Post-consumer recoverable colored polypropylene composition

By preparing a specific range of polypropylene color blends and combining with efficient sorting and washing processes, the purity, pollution and homogeneity of post-consumer recycling of polypropylene materials is solved, and high purity, low pollution and excellent processing properties are achieved. Polypropylene recycled material, suitable for a variety of applications.

CN118900757APending Publication Date: 2024-11-05BOREALIS AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029096.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-09-23
Filing Date
2023-03-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing post-consumer recycling of polypropylene materials has challenges in purity, contaminants, homogeneity, color consistency and processability, especially the residual benzene contamination and surface contamination that limit its application in injection molded products.

Method used

By a polypropylene blended color blend, the content ranges from 85.0 wt.-% to 95.0 wt.-% of crystalline components, 5.0 wt.-% to 15.0 wt.-% of soluble components, 2.0 wt.-% of soluble components, 2.0 wt.- % to 10.0 wt.-% total ethylene content, 93.0 wt.-% to 99.0 wt.-% propylene content, C2 content in the range of [C2]-3.4 wt.-% to [C2]-0.2 wt.-% Inside, a specific range of CIELAB color space is combined with a sorting system of near-infrared and optical sensors, a water washing and drying process is used to remove contaminants to obtain a high-purity, low-contamination polypropylene recovery stream.

Benefits of technology

Polypropylene recycling materials with high purity, low pollution, uniformity and high color consistency have excellent processability and mechanical properties. They are suitable for the manufacture of bottle caps, seals, containers and other products, reducing total carbon emissions and volatility. content of organic matter.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005052000160000061
    Figure BDA0005052000160000061
  • Figure BDA0005052000160000171
    Figure BDA0005052000160000171
  • Figure BDA0005052000160000172
    Figure BDA0005052000160000172
Patent Text Reader

Abstract

The present invention relates to a polypropylene color blend having (i) a crystalline fraction (CF) content in the range of from 85.0 wt.-% to 95.0 wt.-% as determined according to the CRYSTEXQC analysis; (ii) a soluble component (SF) content in the range of 5.0 to 15.0 wt.-%; (iii) the total ethylene content (C2) is in the range of from 2.0 wt.-% to 10.0 wt.-%; (iv) the crystalline fraction (CF) has a propylene content (C3 (CF)) in the range of 93.0 wt.-% to 99.0 wt.-% as determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy; (v) the crystalline component (CF) has an ethylene content (C2 (CF)) in the range of [C2]-3.4 wt.-% to [C2]-0.2 wt.-% as determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, where [C2] is the total ethylene content (C2) defined in (iii); (vi) a CIELAB color space (L * a * b *), as determined according to DIN EN ISO 11664-4: L * is from 30.0 to 73.0; a * is from-10 to 25; b * is-5 to 20. The invention also relates to a process for obtaining the above polypropylene color blend and its use in home applications, automotive applications, electrical appliances, packaging or wire and cable applications. The invention also relates to products prepared from the polypropylene color-mixed blend, such as bottle caps, sealing elements, bottles, containers, automobile accessories and wire and cable supplies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to mixed color polypropylene blends from post-consumer recycle (PCR). Background Art

[0002] The challenge of dealing with the accumulated plastic waste and the corresponding environmental issues have received a lot of attention from the public and the industry. Therefore, the recycling of plastic materials has become an important topic, where plastic waste can be converted into a valuable resource for new plastic products. Therefore, environmental and economic aspects can be combined when recycling and reusing plastic materials.

[0003] Although the recycling of plastic materials has begun since the mid-1990s through the implementation of collection systems that allow a more targeted collection of plastic materials and their separation from other household waste, the reuse of plastic materials from plastic waste is still limited. So-called post-consumer recycled (PCR) plastic materials usually contain a mixture of different plastics and several contaminating materials. Methods for further purification of post-consumer recycled (PCR) plastic materials have been developed.

[0004] Many attempts have been made to purify recycling streams from post-consumer plastic waste. Among these measures, washing, screening, aeration, distillation, etc. can be mentioned. For example, WO2018 / 046578A1 discloses a process for producing polyolefin recyclates from mixed-color polyolefin waste (including packaging waste), which process comprises washing the waste with water cooling, then washing with an alkaline medium at 60°C, and then flake color sorting to obtain a color-sorted monopolyolefin-rich fraction.

[0005] US 5,767,230 A describes a process comprising contacting a PCR polyolefin sheet containing volatile impurities with a heated gas at a superficial velocity sufficient to reduce the volatile impurities (such as odor active substances). However, contamination with residual amounts of benzene has proven to be a problem so far. The source of residual benzene in post-consumer recyclate remains unclear, but it poses an obstacle to end uses in areas such as medical packaging, food packaging, etc. Residual benzene (i.e. trace amounts of benzene) poses a particular problem because odor testing by sniffing experiments becomes impossible. Therefore, end uses that have certain requirements for odor will be hindered.

[0006] WO 2020 / 182435 A1 discloses a polymer composition, which is composed of 50-90wt% recycled polypropylene; 4-50wt% talc; 0-10wt% additives; wherein the additive is selected from polyethylene (PE), maleic anhydride grafted PE (PEMA), maleic anhydride, grafted PP (PP-MA), stabilizer, peroxide, calcium oxide (CaO) or colorant; wherein the talc has a D less than 4 microns 50 (ISO 13317-3), and wt% is relative to the total weight of the polymer composition.

[0007] As another known problem, recyclates suffer from moderate homogeneity, which manifests itself in surface contamination occurring in injection molded products.

[0008] Post-consumer polypropylene-based recyclate (PP-PCR) produced by mechanical recycling processes remains challenging in meeting certain requirements, such as purity, contaminants, bright / white color, odor, quality consistency, batch-to-batch consistency, and homogeneity.

[0009] Therefore, there is still a strong need for recycled materials with properties as close as possible to the original resin. In particular, the object of the present invention is to provide PP-PCR materials that are superior to existing materials in terms of high product purity with respect to polypropylene content, low contaminant content, brighter grey color, low emissions (such as total carbon emissions, VOC, FOG), high color consistency, high homogeneity, high tensile strength and good processability. Summary of the invention

[0010] The problem underlying the present invention is to provide a post-consumer recycled polypropylene composition which solves the above mentioned needs and drawbacks.

[0011] Therefore, the present invention provides a polypropylene mixed color blend having

[0012] (i) a crystalline component (CF) content, determined according to CRYSTEXQC analysis, as determined herein, in the range of 85.0 wt.-% to 95.0 wt.-%,

[0013] (ii) a soluble fraction (SF) content, determined according to CRYSTEXQC analysis, as determined herein, in the range of 5.0 wt.-% to 15.0 wt.-%,

[0014] (iii) a total ethylene content (C2), determined according to CRYSTEXQC analysis, as determined herein, in the range of 2.0 wt.-% to 10.0 wt.-%,

[0015] (iv) the crystalline portion (CF) has a propylene content (C3(CF)) determined by quantitative 13 FT-IR spectroscopy calibrated with C-NMR spectroscopy, as determined herein, in the range of 93.0 wt.-% to 99.0 wt.-%;

[0016] (v) the crystalline fraction (CF) has an ethylene content (C2(CF)) determined by quantitative 13 % to [C2]-0.2 wt.-%, wherein [C2] is the total ethylene content (C2) as defined in (iii),

[0017] (vi) CIELAB color space (L*a*b*), measured according to DIN EN ISO 11664-4, as described herein, is:

[0018] L* is 30.0 to 73.0;

[0019] a* is -10 to 25;

[0020] b* is -5 to 20.

