Preparation method of anode of display screen
By forming an inclined ladder-shaped mask layer on the anode metal layer of the Micro OLED display and etching, the preparation process is simplified, the problems of complex and cost in traditional processes are solved, and efficient display performance is achieved.
Patent Information
- Application Number
- CN202410999417.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-05
AI Technical Summary
The anode preparation process of traditional Micro OLED displays is complex and costly, requiring three hard mask preparation and etching, making it difficult to meet the high-end market's demand for color gamut and resolution.
By forming an inclined ladder-shaped mask layer on the side of the anode metal layer away from the substrate and etching it on it, grooves with different depths are formed to achieve pixel height differences, and the display performance is improved by using the optically strong microcavity effect and simplifying preparation process.
It reduces the preparation cost, improves efficiency, avoids three hard mask preparations, achieves high display performance of the display screen, and meets high-end market standards.
Smart Images

Figure CN118900609A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optical technology, and in particular to a method for preparing an anode of a display screen. Background Art
[0002] Micro OLED is a display technology based on organic materials. It uses organic light-emitting diodes. The light-emitting layer composed of organic materials can emit light under the stimulation of electric current. Micro OLED has the remarkable characteristics of high definition, high refresh rate, high contrast, lightness and thinness, and is widely used in head-mounted displays, AR / VR glasses and other equipment.
[0003] In the current production process of Micro OLED displays, the structure and morphology of the pixel anode determine the performance of the device. At present, in order to further improve the performance of the device and make the device color gamut and resolution reach the high-end market standards, the pixel heights of B, G, and R will be different, so as to utilize the optically strong microcavity effect to improve product quality. The traditional optically strong microcavity preparation process requires three hard mask preparations, patterning and etching, and one anode etching for B, G, and R pixels during the production of the anode structure. The preparation process is complicated and the cost is high. Summary of the invention
[0004] The embodiment of the present invention provides a method for preparing an anode of a display screen. By setting an inclined ladder-shaped mask layer, grooves of different depths can be formed only by etching. At this time, the heights of pixels are different. The display screen can use the optical strong microcavity effect to improve the display performance of the display screen. There is no need to go through three hard mask preparations, thereby reducing costs and improving preparation efficiency.
[0005] According to one aspect of the present invention, there is provided a method for preparing an anode of a display screen, comprising:
[0006] Forming an oblique ladder-shaped mask layer on a surface of the anode metal layer away from the first substrate;
[0007] forming a first photoresist layer above the mask layer;
[0008] performing patterning on the first photoresist layer;
[0009] The mask layer and the anode metal layer exposed by the first photoresist layer are etched to form at least two grooves with different depths on a surface of the anode metal layer away from the first substrate.
[0010] Optionally, before forming the oblique ladder-shaped mask layer on the surface of the anode metal layer away from the first substrate, the method further includes:
[0011] An anode metal layer is formed on the surface of the first substrate.
[0012] Optionally, forming an oblique ladder-shaped mask layer on a surface of the anode metal layer away from the first substrate comprises:
[0013] Aligning a first mask and a second mask having the same structure up and down, and arranging them between the coating target and the first substrate;
[0014] The first mask and the second mask are controlled to move relative to each other in the horizontal direction at a preset speed, and the first substrate is plated at the same time to form an inclined ladder-shaped mask layer on the surface of the anode metal layer away from the first substrate.
[0015] Optionally, after etching the mask layer and the anode metal layer exposed by the first photoresist layer to form at least two grooves with different depths on the surface of the anode metal layer away from the first substrate, the method further comprises:
[0016] The first photoresist layer on the surface of the mask layer is removed.
[0017] Optionally, after removing the first photoresist layer on the surface of the mask layer, the method further includes:
[0018] A second photoresist layer is formed on a surface of the mask layer away from the first substrate, wherein the second photoresist layer covers the mask layer and the surface of the groove.
[0019] Optionally, after forming a second photoresist layer on a surface of the mask layer away from the first substrate, the method further comprises:
[0020] The second photoresist layer outside the groove is removed.
[0021] Optionally, after removing the second photoresist layer outside the groove, the method further includes:
[0022] The mask layer is removed.
[0023] Optionally, after removing the mask layer, the method further includes:
[0024] The anode metal layer not covered by the second photoresist layer is etched.
[0025] Optionally, after etching the anode metal layer not covered by the second photoresist layer, the method further includes:
[0026] The second photoresist layer is removed, and at least two anode metal layers with different heights are formed on the surface of the first substrate.
