Lithium ion semi-finished product battery baking method
By adopting circulating baking and nitrogen inlet methods in low-humidity environments, the performance problems caused by excessive moisture in lithium-ion batteries are solved, and the rapid and efficient removal of moisture is achieved, energy consumption is reduced, and the safety and circulation performance of the battery are improved. .
Patent Information
- Application Number
- CN202411293287.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-05
AI Technical Summary
Excessive moisture in the production process of existing lithium-ion batteries causes the decomposition of lithium salts of the electrolyte, corroding positive and negative electrode materials, reducing circulation and safety performance, and baking methods to remove moisture consume a lot of energy.
In an environment with a relative humidity below 3%, multiple cycle baking steps are used, combining temperature arithmetic rise and nitrogen inlet, vacuum degree is adjusted, and moisture in the battery is quickly removed through pressure and temperature control, reducing energy consumption.
It significantly shortens the baking time, reduces energy consumption, improves the moisture removal efficiency of lithium-ion batteries, avoids the problem of circulating diving, and improves the safety performance of the battery.
Smart Images

Figure CN118899547A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a method for baking a lithium ion semi-finished battery. Background Art
[0002] As the automotive industry pursues power energy, lithium-ion batteries have gradually gained attention due to their high energy density and long cycle life. As a key factor that needs to be strictly controlled in the production process of lithium-ion batteries, excessive moisture will lead to the decomposition of lithium salts in the electrolyte and have a certain corrosive effect on the positive and negative electrode materials and current collectors, and will also cause the battery's cycle performance and safety performance to decrease. The current method of baking moisture in the industry is mainly: put the battery in an oven, set the temperature and vacuum degree for baking, lower the temperature to room temperature after a certain period of time, release the vacuum environment, take out the battery and test the moisture. In order to control the moisture content, this method can only extend the baking time indefinitely and increase energy consumption. Summary of the invention
[0003] The purpose of the present invention is to provide a method for baking a lithium-ion semi-finished battery, which can more quickly and efficiently remove moisture from the semi-finished battery, avoid excessive moisture, performance problems such as cycle diving, reduce the safety risk of the lithium-ion battery, and save energy consumption.
[0004] In order to achieve the above object, the present invention adopts the following technical solution:
[0005] A method for baking a lithium-ion semi-finished battery comprises the following steps: all operations are performed under the condition that the relative humidity of the environment is kept below 3%,
[0006] S1: Apply pressure P1 to the packaged lithium-ion semi-finished battery and place it in an oven;
[0007] S2: baking the lithium-ion semi-finished battery for T1 time at the first baking temperature environment;
[0008] S3: After S2 is completed, the lithium-ion semi-finished battery is baked at the first baking temperature and the first vacuum environment for T2 time;
[0009] S4: After S3, nitrogen is continuously introduced into the oven, the vacuum degree of the oven is adjusted to the second vacuum degree, and the first baking temperature is maintained for baking time T3;
[0010] S5: Recycle steps S3 and S4 three times, and in each cycle, the baking temperature of step S3 increases in an arithmetic progression to maintain the first vacuum degree; step S4 follows the temperature of step S3 in this cycle to maintain the second vacuum degree;
[0011] S6: End the baking and test the moisture content of the lithium-ion semi-finished battery.
[0012] Preferably, the pressure P1 is 0.05-0.08 MPa, and is applied by: clamping pressurization.
[0013] Preferably, the first baking temperature is 85±5°C, and the baking time T1 is 30 minutes, more preferably 85°C to 90°C.
[0014] Preferably, the first vacuum degree is -90±5 KPa, and the baking time T2 is 50 to 60 minutes. The vacuum degree is more preferably -90 KPa to -95 KPa, and the baking time is more preferably 60 minutes.
[0015] Preferably, the second vacuum degree is -15±5 KPa, and the baking time T3 is 15 to 25 minutes. The vacuum degree is more preferably -15 KPa, and the baking time is more preferably 15 minutes.
[0016] The beneficial effect of adopting the above technical solution is as follows: the purpose of setting the second vacuum degree is to reduce the vacuum degree inside the oven by introducing nitrogen, so that the inside of the oven is close to normal pressure, which facilitates the removal of moisture produced by baking.
[0017] Preferably, the arithmetic progression increases the baking temperature by 15 to 20°C per cycle, more preferably by 20°C.
[0018] The beneficial effects of adopting the above technical solution: The main influencing factors of moisture baking of lithium-ion semi-finished batteries are time and oven temperature. In order to improve production efficiency, increasing the temperature is an important direction in the optimization process, but energy consumption and the high temperature resistance of the battery itself must be considered. Therefore, this technical solution adopts an equal value increase method.
[0019] The incremental temperature is 15-20℃, mainly due to the following reasons:
[0020] 1) The shrinkage rate of the battery separator at high temperature, the increasing temperature should not be too high;
[0021] 2) The incremental temperature is small. According to previous experience, the temperature difference is too small and the moisture baking effect is not good.