[0021] The present invention also provides a method for recycling polypropylene mixed color material, the method comprising the following steps:

[0022] a) providing a mixed plastic recycling stream (A);

[0023] b) screening the mixed plastic recycling stream (A) to produce a screened mixed plastic recycling stream (B) having only articles having a longest dimension in the range of 30 mm to 400 mm;

[0024] c) sorting the screened mixed plastic recycling stream (B) by one or more sorting systems including near infrared (NIR) and optical sensors, wherein the screened mixed plastic recycling stream (B) is sorted at least by color and polymer type, thereby producing a sorted mixed color polypropylene recycling stream (CM), which will be subjected to step d) and subsequent steps;

[0025] d) chopping the sorted mixed color polypropylene recycling stream (CM) to form a flake mixed color polypropylene recycling stream (D);

[0026] e) washing the flake mixed color polypropylene recovery stream (D) with a first water washing solution (W1) without inputting heat energy, thereby producing a first suspended polypropylene recovery stream (E);

[0027] f) removing at least a portion of the first aqueous washing solution (W1) from the first suspended polypropylene recovery stream (E) to obtain a first washed polypropylene recovery stream (F);

[0028] g) washing the first washed polypropylene recovery stream (F) with a second aqueous washing solution (W2) to produce a second suspended polypropylene recovery stream (G), wherein sufficient thermal energy is introduced into the second suspended polypropylene recovery stream (G) to provide a temperature in the range of 65° C. to 95° C. during washing;

[0029] h) removing the second aqueous wash solution (W2) and any material not floating on the surface of the second aqueous wash solution from the second suspended polypropylene recovery stream (G) to obtain a second washed polypropylene recovery stream (H); and

[0030] i) drying the second washed polypropylene recycle stream (H) thereby obtaining a dried polypropylene recycle stream (I) comprising the polypropylene melange blend according to the present invention.

[0031] The present invention also provides articles comprising the polypropylene mixed color blend of the present invention, wherein the polypropylene mixed color blend preferably accounts for at least 85wt.-%, more preferably at least 90wt.-%, and even more preferably at least 93wt.-% of the components used to make the article. These articles are particularly suitable for making bottle caps, seals, bottles, containers, automotive products and wire and cable products.

[0032] The polypropylene mixed color blend according to the present invention may preferably further comprise at least one virgin polypropylene and / or another recycled polypropylene to form a blend, which is used for manufacturing the above-mentioned articles. DETAILED DESCRIPTION

[0033] For the purposes of this specification and the subsequent claims, the term "recycled waste" is used to refer to materials recovered from post-consumer waste, rather than virgin polymers and / or materials. Post-consumer waste refers to items that have completed at least their first use cycle (or life cycle), i.e., have served their first purpose. The term "virgin" refers to newly produced materials and / or items prior to first use, which have not yet been recycled. The term "recycled material", as used herein, refers to materials that have been reprocessed from "recycled waste".

[0034] Blend refers to a mixture of two or more components, at least one of which is a polymer. Typically, the blend can be prepared by mixing two or more components. Suitable mixing methods are known in the art. If such a blend includes virgin material, the virgin material is preferably a polypropylene comprising 90 wt-% of a reactor-prepared polypropylene material and optionally carbon black. Virgin material is a polymeric material that has not yet been recycled.

[0035] For the purpose of this specification and the subsequent claims, the term "polypropylene mixed color blend" refers to a polymer material which, in addition to other polymer components of any nature, mainly comprises monomers derived from propylene. For example, these polymer components can be derived from monomer units derived from α-olefins (such as ethylene, butene, octene, etc.), styrene derivatives (such as vinyl styrene), substituted and unsubstituted acrylic acid esters, substituted and unsubstituted methacrylic acid esters.

[0036] The polymer material can be quantitatively 13 C{ 1 H} NMR measurements were performed in polypropylene mixed color blends. The quantitative 13 C{ 1 In the H}NMR measurement, different units in the polymer chain can be distinguished and quantified. These units are propylene units (C3 units), units with 2, 4 and 6 carbons and units with 7 carbon atoms. Therefore, units with 2 carbon atoms (C2 units) can be distinguished as isolated C2 units and continuous C2 units in the NMR spectrum, which shows that the polymer material contains ethylene-based polymers. The polypropylene mixed color blend according to the present invention generally includes a low amount of ethylene-based polymer components.

[0037] Typically, other components may be present, such as fillers, including organic and inorganic fillers (eg talc, chalk, carbon black) and other pigments (eg TiO2) as well as paper and cellulose.

[0038] The present invention has found that the above mentioned objects can be achieved by means of the above defined polypropylene mixed color blends.

[0039] The polypropylene melange blend according to the present invention preferably has a crystalline component (CF) content, determined according to CRYSTEX QC analysis, in the range of 85.0 to 93.0 wt.-%, more preferably in the range of 88.0 to 93.0 wt.-%.

[0040] The crystalline component (CF) of the polypropylene mixed color blend according to the present invention preferably has a propylene content (C3(CF)) determined by the quantitative 13 The content of iodine is determined by FT-IR spectroscopy calibrated with C-NMR spectroscopy in the range of 94.0 wt.-% to 99.0 wt.-%, more preferably in the range of 95.0 wt.-% to 98.5 wt.-%.

[0041] The crystalline fraction (CF) of the polypropylene mixed color blend according to the present invention preferably has a total ethylene content (C2) determined by the quantitative 13The FT-IR spectroscopy calibrated with C-NMR spectroscopy, as determined herein, is in the range of [C2]-3.0 wt.-% to [C2]-0.6 wt.-%, more preferably in the range of [C2]-2.4 wt.-% to [C2]-1.2 wt.-%, wherein [C2] is the total ethylene content (C2) determined according to CRYSTEXQC analysis.

[0042] The polypropylene mixed color blend preferably has a total ethylene content (C2), determined according to CRYSTEX QC analysis, in the range of 2.5 to 8.0 wt.-%, and more preferably in the range of 3.0 to 6 wt.-%, based on the total weight of the polypropylene mixed color blend.

[0043] The polypropylene mixed color blend according to the present invention preferably has a CIELAB color space (L*a*b*), measured according to DIN EN ISO 11664-4, as described herein, of:

[0044] -L* is 40 to 65;

[0045] -a* is -8 to 20;

[0046] -b* is -3 to 15,

[0047] Each of the abovementioned ranges for L*, a* and b* can be combined with one another independently.

[0048] The polypropylene melange blend according to the present invention preferably has a soluble fraction (SF), analyzed by CRYSTEX QC, in the range of 6.0 to 11.0 wt.-%, more preferably in the range of 7.0 to 10.0 wt.-%.

[0049] The polypropylene mixed color blend according to the present invention preferably has an ethylene content in the soluble fraction (C2(SF)) obtained by CRYSTEX QC analysis, determined by quantitative 13 The FT-IR spectrum calibrated with the C-NMR spectrum is 21.0 to 28.0 wt.-%, more preferably 22.0 to 27.0 wt.-%.

