Process for treating initial polyethylene-containing material to produce polyethylene composition for injection molding

By performing heat treatment and mechanical energy imparting in twin-screw extruders, the melt flow index of polyethylene materials and the viscosity are reduced, and the problem that existing polyethylene recycled materials are not suitable for injection molding is solved, and safe and effective polyethylene is achieved Composition production.

CN118900760AActive Publication Date: 2024-11-05TOTALENERGIES SE +4
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202380021342.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-10
Filing Date
2023-02-01
Publication Date
2024-11-05
Estimated Expiration
2043-02-01

AI Technical Summary

Technical Problem

The melt flow index and viscosity of existing polyethylene recycled materials are not suitable for injection molding, limiting their application scope, and traditional methods such as the use of peroxides can cause fire risks and peroxide residue problems.

Method used

By performing heat treatment in a twin-screw extruder, using a thermal adjustment device and a specific screw profile design, self-heating and mechanical energy are carried out, the melt flow index of the polyethylene material is improved and the viscosity is reduced, forming a polyethylene combination suitable for injection molding. Things.

Benefits of technology

The melt flow index of polyethylene materials is significantly improved and the viscosity is reduced, making it suitable for injection molding applications, avoiding the fire risks and peroxide residue problems caused by chemical treatment, and achieving more efficient recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004988395780000221
    Figure BDA0004988395780000221
  • Figure BDA0004988395780000241
    Figure BDA0004988395780000241
  • Figure BDA0004988395780000242
    Figure BDA0004988395780000242
Patent Text Reader

Abstract

A process of treating an initial polyethylene-containing material to produce a polyethylene composition, the process comprising providing a twin screw extruder having a thermal conditioning device; providing an initial polyethylene-containing material comprising at least 50 wt% polyethylene based on the total weight of the initial polyethylene-containing material; extruding the initial polyethylene-containing material to obtain a polyethylene composition; wherein the extrusion is carried out with a residence time of less than 20 minutes; and recovering the polyethylene composition; wherein extruding comprises heat treating the initial polyethylene-containing material by self-heating at a temperature of at least 300 DEG C in one or more hot zones of the extruder to have a maximum barrel temperature ranging from 300 to 460 DEG C in at least one hot zone of the extruder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to processes for producing polyethylene compositions suitable for injection molding, preferably comprising recycled polyethylene. Background Art

[0002] As required, sometimes useful is to have the possibility of processing existing polyolefin or existing polyolefin composition to change some properties. Nowadays, for promoting the subsequent recycling of polyolefin or polyolefin composition, it is necessary to allow such change to be achieved without the processing and technology of blending in other polyolefin and / or additive. The property that may need to be changed is for example melt flow index, viscosity, smell, impurity level etc.

[0003] PCR (post-consumer recycled) containing polyethylene may have low melt index values, typically close to 0.2 g / 10 min MI2 for PCR polyethylene originating from small containers (shampoo bottles...) and close to 1.0 g / 10 min MI2 for PCR polyethylene originating from films, which makes them rather unsuitable for injection molding and, therefore, limits the applications of recycled polyethylene containing materials. Therefore, there is a need for methods of processing these recycled polyethylene containing materials to convert them into polyethylene compositions suitable for injection molding applications.

[0004] A method that can increase and control the melt flow index and / or viscosity of polyethylene or polyethylene-containing materials, such as recycled polyethylene-containing materials, would create significant added value for recycled polyethylene compositions because it expands their areas of application. Such a method may also contribute to the plastic waste problem because more plastics can be converted into useful polyethylene compositions after recycling.

[0005] The increase in the melt index of PCR polyethylene is not significant at all, since the melt index generally decreases during the standard extrusion process. The situation is slightly different for polypropylene, since there are methods to increase the melt flow index of polypropylene. However, these methods involve reactive extrusion with the addition of peroxides. However, such methods lead to polypropylene with peroxide decomposition products, while the demand for "clean" polyolefins is increasing. If high peroxide contents must be avoided, for example to avoid excessive peroxide residues, the increase in the melt index of polypropylene is limited in standard extrusion processes. In addition, the use of organic peroxides leads to branching and crosslinking of the polyethylene.