[0027] Optionally, forming an anode metal layer on the surface of the first substrate includes:
[0028] A reflective layer, an adhesive layer and a light-emitting conductive layer are sequentially formed on the surface of the first substrate from bottom to top.
[0029] An embodiment of the present invention provides a method for preparing an anode of a display screen, a method for preparing an anode of a display screen, forming an inclined ladder-shaped mask layer on the surface of the anode metal layer away from the first substrate, and etching the mask layer and the anode metal layer to form at least two grooves of different depths on the surface of the anode metal layer away from the first substrate. By setting the inclined ladder-shaped mask layer, grooves of different depths can be formed only by etching, and the heights of the pixels are different at this time. The display screen can use the optical strong microcavity effect to improve the display performance of the display screen, and does not need to undergo three hard mask preparations, thereby reducing costs and improving preparation efficiency.
[0030] It should be understood that the contents described in this section are not intended to identify the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 A flow chart of a method for preparing an anode of a first display screen provided by an embodiment of the present invention;
[0033] Figure 2 A schematic diagram of a process for preparing an anode of a first display screen provided by an embodiment of the present invention;
[0034] Figure 3 A flow chart of a method for preparing an anode of a second display screen provided by an embodiment of the present invention;
[0035] Figure 4 A schematic diagram of the anode preparation process of the second display screen provided by an embodiment of the present invention;
[0036] Figure 5 A schematic top view of the structure of a first mask provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0038] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0039] Figure 1 A flow chart of a method for preparing an anode of a first display screen provided by an embodiment of the present invention, Figure 2 A schematic diagram of the anode preparation process of the first display screen provided in the embodiment of the present invention, referring to Figure 1 and Figure 2 , the preparation method comprises:
[0040] S101, forming an oblique ladder-shaped mask layer on a surface of the anode metal layer away from the first substrate.
[0041] Among them, OLED (Organic Light-Emitting Diode), that is, organic light-emitting diode, refers to an organic semiconductor device that emits light through carrier injection and recombination of organic semiconductor materials and luminescent materials under the drive of an electric field. The first substrate 10 is used to provide support for the display screen. The anode metal layer 20 is arranged on a side surface of the first substrate 10, and the anode metal layer 20 emits light when carriers are injected and recombinated. A slanted ladder-shaped mask layer 30 is formed on the side surface of the anode metal layer 20 away from the first substrate 10. The etching rate of the mask layer 30 is less than the etching rate of the anode metal layer 20. After the mask layers 30 of different heights are etched for the same time, the heights of the anode metal layers 20 formed are different, and the pixel heights are different, so that the display screen can use the optical strong microcavity effect to improve the display performance of the display screen.
[0042] In one embodiment, if Figure 2As shown in (a), a mask layer 30 having an oblique ladder shape is formed on a surface of the anode metal layer 20 which is away from the first substrate 10 .
[0043] S102 , forming a first photoresist layer above the mask layer.
[0044] A first photoresist layer 40 is formed on the mask layer 30 , and the required pattern is transferred from the first photoresist layer 40 to the mask layer 30 and the anode metal layer 20 by patterning the first photoresist layer 40 .
[0045] In one embodiment, if Figure 2 As shown in (b), a first photoresist layer 40 is formed on the mask layer 30.
[0046] S103, performing patterning on the first photoresist layer.
[0047] Among them, the patterning process utilizes the covering and protective effect of the first photoresist layer 40 to remove the thin film without protection of the first photoresist layer 40 by chemical reaction or physical action. By exposing and developing the first photoresist layer 40, the patterning process forms the required graphics to provide a basis for subsequent etching.
[0048] In one embodiment, if Figure 2 As shown in (c), the first photoresist layer 40 is patterned.
[0049] S104, etching the mask layer and the anode metal layer exposed by the first photoresist layer to form at least two grooves of different depths on the surface of the anode metal layer away from the first substrate.
[0050] Among them, the etching process refers to the process of selectively corroding or stripping the surface of the substrate or the thin film covered on the surface by chemical or physical methods. The optically strong microcavity effect refers to the light-emitting area of the device being located in a resonant cavity composed of a total reflection film and a semi-reflection film. When the cavity length is of the same order of magnitude as the wavelength of the light wave, light of a specific wavelength will be selected and enhanced, and the spectrum will be narrowed. The optically strong microcavity effect can improve the display performance of the display screen. The mask layer 30 and the anode metal layer 20 exposed by the first photoresist layer 40 are etched. Since the mask layer 30 is in an inclined ladder shape, the height of the mask layer 30 at different positions is different. After the same etching time, grooves 21 with different depths are formed on the surface of the anode metal layer 20. The depth of the groove 21 is determined by the etching process, and the depth of the groove 21 can be set according to actual needs. The embodiment of the present invention does not make specific restrictions on this. As an example, the number of grooves 21 can be 3, which meets the display requirements of three pixels of R, G, and B. In other embodiments, the grooves 21 can also be set to other numbers, and the embodiment of the present invention does not make specific restrictions on this.