[0050] The polypropylene mixed color blend according to the present invention preferably has an inorganic residue, as measured by calcination analysis (TGA) according to DIN ISO 1172: 1996, of 0.1 wt.-% to less than 2.0 wt.-%, more preferably of 0.3 wt.-% to 1.5 wt.-%, relative to the total weight of the polypropylene mixed color blend. The result of the calcination analysis (TGA) is also referred to herein as the ash content.

[0051] The polypropylene mixed color blend according to the present invention preferably has a total carbon emission, measured by HS GC-FID according to VDA 277, of 1.0 to 30 μg carbon / g, more preferably 5.0 to 25 μg carbon / g, relative to the weight of the polypropylene mixed color blend.

[0052] The polypropylene mixed color blend according to the present invention preferably has a total volatile organic content (VOC), determined by HS GC-FID according to VDA 278, relative to the weight of the polypropylene mixed color blend, of 10 μg / g to 150 μg / g, more preferably of 20 μg / g to 120 μg / g, even more preferably of 20 μg / g to 80 μg / g.

[0053] The polypropylene mixed color blend according to the present invention preferably has a total condensable organic content (FOG), determined by HS GC-FID according to VDA 278, of 20 to 450 μg / g, more preferably 30 to 420 μg / g, relative to the weight of the polypropylene mixed color blend.

[0054] The polypropylene mixed color blend according to the present invention preferably has an odor of 5.0 or less (VDA270-B3), more preferably 4.8 or less. It should be understood that many commercial recycled grades that do not report odor are actually even worse because odor testing according to VDA270 is prohibited due to the presence of problematic substances.

[0055] The polypropylene mixed color blend according to the present invention preferably has a large amplitude oscillatory shear-nonlinear coefficient (LAOS-NLF), measured at 190° C., at an angular frequency of 0.628 rad / s and a strain of 1000%, in the range of 1.5 to 3.5, wherein

[0056]

[0057] in

[0058] G1' is the first-order Fourier coefficient

[0059] G3' is the third-order Fourier coefficient

[0060] Without wishing to be bound by theory, it is believed that the processing of the polymer contributes to the branching initiated by the enclosed contaminants. LAOS-NLF can be influenced by selecting the raw materials so that about 10 wt.-% of the material is soft polypropylene. It should be understood that several regions operate collection stations that collect highly consumable pre-sorted plastics. This high-value plastic stream is commercially available and allows upgrading other low-quality streams (e.g., by softer polypropylene blends) from other waste disposal resources.

[0061] The polypropylene mixed color blend according to the present invention preferably has a tensile modulus (ISO527-2, crosshead speed of 1 mm / min; 23°C), using injection molded test specimens as described in EN ISO 1873-2 (dog bone shape, 4 mm thick), of at least 1200 MPa, more preferably at least 1250 MPa, even more preferably at least 1300 MPa. This relatively high flexural modulus is due to the relatively low content of rubbery and plastidic materials in the blend.

[0062] The polypropylene mixed color blend according to the present invention preferably has a tensile modulus in the range of 1200 to 1500 MPa, more preferably in the range of 1250 to 1480 MPa.

[0063] The polypropylene melange blends according to the present invention preferably have a tensile strain at break, measured according to ISO 527-2 and as described in the experimental part below, in the range of 5 to 350%, more preferably in the range of 10 to 200%, even more preferably in the range of 15 to 150%.

[0064] The polypropylene mixed color blend according to the present invention preferably has a Charpy impact strength, measured according to ISO 179-1 / 1eA at 23° C. and as described in the experimental part below, at 3.5 kJ / m 2 Up to 12.0 kJ / m 2 In the range of 4.0 kJ / m 2 Up to 10.0kJ / m 2 In the range of 4.5 kJ / m 2 Up to 9kJ / m 2 within the range.

[0065] The polypropylene mixed color blend according to the present invention preferably has an intrinsic viscosity of the soluble fraction (IV(SF)), determined according to CRYSTEX QC analysis and as determined in the experimental part below, in the range of 1.0 dl / g to 2.2 dl / g, more preferably in the range of 1.2 dl / g to 2.1 dl / g, more preferably in the range of 1.3 dl / g to 2.0 dl / g.

[0066] The polypropylene mixed color blend according to the present invention preferably has a shear thinning factor (STF) value, which is defined as the ratio of the complex viscosity of 0.05 rad / s (η(0.05)) to the complex viscosity of 300 rad / s (η(300)) at 230°C in the frequency range of 0.01 rad / s to 628 rad / s according to ISO 6721-1 and ISO 6721-10, which is in the range of 7.5 to 15, more preferably in the range of 8.0 to 13. STF is a rheological index that indicates the molecular weight breadth of a polymer. The determination of STF will be described in the following experimental part. The higher the STF value, the wider the molecular weight breadth of the material, which is beneficial to the processability of the material.

[0067] The polypropylene mixed color blend according to the present invention preferably has a melt flow rate MFR at 230°C. 2.16 , measured according to ISO1133, is at least 5 g / 10 min, more preferably at least 10 g / 10 min. 2.16 It is preferably not more than 50 g / 10 min, more preferably not more than 30 g / 10 min.

[0068] For some applications, the polypropylene mixed color blend is preferably obtained by visbreaking using peroxide. In these cases, the MFR 2.16 It is preferably at least 50 g / 10 min, more preferably at least 100 g / 10 min, even more preferably at least 150 g / 10 min.

[0069] The visbreaking step can be preferably carried out by using peroxides, mixtures of peroxides or hydroxylamine esters or mercaptan compounds as a source of free radicals (visbreaking agent), or by pure thermal degradation. Decomposition products of the visbreaking process may be present in the resulting blend. It should be understood that decomposition products of the visbreaking process (as is commonly used in the art for the original material) are not considered to be impurities.

[0070] The process of visbreaking is known in the art and can be carried out as described, for example, in WO 2021 / 260053 A1.

[0071] The polypropylene mixed color blend according to the present invention preferably has a carbon content of 900 kg / m 3 Up to 940kg / m 3 , more preferably 905kg / m 3 Up to 935kg / m 3 , even more preferably 910 kg / m 3 Up to 930kg / m 3 density.

[0072] The polypropylene mixed color blend according to the present invention is preferably obtained from post-consumer recycle (PCR), preferably from 100% PCR material. Such PCR material is usually obtained from consumer waste streams, for example from traditional collection systems implemented by the European Union (such as extended producer responsibility schemes, EPR schemes). PCR material may also originate from municipal solid waste outside the EPR collection system.

[0073] According to the present invention, the raw material for obtaining the polypropylene mixed color mixture can be selected from a variety of municipal solid waste (MSS, also commonly known as residual waste, black box waste) to components produced from raw materials based on extended producer responsibility (EPR), such as ARA 414 components from Altstoff Recycling, Austria, or DSD 324 components from German producer responsibility organizations (such as DSD-Duales System Holding Interzero Reclay).

[0074] It is preferred that the polypropylene mixed color blend according to the present invention comprises at least 95.0 wt.-%, more preferably at least 96 wt.-%, even more preferably at least 97 wt.-% from post-consumer waste.