[0006] Even when polypropylene is present in the polyethylene composition, which can be quite frequent in PCR polyethylene, a high content of polyethylene of at least 50 wt% contributes to a reduced melt index during standard pelletizing. Therefore, there is a need for a clean method for treating an initial polyethylene-containing material and / or a method for treating an initial polyethylene-containing material which provides an increase in the melt flow index and improved properties for injection molding applications. Preferably, the method for treating an initial polyethylene-containing material should have a low safety risk, especially in terms of fire risk.

[0007] There is also a need for polyethylene compositions suitable for injection molding applications and which are preferably derived from recycled polyolefins.

[0008] There is a need to produce polyethylene compositions having reduced viscosity suitable for injection molding applications.

[0009] WO2021 / 064113 discloses a method in which a polyolefin composition is produced using the following method: wherein ultrasound is applied to a material that may be a recycled polyolefin. Although the disclosed method provides very good results, there is still room for further improvement in such fields, in particular for implementing the method or process on an industrial level. A simple and cost-effective process is also needed. Summary of the invention

[0010] It has now been discovered that one or more of the above needs can be met by subjecting existing polyethylene-containing materials, such as recycled polyethylene-containing materials, to a single extrusion to produce a new polyethylene composition suitable for injection molding.

[0011] According to a first aspect, the present disclosure relates to a process for treating an initial polyethylene-containing material to produce a polyethylene composition, notably comprising the steps of:

[0012] a) providing a twin screw extruder with a heat regulating device;

[0013] b) providing an initial polyethylene-containing material comprising at least 50 wt. % polyethylene, based on the total weight of the initial polyethylene-containing material;

[0014] c) extruding the initial polyethylene-containing material to obtain a polyethylene composition; wherein the extrusion is performed with a residence time of less than 20 minutes; and

[0015] d) collecting the polyethylene composition;

[0016] wherein the extrusion step (c) comprises heat treating the initial polyethylene-containing material by self-heating of the material at a temperature of at least 300°C in one or more hot zones of the extruder, wherein the one or more hot zones have a total length equal to or greater than 6D, wherein D is the screw diameter, wherein extrusion is carried out with a mechanical specific energy greater than or equal to 0.4 kWh / kg, wherein the screw profile comprises at least one hot zone having successive kneading block elements followed by left-handed elements over a length of at least 4D, wherein D is the screw diameter, wherein the heat regulating device is set to an initial applied barrel temperature in the range between 240 and 320°C and is closed when the barrel temperature in the zone spontaneously exceeds the applied barrel temperature by at least 1°C; preferably, at least 3°C ​​without the need for external heat application.

[0017] Unexpectedly, it has been found that the initial polyethylene-containing material can be upgraded to a higher melt index and lower viscosity by heat treatment, thereby reaching values ​​suitable for injection molding applications; without the need for additives or other special treatments such as ultrasound. In particular, the increase in melt index is obtained without the use of flow modifiers. The process is notable for its simplicity, as it can be carried out in a twin-screw extruder. As shown by the examples, the increase in melt index can be up to 80 times.

[0018] This process is also significant because there is no chemical way to break the polyethylene chain. Under normal processing temperatures and standard extrusion conditions, there is branching of the polyethylene chain (reduction of MI2). The use of organic peroxides leads to polyethylene branching and crosslinking. The huge increase of at least 10 (e.g., at least 20 or at least 40) times of the melt index obtained by specific extrusion conditions together with the general reduction of complex viscosity (e.g., flattening of the complex viscosity curve at low frequencies) allows responding to the long-term needs in the recycling field by expanding the possible applications of recycled raw materials.

[0019] Indeed, as shown by the examples, the process is remarkable in that the viscosity of the polyethylene composition is reduced compared to the viscosity of the initial polyethylene-containing material at both 0.1 rad / s and 100 rad / s, which makes the treated polyethylene suitable for injection molding applications.