[0051] In one embodiment, if Figure 2 As shown in (d), the mask layer 30 and the anode metal layer 20 exposed by the first photoresist layer 40 are etched to form at least two grooves 21 with different depths on the surface of the anode metal layer 20 away from the first substrate 10.
[0052] An embodiment of the present invention provides a method for preparing an anode of a display screen, wherein a mask layer in the shape of a ramp is formed on a surface of an anode metal layer away from a first substrate, and at least two grooves of different depths are formed on a surface of the anode metal layer away from the first substrate by etching the mask layer and the anode metal layer. By setting a mask layer in the shape of a ramp, grooves of different depths can be formed only by etching, and at this time, the heights of pixels are different. The display screen can utilize an optically strong microcavity effect to improve the display performance of the display screen, and does not require three hard mask preparations, thereby reducing costs and improving preparation efficiency.
[0053] Based on the above embodiments, the embodiments of the present invention provide an exemplary description of how to perform multiple etchings according to grooves with different depths to form anode metal layers with different heights. Figure 3 A flow chart of a method for preparing an anode of a second display screen provided by an embodiment of the present invention, Figure 4 A schematic diagram of the anode preparation process of the second display screen provided in an embodiment of the present invention, Figure 5 A schematic diagram of a top view of the first mask provided in an embodiment of the present invention, referring to Figure 3-Figure 5 , the preparation method comprises:
[0054] S201, forming a reflective layer, an adhesive layer and a light-emitting conductive layer in sequence from bottom to top on the surface of the first substrate.
[0055] Among them, the anode metal layer 20 includes a reflective layer 22, an adhesive layer and a light-emitting conductive layer 24. The reflective layer 22 improves the light extraction efficiency of the LED by reflecting light. The reflective layer 22 can form a reflector in the electrode of the OLED chip, and by reflecting the light emitted by the light-emitting conductive layer 24, the absorption of light on the P electrode is reduced, thereby increasing the light extraction efficiency. At the same time, the use of the reflective layer 22 can also reduce the production cost when the electrode is evaporated. The adhesive layer 23 firmly connects the various components such as the chip, the electrode, and the packaging material together, ensuring the stability and reliability of the display screen while protecting the display screen from the influence of the external environment through insulation, thereby extending the service life. The light-emitting conductive layer 24 provides a positive current to excite the organic light-emitting material, so that the display screen emits light under the action of the organic light-emitting material. As an example, the material of the reflective layer 22 is Al, the material of the adhesive layer 23 is TiN, and the material of the light-emitting conductive layer 24 is ITO (transparent conductive indium tin oxide). The embodiment of the present invention does not specifically limit the material of the anode metal layer 20. The reflective layer 22, the adhesive layer 23 and the light-emitting conductive layer 24 are formed on the first substrate 10 to ensure the light-emitting performance of the display screen.
[0056] In one embodiment, if Figure 4 As shown in (a1), a reflective layer 22, an adhesive layer 23 and a light-emitting conductive layer 24 are formed on the surface of the first substrate 10 in sequence from bottom to top.
[0057] S202, aligning a first mask and a second mask having the same structure up and down, and setting them between the coating target and the first substrate.
[0058] Among them, the coating target material 12 deposits one or more layers of thin film on the base material by physical or chemical methods, the first mask 11 and the second mask have the same structure, and the first mask 11 and the second mask 12 have multiple hollow structures. When the first mask 11 and the second mask 12 are aligned up and down, the coating material can be deposited on the first substrate 10 through the hollow structure to form a mask layer 30. Two layers of masks aligned up and down are set to shield the first substrate 10, so as to facilitate the formation of an inclined ladder-shaped mask layer 30 on the surface of the first substrate 10.
[0059] In one embodiment, if Figure 4 As shown in (b1), the first mask 11 and the second mask 12 with the same structure are aligned up and down and arranged between the coating target 13 and the first substrate 10.
[0060] S203, controlling the first mask and the second mask to move relative to each other in the horizontal direction at a preset speed, and coating the first substrate at the same time, forming an inclined ladder-shaped mask layer on the surface of the anode metal layer away from the first substrate.