[0075] The above object can also be achieved by the above method for recycling polypropylene mixed color materials, which comprises steps a) to i). In other words, the polypropylene mixed color blend according to the present invention can be obtained or has been obtained preferably by the above method or the preferred method described below.

[0076] According to step c), the screened mixed plastic recycling stream (B) can preferably be further sorted according to the product form. In this case, artificial intelligence sorting systems (which are commercially available, for example from Tomra systems) can also be used for sorting according to application type (MFR) or specific objects. In the sorting step c), white and natural waste materials are preferably sorted out, so that essentially only non-white and / or non-natural colored waste remains in one or more sorted mixed color polypropylene recycling streams (CM).

[0077] By carrying out the sorting step c), preferably one or more sorted mixed color polypropylene recycling streams (CM) are produced. This can preferably be achieved by removing white and natural polypropylene items as well as non-polypropylene items. In this case, "natural" means that the items have a natural color. This means that the items are essentially free of pigments (including carbon black) or colorants such as dyes or inks. On the other hand, "white" means that the items contain white pigments. The same logic applies to the sorting of flakes described in the following step k).

[0078] In step f), preferably substantially all of the first aqueous wash solution (W1) is removed from the first suspended polypropylene polyolefin recovery stream (E) to obtain said first washed polypropylene polyolefin recovery stream (F).

[0079] In step h), the second aqueous wash solution (W2) and any material not floating on the surface of the second aqueous wash solution are preferably removed by a density separation step.

[0080] The method of the present invention may further comprise at least one of the following steps:

[0081] j) separating the dried polypropylene recovery stream (I) obtained from step i) into a light component and a heavy component polypropylene recovery stream (J);

[0082] k) further sorting the heavy component polypropylene recovery stream (J), or in the absence of step j), sorting the dried polypropylene recovery stream (I), using one or more optical sorters equipped with NIR and / or optical sensors to sort out one or more target polypropylenes by removing any flakes containing materials other than the one or more target polypropylenes or flakes of undesirable colors (such as white, black, etc.) to obtain a purified polypropylene recovery stream (k);

[0083] l) subjecting the purified polypropylene recovery stream (K) to melt extrusion (preferably pelletization), preferably wherein the additive (Ad) is added in the molten state, to form an extruded (preferably pelletized) recovered polypropylene product (L);

[0084] m) aerating the recycled polypropylene product (L) or, in the absence of step 1), aerating the purified polypropylene recycling stream (K) to remove volatile organic compounds, thereby producing an aerated recycled polypropylene product (M), which is either an aerated extruded (preferably pelletized) recycled polypropylene product (M1) or an aerated recycled polypropylene flake (M2);

[0085] The order of step 1) and step m) can be interchanged, so that the purified polypropylene recycling stream (K) is first aerated to form an aerated recycled polypropylene sheet (M2), which is subsequently extruded, preferably wherein the additive (Ad) is added in the molten state, to form an extruded (preferably pelletized) aerated recycled polypropylene product (M3), which is a polypropylene mixed color blend according to the present invention.

[0086] In step j), the separation can preferably be performed by an air sifter. The separation can also be performed based on the aerodynamic properties of particles (such as flakes), for example, separating thin and light flexible flakes from heavy and thick rigid flakes.

[0087] After the above step j), a screening step j1) may be performed, wherein the dried polypropylene recovery stream (I) is screened to remove fines, producing a screened polypropylene recovery stream (J1), which may subsequently be subjected to the above optional step k). In this screening step j1), fines preferably having a size of 2.5 mm or less are removed.

[0088] Furthermore, the present invention relates to articles made from the polypropylene mixed color blend according to the present invention, wherein the polypropylene mixed color blend preferably represents at least 85 wt.-%, more preferably at least 90 wt.-%, even more preferably at least 93 wt.-% of the components used to make the article. The above-mentioned residual components may include additives such as antioxidants, stabilizers, carbon black (optionally in the form of a masterbatch), pigments, colorants (such as dyes or inks).

[0089] According to the present invention, the article can be selected from bottle caps, seals, bottles, containers, automotive products, and wire and cable products.

[0090] The present invention also relates to a blend containing the polypropylene mixed color blend according to the present invention, at least one virgin polypropylene and / or another recycled polypropylene. The virgin polypropylene may be selected from heterophasic polypropylene, random propylene copolymers and propylene homopolymers. The other recycled polypropylene may be the same as or different from the polypropylene mixed color blend according to the present invention. It may also be derived from commercial sources, as described above.

[0091] The present invention also relates to the use of the polypropylene mixed color blend according to the present invention in household applications, automotive applications, electrical appliances, packaging or wire and cable applications.

[0092] Test Method

[0093] Unless otherwise defined, the following definitions of terms and test methods apply to the above general description of the invention as well as the following examples.

[0094] a) Melt flow rate

[0095] The melt flow rate (MFR) is determined according to ISO 1133 and is expressed in g / 10 min. The MFR is an indicator of the fluidity and thus the processability of the polymer. The higher the melt flow rate, the lower the viscosity of the polymer. Here, MFR2 is determined at a temperature of 230°C and a load of 2.16 kg.

[0096] b) Isotacticity and comonomer content of polypropylene

[0097] Quantification of microstructure by NMR spectroscopy (calibration only)

[0098] Calibration was performed using quantitative nuclear magnetic resonance (NMR) spectroscopy.

[0099] Using a Bruker Avance Neo 400 NMR spectrometer, 1 H and 13 C, respectively, were operated at 400.15 MHz and 100.62 MHz, and the quantitative 13 C{ 1 H} NMR spectroscopy. Nitrogen was used for all pneumatics and the temperature was 125 °C. 13 All spectra were recorded with a 10 mm extended temperature probe optimized for 1 0.5 °C. About 200 mg of material was dissolved in about 3 mL of 1,2-tetrachloroethane-d2 (TCE-d2) along with about 3 mg of BHT (2,6-di-tert-butyl-4-methylphenol, CAS 128-37-0) and chromium (III) acetylacetonate (Cr(acac)3) to give a 60 mM solution of the relaxation agent in the solvent as described in G. Singh, A. Kothari, V. Gupta, Polymer Testing 2009, 28(5), 475.

[0100] To ensure that the solution is uniform, the NMR tube is further heated in a rotary furnace for at least 1 hour after preliminary sample preparation in a heat block. After the magnet is inserted, the tube rotates at a frequency of 10 Hz. This setting is selected mainly to obtain the high sensitivity and quantification required for accurate ethylene content quantification. As described in Z. Zhou, R. Kuemmerle, X. Qiu, D. Redwine, R. Cong, A. Taha, D. Baugh, B. Winniford, J. Mag. Reson. 187 (2007) 225 and V. Busico, P. Carbonniere, R. Cipullo, C. Pellecchia, J. Severn, G. Talarico, Macromol. Rapid Commun. 2007, 28, 1128, using an optimized flip angle, 1 s cycle delay and a double-layer WALTZ16 decoupling scheme, in the absence of NOE, a standard single pulse excitation is used. A total of 6144 (6k) transients are obtained for each spectrum.

[0101] Quantitative 13 C{ 1 The H} NMR spectra were processed, integrated, and the relevant quantitative properties were determined from the integration. All chemical shifts were indirectly referenced to the central methylene of the ethylene segment (EEE) at 30.00 ppm using the chemical shift of the solvent. This approach allows similar references to be made even in the absence of this structural unit.

