid is 1:1:
1.
6. The method for modifying the sodium lithium titanate material by nickel ion doping according to claim 4, characterized in that: In step 4, the inlet temperature of the spray drying apparatus is 140° C., the outlet temperature is 80° C., and the peristaltic pump speed is 130 rpm.
7. The method for modifying sodium lithium titanate material by nickel ion doping according to claim 4, characterized in that: In step six, the calcination temperature is 600-800°C, the calcination time is 10h, and the heating rate is 3-5°C / min.
8. The method for modifying sodium lithium titanate material by nickel ion doping according to claim 4, characterized in that: The nickel source is one or more of nickel hydroxide, nickel acetate, and nickel nitrate; the lithium source is one or more of lithium acetate, lithium carbonate, and lithium hydroxide; the sodium source is one or more of sodium acetate, sodium chloride, and sodium carbonate; and the titanium source is tetrabutyl titanate and / or titanium dioxide.
9. A negative electrode sheet, characterized in that: The negative electrode sheet contains the nickel ion-doped modified sodium lithium titanate material according to claim 1 or 2 or the nickel ion-doped modified sodium lithium titanate material prepared by the method of any one of claims 3-8.
10. A battery, characterized in that: The invention comprises the negative electrode sheet as claimed in claim 9, and also comprises a battery casing, a positive electrode sheet, a separator and an electrolyte.