[0020] In one embodiment, the screw profile comprises two or more hot zones, wherein the first hot zone comprises a series of kneading block elements over a length of at least 4D followed by left-handed elements, wherein D is the screw diameter, and one or more additional hot zones located downstream of the first hot zone are filled mixing zones, each comprising a kneading block element over a length of at least 4D followed by a kneading left-handed element or a left-handed element, wherein D is the screw diameter.

[0021] In one embodiment, the tandem kneading block elements of at least one hot zone of the extruder comprise disks having a 90 degree disk offset and a disk width of at least 0.3D, where D is the screw diameter.

[0022] In one embodiment, a hot zone of the extruder is or comprises the melt zone of the extruder.

[0023] In a preferred embodiment, the ratio of the melt index of the polyethylene composition (MI2 T) to the melt index of the initial polyethylene-containing material (MI2 R) is at least 10. This can be obtained by appropriate choice of temperature and residence time of the heat treatment.

[0024] In a preferred embodiment, the specific mechanical energy used during extrusion is selected so that the ratio of the melt index of the polyethylene composition (MI2 T) to the melt index of the initial polyethylene-containing material (MI2 R) is at least 10.

[0025] For example, the ratio of the melt index (MI2 T) of the polyethylene composition to the melt index (MI2 R) of the initial polyethylene-containing material is at least 10; preferably, at least 15; preferably, at least 20; preferably, at least 30; preferably, at least 40.

[0026] In one embodiment, the initial polyethylene-containing material is selected to have:

[0027] - a high load melt index (HLMI R) of at least 1.0 g / 10 min when measured at 190°C under a load of 21.6 kg according to ISO 1133-2011; and / or

[0028] - a melt index (MI2 R) of at most 3.0 g / 10 min when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg; and / or

[0029] - At least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012 3 density.

[0030] For example, the initial polyethylene-containing material is selected to have a melt index ranging from a high load melt index (HLMI R) of at least 1.0 g / 10 minutes when measured at 190°C under a load of 21.6 kg according to ISO 1133-2011 to a melt index (MI2 R) of at most 3.0 g / 10 minutes when measured at 190°C under a load of 2.16 kg according to ISO 1133-2011.

[0031] For example, the initial polyethylene-containing material is selected to have:

[0032] - a high load melt index (HLMI R) of at least 1.0 g / 10 min when measured according to ISO 1133-2011 at 190°C under a load of 21.6 kg, a melt index (MI2 R) of at most 0.45 g / 10 min when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg, and at least 0.940 g / cm2 when measured according to ISO 1183-1:2012 at 23°C 3 density; or

[0033] - a melt index (MI2 R) ranging from 0.8 to 1.5 g / 10 min when measured at 190°C under a load of 2.16 kg according to ISO 1133-2011, and ranging from 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012 3 To less than 0.940g / cm 3 ; preferably 0.910g / cm 3 Up to 0.935g / cm 3 , and more preferably 0.910 g / cm 3 Up to 0.930g / cm 3 density.

[0034] In one embodiment, the initial polyethylene-containing material further has:

[0035] - an Mz / Mw of at least 4.0 when measured by size exclusion chromatography (SEC); and / or

[0036] - a complex viscosity at 1 rad / s at 190°C in the range of 20,000 to 80,000 Pa·s; and / or

[0037] - a Mw / Mn in the range of 5.0 to 30.0 when determined by size exclusion chromatography; and / or

[0038] - a complex viscosity ratio above 10, wherein the complex viscosity ratio is the ratio of the complex viscosity at a frequency of 0.1 rad / sec to the complex viscosity at a frequency of 100 rad / sec when measured at 190°C.

[0039] In one embodiment, the initial polyethylene-containing material further has a tan δ (G" / G' measured at 0.1 rad / sec at 190°C) of at most 3.0, preferably at most 2.6.

[0040] In one embodiment, the initial polyethylene-containing material further has a tan delta (G" / G' measured at 0.1 rad / sec at 190°C) of at least 0.5, preferably at least 0.8.

[0041] In one embodiment, the initial polyethylene-containing material further has a tan δ (G" / G' measured at 0.1 rad / sec at 190°C) ranging from 0.5 to 3.0; preferably, 0.8 to 2.6.