[0102] Characteristic signals corresponding to ethylene incorporation were observed (as described in Cheng, HN, Macromolecules 1984, 17, 1950) and the comonomer fraction was calculated as the ratio of ethylene in the polymer relative to all monomers in the polymer:

[0103] fE=(E / (P+E)

[0104] The comonomer fraction was calculated using the method of WJ. Wang and S. Zhu, Macromolecules 2000, 33 1157. 13 C{ 1 Quantification is performed by integration of multiple signals over the entire spectral region in the H} spectrum. The integration region is fine-tuned to improve applicability over the entire range of comonomer contents encountered.

[0105] The mole percentage of comonomer incorporation is calculated from the mole fraction:

[0106] E[mol%]=100*fE

[0107] The weight percent of comonomer incorporation is calculated from the mole fraction:

[0108] E[wt%]=100*(fE*28.06) / ((fE*28.06)+((1-fE)*42.08)).

[0109] c) Crystex analysis, crystalline fraction (CF) and soluble fraction (SF)

[0110] The crystalline fraction (CF) and soluble fraction (SF) of the PCR polypropylene composition as well as the ethylene content and intrinsic viscosity of each part were analyzed using a CRYSTEX instrument (Polymer Char, Valencia, Spain) according to ISO 6427 Appendix B. Details of the technology and method can be found in the literature (Ljiljana Jeremic, Andreas Albrecht, Martina Sandholzer & Markus Gahleitner (2020) Rapid characterization of high-impact ethylene-propylene copolymer composition by crystallization extraction separation: comparability to standard separation methods, International Journal of Polymer Analysis and Characterization, 25: 8, 581-596).

[0111] The crystalline and amorphous components were separated by a temperature cycle of dissolution at 160° C., crystallization at 40° C. and redissolution in 1,2,4-trichlorobenzene at 160° C. Quantification of SF and CF and determination of the ethylene content (C2) were achieved by an integrated infrared detector (IR4), and the intrinsic viscosity (IV) was determined using an online 2-capillary viscometer.

[0112] The IR4 detector is a multi-wavelength detector that detects the vibration of CH3 at two different wavelengths (at about 2960 cm -1 centered) and CH stretching vibration (2700cm -1 -3000cm -1 )) measure IR absorbance, these two different bands are used to determine the concentration and ethylene content in ethylene-propylene copolymers. A series of known ethylene contents ranging from 2 wt.-% to 69 wt.-% (given by 13 C-NMR measurement) and calibrated the IR4 detector in a concentration range of 2 mg / ml to 13 mg / ml for each. In order to simultaneously meet the two characteristics (concentration and ethylene content) of the various polymer concentrations expected in Crystex analysis, the following calibration equation was applied:

[0113] Conc=a+b*Abs(CH)+c*(Abs(CH)) 2 +d*Abs(CH3)+e*(Abs(CH3) 2+f*Abs(CH)*Abs(CH3)

[0114] CH3 / 1000C=a+b*Abs(CH)+c*Abs(CH3)+d*(Abs(CH3) / Abs(CH))+e*(Abs(CH3) / Abs(CH)) 2

[0115] Constants a to e in Equation 1 and constants a to f in Equation 2 were determined by least squares regression analysis.

[0116] The CH3 / 1000C is converted to ethylene content wt.-% using the following relationship:

[0117] Wt.-% (ethylene in EP copolymer) = 100-CH3 / 1000TC*0.3

[0118] The intrinsic viscosity (IV) of the PCR polypropylene composition and its soluble and crystalline components was determined with an online 2-capillary viscometer and correlated to the corresponding IV determined with the standard method in decalin according to ISO 1628-3. The calibration was done using various EP PP copolymers with IV = 2-4 dL / g. The calibration curve determined was linear:

[0119] IV(dL / g)=a*Vsp / c

[0120] The samples to be analyzed were weighed at a concentration of 10 to 20 mg / ml. To avoid injection of possible gels and / or polymers (such as PET and PA) not soluble in TCB at 160°C, the weighed samples were loaded into a stainless steel mesh (MW 0,077 / D 0,05 mm).

[0121] After the vial was automatically filled with 1,2,4-TCB containing 250 mg / l 2,6-tert-butyl-4-methylphenol (BHT) as an antioxidant, the sample was dissolved at 160°C until complete dissolution was achieved, which usually took 60 min, with continuous stirring at 400 rpm. In order to avoid sample degradation, the polymer solution was protected under N2 atmosphere during the dissolution process.

[0122] A certain volume of sample solution is injected into a column filled with an inert carrier, where crystallization of the sample and separation of the soluble and crystalline components are carried out. This process is repeated twice. In the first injection, the entire sample is measured at high temperature and IV [dl / g] and C2 [wt.-%] of the PP composition are determined. In the second injection, the soluble components (at low temperature) and the crystalline components (at high temperature) in the crystallization cycle are measured (wt.-% SF, wt.-% CF, wt.-% C2, IV), where wt.-% CF is calculated as follows:

[0123] wt.-%CF=100-wt.-%SF

[0124] d) Cross-fractionation chromatography

[0125] The chemical composition distribution and the molecular weight distribution at a specific elution temperature (polymer crystallinity in solution) and the corresponding molecular weight averages (Mn, Mw and Mv) were determined by fully automated cross-fractionation chromatography (CFC) as described by Ortin A., Monrabal B., Sancho-Tello J., Macromol. Symp., 2007, 257, 13-28.

[0126] Cross-fractionation chromatography (TREF×SEC) was performed using a CFC instrument (PolymerChar, Valencia, Spain). The concentration was monitored using a quad-band IR5 infrared detector (PolymerChar, Valencia, Spain). The polymer was dissolved at a concentration of about 1 mg / ml at 160°C for 150 minutes.

[0127] In order to avoid injection of possible gels and / or polymers (like PET and PA) that are not soluble in TCB at 160°C, the weighed samples were loaded into a stainless steel mesh (MW 0,077 / D 0,05 mmm).

[0128] Once the sample was completely dissolved, a 0.5 ml aliquot was loaded into a TREF column and stabilized for a period of time at 110° C. The polymer was crystallized and precipitated to a temperature of 30° C. by applying a constant cooling rate of 0.1° C. / min. A discontinuous elution process was performed using the following temperature steps: (35, 40, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 103, 106, 109, 112, 115, 117, 119, 121, 123, 125, 127, 130, 135, and 140).

[0129] In the second dimension GPC analysis, three PL Olexis columns and one Olexis Guard column from Agilent (ChurchStretton, UK) were used as stationary phases. 1,2,4-Trichlorobenzene (TCB, stabilized with 250 mg / L 2,6-di-tert-butyl-4-methylphenol) was used as the eluent at a constant flow rate of 1 mL / min at 150 °C. The column set was calibrated using a universal calibration method (according to ISO 16014-2:2003) using at least 15 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11500 kg / mol. The following Mark Houwink constants were used to convert PS molecular weights to PP molecular weight equivalents.

[0130] K PS =19x 10 -3 mL / g, α PS =0.655

[0131] K PP =19x 10 -3 mL / g, α PP =0.725

[0132] A third order polynomial fit was used to fit the calibration data. Data processing was performed using the PolymerChar software provided with the CFC instrument.