[0061] Among them, the preset speed is a pre-set speed for controlling the movement of the first mask 11 or the second mask 12, and the preset speed is related to the height of the mask layer 30. Since the first mask 11 and the second mask 12 are aligned up and down, while the first substrate 10 is coated, the first mask 11 and the second mask 12 move relative to each other in the horizontal direction. As the first mask 11 and the second mask 12 move, the overlapping area of the hollow structure of the first mask and the hollow structure of the second mask is reduced. At this time, the coating material deposited on the first substrate 10 is reduced. By continuously moving the first mask 11 and the second mask 12, the height of the mask layer 30 formed at different positions on the surface of the first substrate 10 is different, and a ladder-shaped mask layer 30 is formed on the surface of the first substrate 10. The moving direction of the first mask 11 and the second mask 12 can be set according to actual needs, and the embodiment of the present invention does not impose specific restrictions on this. As an example, the first mask 11 may be fixed and the second mask 12 may be moved horizontally. In other implementations, the second mask 12 may be fixed and the first mask 11 may be moved horizontally, or the first mask 11 and the second mask 12 may be moved horizontally in opposite directions. This embodiment of the present invention does not impose any specific limitation on this.
[0062] In one embodiment, if Figure 4 As shown in (c1), the first mask 11 and the second mask 12 are controlled to move relative to each other in the horizontal direction at a preset speed, and the first substrate 10 is plated at the same time to form an inclined ladder-shaped mask layer 30 on the surface of the anode metal layer 20 away from the first substrate 10.
[0063] S204 , forming a first photoresist layer above the mask layer.
[0064] In one embodiment, if Figure 4 As shown in (d1), a first photoresist layer 40 is formed on the mask layer 30.
[0065] S205 , patterning the first photoresist layer.
[0066] In one embodiment, if Figure 4 As shown in (e1), the first photoresist layer 40 is patterned.
[0067] S206, etching the mask layer and the anode metal layer exposed by the first photoresist layer to form at least two grooves of different depths on the surface of the anode metal layer away from the first substrate.
[0068] In one embodiment, if Figure 4 As shown in (f1), the mask layer 30 and the anode metal layer 20 exposed by the first photoresist layer 40 are etched to form at least two grooves 21 with different depths on the surface of the anode metal layer 20 away from the first substrate 10.
[0069] S207 , removing the first photoresist layer on the surface of the mask layer.
[0070] The first photoresist layer 40 is removed by physical or chemical means, so as to facilitate further processing of the mask layer 30 and the anode metal layer 20 to form the anode metal layer 20 with different heights.
[0071] In one embodiment, if Figure 4 As shown in (g1), the first photoresist layer 40 on the surface of the mask layer 30 is removed.
[0072] S208 , forming a second photoresist layer 50 on a surface of the mask layer 30 away from the first substrate 10 .
[0073] The second photoresist layer 50 covers the mask layer 30 and the surface of the groove 21. The second photoresist layer 50 covering the mask layer 30 and the surface of the groove 21 of the anode metal layer 20 is provided to provide a basis for the subsequent removal of the mask layer 30. The materials of the second photoresist layer 50 and the first photoresist layer 40 can be the same or different materials, and the embodiment of the present invention does not impose specific restrictions on this.
[0074] In one embodiment, if Figure 4 As shown in (h1), a second photoresist layer 50 is formed on a surface of the mask layer 30 which is away from the first substrate 10 .
[0075] S209, removing the second photoresist layer outside the groove.
[0076] The second photoresist layer 50 outside the groove 21 is removed so that the second photoresist layer 50 covers the surface of the groove 21 , and the groove 21 is protected when the mask layer 30 is removed later.
[0077] In one embodiment, if Figure 4 As shown in (i1), the second photoresist layer 50 outside the groove 21 is removed.
[0078] S210, removing the mask layer.
[0079] The mask layer 30 is removed, that is, the second photoresist layer 50 covering the surface of the groove 21 is retained to protect the groove 21. As an example, a higher etching gas is selected for etching the mask layer 30 than the anode metal layer 20, that is, the etching gas has a stronger etching ability to the mask layer 30, and basically does not etch the anode metal layer 20, and etches the medium to ensure the display performance of the display screen.
[0080] In one embodiment, if Figure 4 As shown in (j1), the mask layer 30 is removed.
[0081] S211, etching the anode metal layer not covered by the second photoresist layer.