[0042] For example, the initial polyethylene-containing material comprises at least 80 wt% polyethylene based on the total mass of the initial polyethylene-containing material; and / or is a recycled polyethylene-containing material.

[0043] For example, the initial polyethylene-containing material contains at least one polymer different from polyethylene in an amount ranging from 0 to 50 wt % based on the total weight of the initial polyethylene-containing material, wherein the at least one polymer different from polyethylene is selected from polypropylene (PP), polyacrylate (PA), polyethylene terephthalate (PET), polystyrene (PS), polylactic acid (PLA), and any mixture thereof.

[0044] For example, the process is performed in the absence of peroxide and / or in the absence of ultrasound.

[0045] In a preferred embodiment, the step (c) of extruding the initial polyethylene-containing material comprises heat treatment by self-heating of the material, wherein the extrusion is carried out with a mechanical specific energy greater than or equal to 0.45 kWh / kg, preferably greater than or equal to 0.5 kWh / kg; more preferably greater than or equal to 0.6 kWh / kg.

[0046] For example, the step (c) of extruding the initial polyethylene-containing material comprises a thermal treatment by self-heating of the material or by heating the material, wherein the extrusion is carried out in at least one thermal zone at a maximum barrel temperature in the range of 300 to 460°C; preferably at a maximum barrel temperature in the range of 310 to 450°C; more preferably at a maximum barrel temperature in the range of 320 to 430°C; even more preferably at a maximum barrel temperature in the range of 330 to 410°C, and most preferably at a maximum barrel temperature in the range of 340 to 390°C.

[0047] For example, step (c) of extruding the initial polyethylene-containing material comprises heat treatment in at least one hot zone at a temperature in the range of 300 to 460°C; preferably at a temperature in the range of 310 to 450°C; more preferably at a temperature in the range of 320 to 430°C; even more preferably at a temperature in the range of 330 to 410°C, and most preferably at a temperature in the range of 340 to 390°C, or at a temperature in the range of 320 to 460°C.

[0048] For example, step (c) of extruding the initial polyethylene-containing material comprises a heat treatment at a temperature of at least 300°C or at least 305°C; preferably at a temperature of at least 315 or at least 320°C; more preferably at a temperature of at least 330°C; even more preferably at a temperature of at least 340°C, and most preferably at a temperature of at least 350°C, or at a temperature of at least 355°C, or at a temperature of at least 360°C.

[0049] For example, step (c) of extruding the initial polyethylene-containing material comprises a heat treatment at a temperature of at most 460°C; preferably, at most 450°C; more preferably, at most 440°C; even more preferably, at most 440°C; most preferably, at most 430°C; even most preferably, at most 420°C or at most 410°C or at most 405°C or at most 400°C or at most 395°C or at most 390°C.

[0050] For example, step (c) of extruding the initial polyethylene-containing material comprises performing the extrusion at a screw speed ranging from 100 to 1200 rpm.

[0051] For example, step (c) of extruding the initial polyethylene-containing material comprises carrying out the extrusion with a residence time in the range of 10 seconds to 10 minutes; preferably with a residence time in the range of 20 seconds to 5 minutes; more preferably with a residence time in the range of 10 to 180 seconds; even more preferably, 10 to 120 seconds; most preferably, 20 to 100 seconds; and even most preferably, 30 to 80 seconds.

[0052] In one embodiment, the polyethylene composition recovered in step (d) has one or more selected from the group consisting of:

[0053] - At least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012 3 density; and / or

[0054] - a melt index MI2 ranging from 3.0 to 60.0 g / 10 min when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg; and / or

[0055] - an unsaturation index greater than 2,000, wherein the unsaturation index is the product of the units of vinyl unsaturation per 1,000 carbon atoms and the Mn in Daltons when determined by ASTM D6248-98:2004; and / or

[0056] - A complex viscosity at 0.1 rad / s at 190° C. of at most 20,000 Pa·s.