[0133] e) Tensile modulus and tensile strain at break

[0134] The tensile modulus and tensile strain at break were measured according to ISO 527-2 (crosshead speed = 1 mm / min; test speed 50 mm / min at 23° C.) using injection molded specimens as described in EN ISO 1873-2 (dog bone shape, 4 mm thick). The specimens were measured after a conditioning time of 96 h.

[0135] f) Impact strength (Charpy NIS)

[0136] Impact strength was determined as notched Charpy impact strength (1 eA) according to ISO 179-1 eA at +23° C. on 80×10×4 mm injection molded specimens prepared according to EN ISO 1873-2 (non-instrumented, ISO 179-1 at +23° C.).

[0137] g) Inorganic residues

[0138] Inorganic residues were measured by TGA with a Perkin Elmer TGA 8000 according to DIN ISO 1172:1996. About 10-20 mg of material was placed in a platinum pan. The temperature was equilibrated at 50°C for 10 min and then raised to 950°C under nitrogen at a heating rate of 20°C / min. The ash content was estimated as wt% at 850°C.

[0139] h) CIELAB color space (L*a*b*)

[0140] In the CIEL*a*b* uniform color space, the color coordinates are: L*—lightness coordinate; a*—red / green coordinate, where +a* represents red and -a* represents green; b*—yellow / blue coordinate, where +b* represents yellow and -b* represents blue. The L*, a*, and b* axes define the three-dimensional CIE color space. Standard Konica / Minolta color measurement instrument CM-3700A.

[0141] i) Odor (VDA270-B3)

[0142] VDA 270 is used to determine the odor properties of materials used in motor vehicle interiors. In this study, the odor was determined according to VDA 270 (2018) variant B3. Each assessor evaluated the odor of their respective sample according to VDA 270 with the can lid opened as little as possible. The six-point rating scale consists of the following grades: 1: not perceptible, 2: perceptible but not disturbing, 3: clearly perceptible but not disturbing, 4: disturbing, 5: very disturbing, 6: unacceptable. The assessors remained calm during the assessment and were not allowed to bias each other by discussing individual results during the test. They were also not allowed to adjust their assessment after testing another sample. For statistical reasons (and accepted by VDA 270), the assessors had to use integer ratings in their assessments. The odor rating was therefore based on the average of all individual assessments and rounded to an integer.

[0143] j) Total organic emissions from non-metallic materials (VDA 277, January 1995)

[0144] The following method description provides the skilled reader with an overview of the relevant parameters. In case of doubt, only the original method can be used for comparison of results. Standards comparable to VDA 277 are PV3341 (Volkswagen) and VCS1027,2749 (Volvo).

[0145] VDA 277 is intended for the determination of organic compounds from non-metallic materials that are relevant for vehicle interiors. It allows the determination of the emission potential using static headspace techniques in combination with gas chromatography.

[0146] For transport and storage, the samples were packed tightly in aluminum-coated polyethylene bags. If not described elsewhere, the samples were neither stored in the open air nor pre-treated in any other way before analysis. Before weighing the samples, the injection molded parts were cut into smaller pieces without the risk of heating the samples. The pellets were weighed directly without an additional cutting step.

[0147] Then take 2g sample respectively and put it into 20ml headspace vial, and close it tightly. Before the subsequent GC analysis, heat the vial immediately. At 120℃ (+ / -1℃), incubate for 5 hours (+ / -5min) in the headspace sampler, which is connected to the gas chromatograph with a heated transmission line. The chromatographic separation is separated on a so-called wax column (WCOT capillary column, 100% polyethylene glycol) and detected by a flame ionization detector (FID).

[0148] In the evaluation, only the following peaks are considered:

[0149] - Its height exceeds the baseline noise by at least 3 times, and

[0150] - Its area is greater than 10% of the area of ​​the acetone peak, where the concentration in the calibration solution is 0.5 g / L.

[0151] The result is based on a semi-quantitative evaluation in which the blank peak area is subtracted from the total peak area of ​​the sample chromatogram. The evaluation refers to calibration with acetone and its carbon content, respectively. The final total emission value (or TVOC = Total Volatile Organic Compounds) is therefore given in carbon equivalents.

[0152] k) Thermal desorption analysis of organic emissions for characterization of non-metallic materials (VDA 278, October 2011)

[0153] The following method descriptions provide the skilled reader with an overview of the relevant parameters. In case of doubt, only the original method should be used for comparison of results.

[0154] VDA 278 is intended for the determination of emissions released by non-metallic materials used in automotive injection mouldings, such as textiles, carpets, adhesives, sealing compounds, foams, leather, plastic parts, films and sheets, coatings or material combinations.

[0155] In a VDA 278 experiment, volatile and semivolatile substances are extracted from the sample in a thermal desorption step by heating and a flow of an inert gas (usually helium). The extracted compounds are cryofocused in a cooling trap before hot injection into a gas chromatograph for separation. Mass spectrometry is used for detection.

[0156] The analysis includes the semi-quantification of two specifically defined cumulative emission values, namely the fraction of volatile organic compounds (VOC) and condensable substances (FOG value). In addition, individual substances are determined.

[0157] In the VOC analysis, the sample is heated to 90 ° C and kept for 30 minutes to extract the volatile organic compounds, taking into account the emissions of up to n-pentacosane (C25) in the chromatogram. FOG analysis involves a further thermal desorption step. For this purpose, after the VOC analysis, the sample is retained in the desorption tube and reheated to 120 ° C and kept for 60 minutes. The FOG value is defined as the fraction of semi-volatile organic compounds eluting from n-tetradecane (C14) to n-triadecane (C32) in the chromatogram. The semi-quantitative analysis of the VOC values ​​is calculated as toluene equivalents. The FOG values ​​are calculated separately as hexadecane equivalents.

[0158] The instruments used for the analysis must meet the minimum requirements specified in VDA 278 (Chapter 3.1).

[0159] Although a typical result variation of up to 15% can be expected within one laboratory, this does not allow for a generally valid precision. Therefore, separate measurement series are required to investigate the correlation matrix.

[0160] According to VDA 278, the results obtained do not apply to:

[0161] - further assessment of any type of health impact of the emissions,

[0162] - in any form as a basis for an assessment of the concentrations that may be found in an intact vehicle when stationary, driving or under similar driving conditions.

[0163] l) Dynamic rheological measurement

[0164] The characterization of polymer melts by dynamic shear measurements complies with ISO standards 6721-1 and 6721-10. The measurements were performed on an Anton Paar MCR501 stress-controlled rotational rheometer equipped with a 25 mm parallel plate geometry. The measurements were performed on compression molded plates, using a nitrogen atmosphere and setting the strain in the linear viscoelastic range. Oscillatory shear tests were performed on PE and PP at 190 °C and 200 °C, respectively, applying a frequency range of 0.01 rad / s to 600 rad / s and setting a gap of 1.3 mm.