[0022] Preferably, the moisture requirement in S6 is: ≤300ppm for the positive electrode and ≤300ppm for the negative electrode.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The method for baking semi-finished lithium-ion batteries provided by the present invention combines two methods of temperature arithmetic rise and multiple ventilation, which greatly reduces the baking time, saves energy consumption during the baking process, and effectively improves the baking efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 . DETAILED DESCRIPTION
[0026] Embodiments of the present invention are described below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but are not to be construed as limiting the present invention.
[0027] Example 1
[0028] Take 50 23Ah lithium iron phosphate lithium-ion semi-finished batteries, record them as batch A, and perform the following steps: All operations are performed under the condition that the relative humidity of the environment is kept below 3%.
[0029] (1) The packaged lithium-ion semi-finished battery is placed in an oven with a pressure of 0.07 MPa applied by a clamping pressurization method;
[0030] (2) Adjust the oven temperature to 85°C and set the baking time to 30 minutes under this environment;
[0031] (3) After the set baking time is over, adjust the vacuum degree in the oven to -90 KPa, maintain the oven temperature at 85 °C, and set the baking time to 60 min under this environment;
[0032] (4) After the set baking time is over, nitrogen is continuously introduced into the oven, the vacuum degree is reduced to -15 KPa, the oven temperature is maintained at 85 ° C, and the baking time is set to 15 min under this environment;
[0033] (5) After the set baking time is over, adjust the vacuum degree in the oven to -90 KPa, maintain the oven temperature at 105 °C, and set the baking time to 60 min under this environment;
[0034] (6) After the set baking time is over, nitrogen is continuously introduced into the oven, the vacuum degree is reduced to -15 KPa, the oven temperature is maintained at 105 ° C, and the baking time is set to 15 min under this environment;
[0035] (7) After the set baking time is over, adjust the vacuum degree in the oven to -90 KPa, maintain the oven temperature at 125 ° C, and set the baking time to 60 min under this environment;
[0036] (8) After the set baking time is over, nitrogen is continuously introduced into the oven, the vacuum degree is reduced to -15 KPa, the oven temperature is maintained at 125 ° C, and the baking time is set to 15 min under this environment;
[0037] (9) After the set baking time is over, adjust the vacuum degree in the oven to -90 KPa, maintain the oven temperature at 145 ° C, and set the baking time to 60 min under this environment;
[0038] (10) After the set baking time is over, nitrogen is continuously introduced into the oven, the vacuum degree is reduced to -15 KPa, the oven temperature is maintained at 145 °C, and the baking time is set to 15 min under this environment;
[0039] (11) After the set baking time is over, the oven is cooled down, and the oven door is opened after the dry gas is continuously filled for 5 minutes. The 50 lithium-ion semi-finished batteries are taken out for moisture testing. The moisture requirements are: positive electrode ≤300ppm, negative electrode ≤300ppm.
[0040] Table 1 Moisture test results of batch A in Example 1
[0041]
[0042]
[0043]
[0044] In the above table, the moisture requirements are: positive electrode ≤300ppm, negative electrode ≤300ppm; after implementing this method, the moisture content of 50 lithium-ion semi-finished batteries all passed the test.
[0045] Example 2
[0046] Take 50 23Ah lithium iron phosphate lithium-ion semi-finished batteries, record them as batch B, and follow the following steps: All operations are carried out under the condition that the relative humidity of the environment is kept below 3%.
[0047] (1) The packaged lithium-ion semi-finished battery is placed in an oven with a pressure of 0.07 MPa applied by a clamping pressurization method;
[0048] (2) Adjust the oven temperature to 90°C and set the baking time to 30 minutes under this environment;
[0049] (3) After the set baking time is over, adjust the vacuum degree in the oven to -95KPa, maintain the oven temperature at 90°C, and set the baking time to 60min under this environment;
[0050] (4) After the set baking time is over, nitrogen is continuously introduced into the oven, the vacuum degree is reduced to -15 KPa, the oven temperature is maintained at 90°C, and the baking time is set to 15 min under this environment;
[0051] (5) After the set baking time is over, adjust the vacuum degree in the oven to -95KPa, maintain the oven temperature at 110°C, and set the baking time to 60min under this environment;
[0052] (6) After the set baking time is over, nitrogen is continuously introduced into the oven, the vacuum degree is reduced to -15 KPa, the oven temperature is maintained at 110 ° C, and the baking time is set to 15 min under this environment;
[0053] (7) After the set baking time is over, adjust the vacuum degree in the oven to -95KPa, maintain the oven temperature at 130°C, and set the baking time to 60min under this environment;
[0054] (8) After the set baking time is over, nitrogen is continuously introduced into the oven, the vacuum degree is reduced to -15 KPa, the oven temperature is maintained at 130 ° C, and the baking time is set to 15 min under this environment;
[0055] (9) After the set baking time is over, adjust the vacuum degree in the oven to -95KPa, maintain the oven temperature at 150°C, and set the baking time to 60min under this environment;
[0056] (10) After the set baking time is over, nitrogen is continuously introduced into the oven, the vacuum degree is reduced to -15 KPa, the oven temperature is maintained at 150 °C, and the baking time is set to 15 min under this environment;
[0057] (11) After the set baking time is over, the oven is cooled down, and the oven door is opened after the dry gas is continuously filled for 5 minutes. The 50 lithium-ion semi-finished batteries are taken out for moisture testing. The moisture requirements are: positive electrode ≤300ppm, negative electrode ≤300ppm.