[0057] In a preferred embodiment, the polyethylene composition recovered in step (d) has:

[0058] - At least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012 3 density;

[0059] - a melt index MI2 ranging from 3.0 to 60.0 g / 10 minutes when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg;

[0060] - an unsaturation index greater than 2,000, wherein the unsaturation index is the product of the units of vinyl unsaturation per 1,000 carbon atoms and the Mn in Daltons when determined by ASTM D6248-98:2004; and

[0061] - A complex viscosity at 0.1 rad / s at 190° C. of at most 20,000 Pa·s.

[0062] For example, the polyethylene composition recovered in step (d) has a molecular weight of at least 0.910 g / cm2 when measured according to ISO 1183-1:2012 at 23°C. 3 ; preferably at least 0.912g / cm 3 density.

[0063] For example, the polyethylene composition recovered in step (d) has a melt index MI2 ranging from 3.0 to 60.0 g / 10 min; preferably ranging from 4.0 to 20.0 g / 10 min, when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg.

[0064] For example, the polyethylene composition recovered in step (d) has an unsaturation index higher than 2,000, preferably higher than 5000, even preferably higher than 7000, wherein the unsaturation index is the product of the ethylenic unsaturated units per 1,000 carbon atoms and the Mn in Daltons when determined by ASTM D6248-98:2004; wherein the unsaturation index is the product of the ethylenic unsaturated units per 1,000 carbon atoms and the Mn in Daltons.

[0065] For example, the polyethylene composition recovered in step (d) has a complex viscosity at 0.1 rad / s at 190° C. of at most 20,000 Pa·s; preferably at most 18,000 Pa·s.

[0066] For example, the polyethylene composition recovered in step (d) has a complex viscosity ratio of at most 8.0, wherein the complex viscosity ratio is the ratio of the complex viscosity at a frequency of 0.01 rad / sec to the complex viscosity at a frequency of 100 rad / sec when measured at 190°C.

[0067] Preferably, the polyethylene composition recovered in step (d) further has a Mz / Mw of at most 7.0; preferably at most 6.0; preferably at most 5.0, when determined by size exclusion chromatography.

[0068] For example, the polyethylene composition recovered in step (d) further has a Mw / Mn in the range of 2.5 to 10.0 when determined by size exclusion chromatography.

[0069] For example, the polyethylene composition recovered in step (d) further has a tan delta (G" / G') at 0.1 rad at 190°C of above 2.5; preferably at least 3.0; more preferably at least 5.0, and even more preferably at least 10.0.

[0070] According to a second aspect, the present disclosure relates to a polyethylene composition, notable in that it is a polyethylene composition obtained by the process according to the first aspect.

[0071] According to a third aspect, the present disclosure relates to an article produced from the polyethylene composition according to the second aspect, notably, the article is an injection molded article; preferably, the article is selected from a bottle or a container.

[0072] According to a fourth aspect, the present disclosure relates to a method for producing an injection molded article, which is notable in that it includes producing a polyethylene composition from an initial polyethylene-containing material according to a process according to the first aspect, and using the polyethylene composition obtained by the process (or using the polyethylene composition according to the second aspect) to produce an injection molded article; preferably, the initial polyethylene-containing material is a recycled polyethylene-containing material.

[0073] According to a fourth aspect, the present disclosure relates to a method for producing an injection molded article, which is notable in that it comprises producing a polyethylene composition from an initial polyethylene-containing material according to a process as defined in the first aspect in a first step, and using the polyethylene composition produced in the first step to produce an injection molded article in a second step; preferably, the initial polyethylene-containing material is a recycled polyethylene-containing material. BRIEF DESCRIPTION OF THE DRAWINGS

[0074] - Figure 1 Possible screw profiles for use in the context of the present disclosure are shown.

[0075] - Figure 2 MI2 was plotted against screw speed for a fixed flow rate of 1.5 kg / h.

[0076] - Figure 3 MI2 was plotted against screw speed for a fixed flow rate of 2.5 kg / h.

[0077] - Figure 4 The complex viscosity of various polyethylene-containing compositions was plotted versus angular frequency in comparison to the initial polyethylene-containing material.