[0165] In a dynamic shear test, the probe is subjected to uniform deformation under sinusoidally varying shear strain or shear stress (strain and stress controlled modes, respectively). In a controlled strain test, the sinusoidal strain to which the probe is subjected can be expressed as

[0166] (t) = γ0 sin(ωt) (1)

[0167] If the applied strain is within the linear viscoelastic range, the resulting sinusoidal stress response can be expressed as:

[0168] (t) = σ0 sin(ωt+δ) (2)

[0169] in

[0170] σ0 and γ0 are stress and strain amplitudes, respectively

[0171] ω is the angular frequency

[0172] δ is the phase shift (loss angle between applied strain and stress response)

[0173] t is time.

[0174] Dynamic test results are usually expressed in terms of several different rheological functions, namely the shear storage modulus G', the shear loss modulus G", the complex shear modulus G*, the complex shear viscosity η*, the dynamic shear viscosity η', the heterogeneous component of the complex shear viscosity η", and the loss tangent tanδ, which can be expressed as follows:

[0175]

[0176]

[0177] G*=G'+iG"[Pa](5)

[0178] η*=η'-iη”[Pa.s] (6)

[0179]

[0180]

[0181] The so-called shear thinning factor (STF) is determined as described in Equation 9.

[0182]

[0183] These values ​​were determined by means of a single-point interpolation procedure defined in the Rheoplus software. In cases where a given G* value was not reached experimentally, this value was determined by extrapolation to 10 using the same procedure as before. In both cases (interpolation or extrapolation), the options in Rheoplus “-Interpolate y values ​​to x values ​​from parameters” and “Logarithmic interpolation type” were applied.

[0184] The tests were performed on compression molded discs made from cryogenically ground powders.

[0185] m) LAOS nonlinear viscoelastic ratio

[0186] The nonlinear viscoelastic behavior under shear flow is investigated using the large amplitude oscillatory shear method. The method requires the application of a sinusoidal strain amplitude γ0 at a given angular frequency ω for a given time t. As long as the applied sinusoidal strain is high enough, a nonlinear response will occur. In this case, the stress σ is a function of the applied strain amplitude, time, and angular frequency. Under these conditions, the nonlinear stress response is still a periodic function; however, it can no longer be represented by a single harmonic sine wave. The stress [0-0] resulting from the nonlinear viscoelastic response can be represented by a Fourier series that includes contributions from higher-order harmonics:

[0187] σ(t,ω,γ0)=γ0.Σ n [G' n (ω,γ0).sin(nωt)+G” n (ω,γ0).cos(nωt)]

[0188] Where, σ-stress response

[0189] t-time

[0190] ω-Frequency

[0191] γ0-strain amplitude

[0192] n - number of harmonics

[0193] G n '-nth order elastic Fourier coefficient

[0194] G n ” -nth order viscosity Fourier coefficient

[0195] Large amplitude oscillatory shear (LAOS) was used to analyze the nonlinear viscoelastic response [4-6]. Time scan measurements were performed on an RPA2000 rheometer from Alpha Technologies in combination with a standard double cone die. During the measurement, the test chamber was sealed and a pressure of approximately 6 MPa was applied. LAOS tests were performed at a temperature of 190°C, an angular frequency of 0.628 rad / s and a strain of 1000% applied 10 times. To ensure that steady-state conditions were achieved, the nonlinear response was determined only after at least 20 cycles were completed for each measurement. The large amplitude oscillatory shear nonlinear coefficient (LAOS_NLF) is defined as:

[0196]

[0197] Where G1' - first order Fourier coefficient

[0198] G3' - third order Fourier coefficient

[0199] These tests were conducted on cryogenically milled powders.

[0200] [1] J.M. Dealy, K.F. Wissbrun, Melt Rheology and Its Role in Plastics Processing: Theory and Applications; edited by Van Nostrand Reinhold, New York (1990)

[0201] [2] S. Filipe, Non-Linear Rheology of Polymer Melts, AIP Conference Proceedings 1152, pp. 168 - 174 (2009)

[0202] [3] M. Wilhelm, Macromol. Mat. Eng. 287, 83 - 105 (2002)

[0203] [4] S. Filipe, K. Hofstadler, K. Klimke, A.T. Tran, Non-Linear Rheological Parameters for Characterisation of Molecular Structural Properties in Polyolefins, Proceedings of Annual European Rheology Conference, 135 (2010)

[0204] [5] S. Filipe, K. Klimke, A.T. Tran, J. Reussner, Proceedings of Novel Non-Linear Rheological Parameters for Molecular Structural Characterisation of Polyolefins, Novel Trends in Rheology IV, Zlin, Check Republik (2011)

[0205] [6] K.Klimke, S.Filipe, ATTran, Non-linear rheological parameters for characterization of molecular structural properties in polyolefins, Proceedings of European Polymer Conference, Granada, Spain (2011)

[0206] Example

[0207] The raw materials of IE1 come from DSD324 (German Green Dot System), which is based on EPR-based raw materials.

[0208] The raw material for IE2 is obtained from polypropylene sorted from municipal solid waste in Poland and Greece.

[0209] The raw materials of CE1 come from is a grey post-consumer recycled material consisting mainly of pre-sorted community waste and is a commercial product produced by mtm plastics GmbH in Niedergebra, Germany.

[0210] The feedstock material for CE2 comes from Van Werven BB2 06 / 2020, a rigid plastic waste from post-consumer recyclate in the form of flakes that have been sorted and washed. These flakes are sent to pelletizing to produce pellets.

[0211] To obtain IE1 and IE2 materials, polypropylene mixed color blends were obtained from these raw materials by the following steps:

[0212] Sorting out non-PP materials, including polystyrene, polyamide, polyethylene, metal, paper and wood, thus providing post-consumer plastic materials;

[0213] Sorting out natural (i.e. uncolored) and white products to provide a post-consumer mixed-color polypropylene recycling stream with a specific color mix, resulting in a gray / slightly gray final color after extrusion, such as shampoo or shower gel bottles, jars, etc.;

[0214] The selected post-consumer plastic material having this specific color mix is ​​ground, washed in aqueous solutions containing various detergents, and subsequently dried, air-sieved, and screened;

[0215] Further sorting of the pre-treated post-consumer plastic material to eliminate non-polyolefin and color fractions to produce a purified polypropylene polyolefin recycling stream;

[0216] melt extruding the material to obtain a polypropylene blend in the form of pellets as an extruded, pelletized, recycled polypropylene product; and

[0217] The extruded, pelletized and recycled polypropylene products are subjected to an aeration treatment at a temperature range of 100-130° C. The extruded, pelletized and recycled polypropylene products are preheated to a target temperature by using an air flow with a temperature of at least 100° C.

[0218] The properties of the obtained polypropylene mixed color blends and commercial samples are shown in the following table.

[0219] surface

[0220]

[0221]

[0222]

[0223] (1) Average value of 20-30 samples

[0224] (2) Average value of 7 samples

[0225] (3) Average value of 10 samples

[0226] (4) Average of 3 samples

[0227] From the above results, it can be seen that Compared with commercial products such as Van Werven (CE1) or Van Werven (CE2), the recycled polypropylene mixed color blends according to IE1 and IE2 show higher purity (expressed as C2 content), especially the C2 content of the crystalline part (C2 (CF)), and lower emission performance (total carbon emission, VOC, FOG). In addition, the composition of the present invention also shows excellent mechanical properties such as tensile modulus, tensile strain at break and impact strength.