[0058] Table 2 Moisture test results of batch B in Example 2
[0059]
[0060]
[0061]
[0062] In the above table, the moisture requirements are: positive electrode ≤300ppm, negative electrode ≤300ppm; after implementing this method, the moisture content of 50 lithium-ion semi-finished batteries all passed the test.
[0063] Comparative Example 1
[0064] Take 50 23Ah lithium iron phosphate lithium-ion semi-finished batteries, record them as batch C, and perform the following steps: All operations are carried out under the condition that the relative humidity of the environment is kept below 3%.
[0065] (1) 50 semi-finished lithium iron phosphate lithium-ion batteries are placed in turn on a hot press plate capable of heating and pressurizing for hot pressing and baking, the heating temperature is 95° C., the heating time is 50 min, and the surface pressure of the single battery is 0.5 MPa;
[0066] (2) Place the hot-pressed battery in a vacuum oven that has been heated to 95°C in advance, maintain this temperature and perform the following operations: evacuate to below -0.099 MPa and hold for 50 min, fill with nitrogen and hold for 20 min, evacuate to below -0.099 MPa and hold for 50 min, fill with nitrogen and hold for 20 min, evacuate to below -0.099 MPa and hold for 50 min, fill with nitrogen and hold for 20 min, evacuate to below -0.099 MPa and hold for 50 min, fill with nitrogen and hold for 20 min, evacuate to below -0.099 MPa and hold for 50 min, fill with nitrogen and hold for 20 min, evacuate to below -0.099 MPa and hold for 50 min, fill with nitrogen and hold for 20 min, evacuate to below -0.099 MPa and hold for 50 min, fill with nitrogen and hold for 20 min, evacuate to below -0.099 MPa and hold for 50 min, fill with nitrogen and hold for 20 min;
[0067] (3) Evacuate the vacuum oven to below -0.099 MPa, stop heating, wait until the vacuum oven temperature cools to below 45°C, fill it with nitrogen again, and then take out the battery;
[0068] (4) Take these 50 lithium-ion semi-finished batteries and conduct a moisture test. The moisture requirements are: positive electrode ≤ 300ppm, negative electrode ≤ 300ppm.
[0069] Table 3 Comparative Example 1 Batch C Moisture Test Results
[0070]
[0071]
[0072]
[0073] In the above table, the moisture requirements are: positive electrode ≤300ppm, negative electrode ≤300ppm; after the implementation of this method, after 470 minutes, the moisture content of 50 lithium-ion semi-finished batteries was qualified.
[0074] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for baking a semi-finished lithium-ion battery. It is characterized in that The following steps are involved: All operations were carried out in an environment with relative humidity kept below 3%. S1: Apply pressure P1 to the packaged lithium-ion semi-finished battery and place it in an oven; S2: baking the lithium-ion semi-finished battery for T1 time at the first baking temperature environment; S3: After S2 is completed, the lithium-ion semi-finished battery is baked at the first baking temperature and the first vacuum environment for T2 time; S4: After S3, nitrogen is continuously introduced into the oven, the vacuum degree of the oven is adjusted to the second vacuum degree, and the first baking temperature is maintained for baking time T3; S5: Recycle steps S3 and S4 three times, and in each cycle, the baking temperature of step S3 increases in an arithmetic progression to maintain the first vacuum degree; step S4 follows the temperature of step S3 in this cycle to maintain the second vacuum degree; S6: End the baking and test the moisture content of the lithium-ion semi-finished battery.
2. A method for baking a lithium-ion semi-finished battery according to claim 1, It is characterized in that The pressure P1 is 0.05-0.08 MPa, and is applied by: clamping pressurization.
3. A method for baking a lithium-ion semi-finished battery according to claim 1, It is characterized in that The first baking temperature is 85±5° C., and the baking time T1 is 30 minutes.
4. A method for baking a lithium-ion semi-finished battery according to claim 1, It is characterized in that The first vacuum degree is -90±5 KPa, and the baking time T2 is 50 to 60 minutes.
5. A method for baking a lithium-ion semi-finished battery according to claim 1, It is characterized in that The second vacuum degree is -15±5 KPa; and the baking time T3 is 15 to 25 minutes.
6. A method for baking a lithium-ion semi-finished battery according to claim 1, It is characterized in that The arithmetic progression increases the baking temperature by 15 to 20° C. in each cycle.