[0078] - Figure 5 The complex viscosity is plotted against the angular frequency and further the loss (G") and storage modulus (G') of PE1 of the polyethylene composition obtained by extrusion at 800 rpm and 360°C are shown. DETAILED DESCRIPTION

[0079] It should be understood that the present disclosure is not limited to the particular processes or compositions described, as such processes or compositions may, of course, vary. It should also be understood that the terminology used herein is not intended to be limiting, as the scope of the present disclosure will be limited only by the appended claims.

[0080] When describing the polymers, uses and processes of the present disclosure, the terms used are interpreted by the following definitions unless the context dictates otherwise. For the present disclosure, the following definitions are given:

[0081] As used herein, the singular forms "a," "an," and "the" include both singular and plural referents unless the context dictates otherwise. By way of example, "a composition" means one composition or more than one composition.

[0082] As used herein, the terms "comprising" and "consisting of" are synonymous with "including" or "containing", and are inclusive or open-ended and do not exclude additional, unrecited members, elements, or method steps. The terms "comprising" and "consisting of" also include the term "consisting of".

[0083] The recitation of numerical ranges by endpoints includes all integers and, where appropriate, fractions contained within the range (e.g., 1 to 5 may include 1, 2, 3, 4, 5 when referring to, for example, the number of elements, and may also include 1.5, 2, 2.75, and 3.80 when referring to, for example, measurements). The recitation of endpoints also includes the endpoint values ​​themselves (e.g., 1.0 to 5.0 includes both 1.0 and 5.0). Any numerical range recited herein is intended to include all subranges contained therein.

[0084] All references cited in this specification are incorporated herein by reference in their entirety. In particular, the teachings of all references specifically mentioned herein are incorporated by reference. If the year of the standard is not indicated, the reference to the standard method for determining the parameter refers to the reference to the standard in force on the priority date of the application.

[0085] References throughout this specification to "one embodiment" or "an embodiment" mean that a particular feature, structure, or characteristic described in conjunction with that embodiment is included in at least one embodiment of the present disclosure. Therefore, the phrases "in one embodiment" or "in an embodiment" that appear in various places throughout this specification do not necessarily all refer to the same embodiment, but may refer to the same embodiment. In addition, in one or more embodiments, the particular features, structures, or characteristics may be combined in any suitable manner, as will be apparent to those skilled in the art from this disclosure. In addition, although some embodiments described herein include some features included in other embodiments but do not include other features included in other embodiments, the combination of features of different embodiments is intended to be within the scope of the present disclosure and to form different embodiments, as will be understood by those skilled in the art. For example, in the following claims and statements, any embodiment may be used in any combination.

[0086] Unless otherwise defined, all terms used in disclosing the present disclosure, including technical and scientific terms, have the meaning commonly understood by ordinary technicians in the field to which the present disclosure belongs. By further guidance, definitions of terms used in the specification are included to better understand the teachings of the present disclosure.

[0087] The terms "polyethylene" (PE) and "ethylene polymer" are used synonymously. The term "polyethylene" encompasses ethylene homopolymers and ethylene copolymer resins, which may be derived from ethylene and selected from C3-C 20One or more comonomers of α-olefins such as propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene and 1-eicosene.

[0088] The term "polyethylene resin" or "ethylene homopolymer resin" or "ethylene copolymer resin" refers to extruded and / or melted and / or pelletized polyethylene fluff or powder, and can be produced by compounding and homogenizing the polyethylene resin as taught herein, for example, with a mixing and / or extruder device. As used herein, the term "polyethylene" can be used as an abbreviation for "polyethylene resin." The term "fluff" or "powder" refers to a polyethylene material having hard catalyst particles at the core of each particle, and is defined as a polymer material after it leaves a polymerization reactor (or in the case of multiple reactors connected in series, the final polymerization reactor).

[0089] The term "post-consumer resin" (which may be abbreviated as "PCR") is used to denote components of domestic waste, household waste, or end-of-life vehicle waste. In other words, PCR is made from recycled products of waste generated by consumers. The term "post-industrial resin" (which may be abbreviated as "PIR") is used to denote waste components from pre-consumer resins during the packaging process. In other words, PIR is made from recycled products produced by manufacturers from waste materials.