[0082] When the anode metal layer 20 is etched, the second photoresist layer 50 covering the surface of the groove 21 is retained to protect the groove 21, and the anode metal layer 20 for display is retained.
[0083] In one embodiment, if Figure 4 As shown in (k1), the anode metal layer 20 not covered by the second photoresist layer 50 is etched.
[0084] S212, removing the second photoresist layer, and forming at least two anode metal layers with different heights on the surface of the first substrate.
[0085] Among them, at least two anode metal layers 20 with different heights are formed on the surface of the first substrate 10. At this time, the heights of the pixels are different, and the display screen can use the optical strong microcavity effect to improve the display performance of the display screen. As an example, the number of anode metal layers 20 can be 3 to meet the display requirements of three pixels of R, G, and B. In other embodiments, the anode metal layers 20 can also be set to other numbers, and the embodiment of the present invention does not specifically limit this.
[0086] In one embodiment, if Figure 4 As shown in (l1), the second photoresist layer 50 is removed, and at least two anode metal layers 20 with different heights are formed on the surface of the first substrate 10.
[0087] The anode preparation method of the display screen provided by the embodiment of the present invention forms an oblique ladder-shaped mask layer on the surface of the anode metal layer away from the first substrate, and forms at least two grooves of different depths on the surface of the anode metal layer away from the first substrate by etching the mask layer and the anode metal layer. After three etchings, at least two anode metal layers of different heights are formed on the surface of the first substrate. By further etching the mask layer and the anode metal layer, the height of the anode metal layer on the surface of the first substrate is different, and the height of the pixels is different at this time. The display screen can use the optical strong microcavity effect to improve the display performance of the display screen, and does not need to be prepared by three hard masks, further reducing costs and improving preparation efficiency.
[0088] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an anode of a display screen, characterized in that: include: Forming an oblique ladder-shaped mask layer on a surface of the anode metal layer away from the first substrate; forming a first photoresist layer above the mask layer; performing patterning on the first photoresist layer; The mask layer and the anode metal layer exposed by the first photoresist layer are etched to form at least two grooves with different depths on a surface of the anode metal layer away from the first substrate.
2. The method for preparing an anode of a display screen according to claim 1, characterized in that: Before forming an oblique ladder-shaped mask layer on the surface of the anode metal layer away from the first substrate, the method further includes: An anode metal layer is formed on the surface of the first substrate.
3. The method for preparing an anode of a display screen according to claim 1, characterized in that: A mask layer in an oblique ladder shape is formed on a surface of the anode metal layer away from the first substrate, comprising: Aligning a first mask and a second mask having the same structure up and down, and arranging them between the coating target and the first substrate; The first mask and the second mask are controlled to move relative to each other in the horizontal direction at a preset speed, and the first substrate is plated at the same time to form an inclined ladder-shaped mask layer on the surface of the anode metal layer away from the first substrate.
4. The method for preparing an anode of a display screen according to claim 1, characterized in that: After etching the mask layer and the anode metal layer exposed by the first photoresist layer to form at least two grooves with different depths on the surface of the anode metal layer away from the first substrate, the method further comprises: The first photoresist layer on the surface of the mask layer is removed.
5. The method for preparing an anode of a display screen according to claim 4, characterized in that: After removing the first photoresist layer on the surface of the mask layer, the method further includes: A second photoresist layer is formed on a surface of the mask layer away from the first substrate, wherein the second photoresist layer covers the mask layer and the surface of the groove.
6. The method for preparing an anode of a display screen according to claim 5, characterized in that: After forming a second photoresist layer on a surface of the mask layer away from the first substrate, the method further comprises: The second photoresist layer outside the groove is removed.
7. The method for preparing an anode of a display screen according to claim 6, characterized in that: After removing the second photoresist layer outside the groove, the method further includes: The mask layer is removed.
8. The method for preparing an anode of a display screen according to claim 7, characterized in that: After removing the mask layer, the method further includes: The anode metal layer not covered by the second photoresist layer is etched.
9. The method for preparing an anode of a display screen according to claim 8, characterized in that: After etching the anode metal layer not covered by the second photoresist layer, the method further comprises: The second photoresist layer is removed, and at least two anode metal layers with different heights are formed on the surface of the first substrate.
10. The method for preparing an anode of a display screen according to claim 2, characterized in that: Forming an anode metal layer on the surface of the first substrate comprises: A reflective layer, an adhesive layer and a light-emitting conductive layer are sequentially formed on the surface of the first substrate from bottom to top.
Citation Information
Cited By
Anode plate etching device
CN119997770A
Anode plate etching device
CN119997770B