[0228] The compositions of the invention also exhibit high color consistency and brighter chroma (CIELab). The compositions of the invention also exhibit good processability, as indicated by a higher shear thinning coefficient, despite their lower MFR compared to the comparative examples.

Claims

1. A polypropylene mixed color blend having (i) a crystalline component (CF) content, determined according to CRYSTEXQC analysis, as determined herein, in the range of 85.0 wt.-% to 95.0 wt.-%, (ii) a soluble fraction (SF) content, determined according to CRYSTEXQC analysis, as determined herein, in the range of 5.0 wt.-% to 15.0 wt.-%, (iii) a total ethylene content (C2), determined according to CRYSTEXQC analysis, as determined herein, in the range of 2.0 wt.-% to 10.0 wt.-%, (iv) the crystalline portion (CF) has a propylene content (C3(CF)) determined by quantitative 13 FT-IR spectroscopy calibrated with C-NMR spectroscopy, as determined herein, in the range of 93.0 wt.-% to 99.0 wt.-%; (v) the crystalline component (CF) has an ethylene content (C2(CF)) determined by quantitative 13 % to [C2]-0.2 wt.-%, wherein [C2] is the total ethylene content (C2) as defined in (iii), (vi) CIELAB color space (L*a*b*), measured according to DIN EN ISO 11664-4, as described herein, is: L* is 30.0 to 73.0; a* is -10 to 25; b* is -5 to 20.

2. The polypropylene mixed color blend according to claim 1, having an inorganic residue, as measured by calcination analysis (TGA) according to DIN ISO 1172:1996, of 0.1 wt.-% to less than 2.0 wt.-%, relative to the total weight of the polypropylene mixed color blend.

3. The polypropylene mixed color blend according to claim 1 or 2, which has a total carbon emission, measured by HSGC-FID according to VDA277, of 1.0 μg carbon / g to 30 μg carbon / g relative to the total weight of the polypropylene mixed color blend.

4. The polypropylene mixed color blend according to any one of claims 1 to 3, wherein the soluble fraction (SF) obtained by CRYSTEX QC analysis has an ethylene content (C2(SF)) determined by quantitative 13 The content of 2-nitropropene was determined by FT-IR spectroscopy calibrated with C-NMR spectroscopy in the range of 20.0 wt.-% to 30.0 wt.-%.

5. The polypropylene mixed color blend according to any one of the preceding claims having a Large Amplitude Oscillatory Shear-Non-Linear Coefficient (LAOS-NLF) measured at 190°C, an angular frequency of 0.628 rad / s and a strain of 1000%, as described herein in G1' is the first-order Fourier coefficient G3' is the third-order Fourier coefficient The coefficient is in the range of 1.5 to 3.

5.

6. A polypropylene mixed color blend according to any one of the preceding claims having a shear thinning factor (STF) value, defined as the ratio of the complex viscosity η(0.05) to η(300) at 230°C in the frequency range of 0.01 rad / s to 600 rad / s according to ISO 6721-1 and ISO 6721-10, determined as described herein, in the range of 7.5 to 15, and / or It has a total condensable organic content (FOG), determined by HS GC-FID according to VDA 278, of 20 to 450 μg / g relative to the total weight of the polypropylene mixed color blend.

7. Polypropylene mixed color blend according to any one of the preceding claims, obtained by visbreaking using peroxide.

8. The polypropylene mixed color blend according to any one of the preceding claims, having a melt flow rate MFR at 230°C 2.16 , is at least 5 g / 10 min as determined herein.

9. A method for recycling polypropylene mixed color material, comprising the following steps: a) providing a mixed plastic recycling stream (A); b) screening the mixed plastic recycling stream (A) to produce a screened mixed plastic recycling stream (B) having only articles having a longest dimension in the range of 30 mm to 400 mm; c) sorting the screened mixed plastic recycling stream (B) by one or more sorting systems including near infrared (NIR) and optical sensors, wherein the screened mixed plastic recycling stream (B) is sorted at least by color and polymer type and optionally by product form, thereby producing a sorted mixed color polypropylene recycling stream (CM), which will be subjected to step d) and subsequent steps; d) chopping the sorted mixed color polypropylene recycling stream (CM) to form a flake mixed color polypropylene recycling stream (D); e) washing the flake mixed color polypropylene recovery stream (D) with a first water washing solution (W1) without inputting heat energy, thereby producing a first suspended polypropylene recovery stream (E); f) removing at least a portion of the first aqueous washing solution (W1) from the first suspended polypropylene recovery stream (E) to obtain a first washed polypropylene recovery stream (F); g) washing the first washed polypropylene recovery stream (F) with a second aqueous washing solution (W2) to produce a second suspended polypropylene recovery stream (G), wherein sufficient thermal energy is introduced into the second suspended polypropylene recovery stream (G) to provide a temperature in the range of 65° C. to 95° C. during washing; h) removing the second aqueous wash solution (W2) and any material not floating on the surface of the second aqueous wash solution from the second suspended polypropylene recovery stream (G) to obtain a second washed polypropylene recovery stream (H); and i) drying the second washed polypropylene recycle stream (H) to obtain a dried polypropylene recycle stream (I) comprising the polypropylene melange blend according to any one of the preceding claims.

10. The method according to claim 9, further comprising at least one of the following steps: j) separating the dried polypropylene recovery stream (I) obtained from step i) into a light component and a heavy component polypropylene recovery stream (J); k) further fractionating the heavy component polypropylene recovery stream (J), or in the absence of step j), fractionating the dried polypropylene recovery stream (I), using one or more optical separators to separate the one or more target polypropylenes by removing any flakes containing materials other than the one or more target polypropylenes to obtain a purified polypropylene recovery stream (k); l) subjecting the purified polypropylene recovery stream (K) to melt extrusion, preferably to pelletization, preferably wherein the additive (Ad) is added in the molten state, to form an extruded recycled polypropylene product (L), preferably a pelletized recycled polypropylene product (L); m) aerating the recycled polypropylene product (L) or, in the absence of step 1), aerating the purified polypropylene recycling stream (K) to remove volatile organic compounds, thereby producing an aerated recycled polypropylene product (M), which is either an aerated extruded recycled polypropylene product (M1), preferably a pelletized recycled polypropylene product (M1), or an aerated recycled polypropylene flake (M2), The order of step 1) and step m) can be interchanged, so that the purified polypropylene recycling stream (K) is first inflated to form an inflated recycled polypropylene sheet (M2), and then extruded, preferably wherein the additive (Ad) is added in the molten state to form an extruded inflated recycled polypropylene product (M3), preferably a pelletized inflated recycled polypropylene product (M3), which is a polypropylene mixed color blend according to any one of the preceding claims 1 to 8.

11. Polypropylene mixed color blend according to any one of the preceding claims, obtainable or obtained according to the process of claim 9 or 10.

12. A blend comprising the polypropylene mixed color blend according to any one of claims 1 to 8 and at least one virgin polypropylene and / or recycled polypropylene.

13. An article comprising the polypropylene mixed color blend according to any one of claims 1 to 8 or the blend according to claim 12.

14. The article of claim 13, selected from the group consisting of bottle caps, seals, bottles, containers, automotive products, and wire and cable products.

15. Use of the polypropylene mixed color mixture according to any one of claims 1 to 8 and 11 in household applications, automotive applications, electrical appliances, packaging or wire and cable applications.