[0090] The term "recycled polyethylene composition" or "recycled polyethylene-containing material" is in contrast to the term "virgin polyethylene composition", "virgin polyethylene-containing material", the term "virgin" being used to denote a polyethylene composition or material obtained directly from a polyethylene-containing polymerization plant. The term "directly obtained" is meant to include that the polyethylene composition may optionally have passed through a pelletizing step or an addition step or both.

[0091] In a production facility under normal production conditions, it is expected that the melt index (MI2, HLMI, MI5) of the fluff will be different from that of a polyethylene containing resin. In a production facility under normal production conditions, it is expected that the density of the fluff will be slightly different from that of a polyethylene containing resin (if PCR resins are considered, it is not a question of fluff (powder) or pellets, but of flakes or pellets). Unless otherwise indicated, the density and melt index of a polyethylene containing resin refer to the density and melt index as measured on a polyethylene containing resin as defined above.

[0092] The present disclosure provides a process for treating an initial polyethylene-containing material to produce a polyethylene composition. The process, the initial polyethylene-containing material, and the polyethylene composition produced by such a process (ie, the treated polyethylene composition) will be described in conjunction.

[0093] According to the disclosure, the process for treating an initial polyethylene-containing material to produce a polyethylene composition is notable in that it comprises the following steps:

[0094] a) providing a twin screw extruder with a heat regulating device;

[0095] b) providing an initial polyethylene-containing material comprising at least 50 wt. % polyethylene, based on the total weight of the initial polyethylene-containing material;

[0096] c) extruding the initial polyethylene-containing material to obtain a polyethylene composition; wherein the extrusion is performed with a residence time of less than 20 minutes; and

[0097] d) collecting the polyethylene composition;

[0098] wherein the extrusion step (c) comprises heat treating the initial polyethylene-containing material by self-heating of the material at a temperature of at least 300°C in one or more hot zones of the extruder, wherein the one or more hot zones have a total length equal to or greater than 6D, wherein D is the screw diameter, wherein extrusion is carried out with a mechanical specific energy greater than or equal to 0.4 kWh / kg, wherein the screw profile comprises at least one hot zone having a succession of kneading block elements followed by left-handed elements over a length of at least 4D, wherein D is the screw diameter, wherein the heat regulating device is set to an initial applied barrel temperature in the range between 240 and 320°C and is closed when the barrel temperature in the zone spontaneously exceeds the applied barrel temperature by at least 1°C without the need for external heat application.

[0099] The process of treating an initial polyethylene-containing material involves increasing the melt index of the initial polyethylene-containing material to produce a polyethylene composition having a melt index increased by greater than 6.0 times k; preferably at least 7.0 times k; preferably at least 8.0 times k; preferably at least 10.0 times k; preferably at least 15.0 times k; preferably at least 20.0 times k; preferably at least 30.0 times k; preferably at least 35.0 times k; preferably at least 40.0 times k.

[0100] The ratio of the melt index (MI2 T) of the polyethylene composition to the melt index (MI2 R) of the initial polyethylene-containing material is greater than 6.0; preferably at least 7.0, preferably at least 8.0; preferably at least 10.0; preferably at least 15.0; preferably at least 20.0; preferably at least 30.0; preferably at least 35.0; preferably at least 40.0.

[0101] A twin-screw extruder having a heat regulating device and extruding the initial polyethylene-containing material to obtain polyethylene Step c) of preparing the olefin composition

[0102] The processing of the initial polyethylene-containing material to obtain the polyethylene composition is carried out by extrusion, wherein the extrusion is carried out with a residence time of less than 20 minutes, and wherein the extrusion step (c) comprises heat treating the initial polyethylene-containing material at a temperature of at least 300° C. in one or more hot zones of the extruder.

[0103] The extruder is a twin-screw extruder. The extruder is provided with a screw profile showing an aggressive design, such as Figure 1 As shown in , to impart high mechanical energy to the initial polyethylene-containing material.

[0104] As known to those skilled in the art, the heat conditioning device may be used as a heating device to impart thermal energy to the initial polyethylene-containing material in the extruder in addition to the thermal energy already generated by mixing.

[0105] Extrusion mixing varies with the type of screw and the screw profile, and can significantly generate mechanical energy, such as shear energy and / or elongation energy. Thus, energy is introduced into the extrusion process in terms of mechanical energy and thermal energy. The heating and / or cooling of the barrel can be achieved, for example, by electricity, by steam or by the circulation of a heat-controlled liquid such as oil or water.

[0106] The extruder screw includes a screw body, which is composed of a cylindrical element and a rotating shaft supporting the element. The rotating shaft extends straight from its base end to its tip. In a state in which the extruder screw is rotatably inserted into the barrel of the barrel, the base end of the extruder screw is located on one end side of the barrel, on which a supply port is provided, and the tip end of the extruder screw is located on the other end side of the barrel, on which a discharge port is provided.

[0107] The screw extruder has a modular system that allows different screw elements to be pulled into the central shaft to build a defined screw profile. The extruder screw may include one or more elements selected from conveying elements, kneading elements, right-handed (forward) screw elements, left-handed (reverse) screw elements, and any combination thereof. These elements are arranged in a defined order from the base end to the tip of the extruder screw, and the order and the type and quantity of the elements involved define the screw profile. Extruders and screw elements are commercially available, for example, at Leistritz.

[0108] In one embodiment of the present disclosure, processing of the initial polyethylene-containing material is manipulated by mechanical energy.

[0109] When high mechanical energy is required, the extruder provided has a specific screw profile that is constructed to be "aggressive", which means that high mechanical energy will be imparted to the initial polyethylene-containing material. As known to those skilled in the art, high mechanical energy will lead to an increase in temperature in the extruder, thereby performing a thermal treatment by self-heating of the material.

[0110] In such an embodiment, the twin screw extruder is selected to include one or more hot zones, preferably filled mixing zones, wherein the total length of the one or more hot zones is equal to or greater than 6D, where D is the screw diameter.

[0111] It is understood that in the case where the screw profile is selected to include a single hot zone, the total length of the hot zone is equal to or greater than 6D, where D is the screw diameter. In such a case, the hot zone is also the melting zone of the twin screw extruder.

[0112] In case the screw profile comprises two or more hot zones, then the first hot zone comprises kneading block elements in succession over a length of at least 4D followed by left-handed elements, wherein D is the screw diameter, and one or more additional hot zones placed downstream of the first hot zone are filled mixing zones, each comprising kneading block elements over a length of at least 4D followed by kneading left-handed elements or left-handed elements, wherein D is the screw diameter. For example, the twin-screw extruder comprises two filled mixing zones, wherein each of the filled mixing zones has a length equal to or greater than 4D, wherein D is the screw diameter. Preferably, the first hot zone is or comprises the melting zone of the extruder.

[0113] Various mixing elements are contemplated in the one or more hot zones, but the most preferred mixing elements do not drive any forward transport (dispersed kneading block elements with 90 degree disc offset). Other disc offset angles are contemplated (e.g., 30, 45, and / or 60 degrees), but 90 degrees is preferred. The preferred minimum width of the disc is 0.3D.

[0114] Thus, preferably, the successive kneading block elements of at least one hot zone comprise disks having a disk offset of 90 degrees and a disk width of at least 0.3D, where D is the screw diameter.

[0115] For example, the twin-screw extruder includes more than two filled mixing zones, wherein the total length of the filled mixing zones is equal to or greater than 8D, where D is the screw diameter.

[0116] For example, the intensive melting zone of the twin-screw extruder is made of successive mixing elements over a length of 4D, where D is the screw diameter, followed by left-handed elements; preferably full-flight left-handed elements.

[0117] In a preferred embodiment, the thermal regulating device of the twin-screw extruder allows cooling of the barrel, and the process includes shutting down the thermal regulating device when the barrel temperature in the zone spontaneously exceeds the applied barrel temperature by at least 1°C without the need for external heat application; preferably, at least 2°C, preferably, at least 3°C; more preferably, at least 5°C; even more preferably, at least 8°C; and most preferably, at least 10°C.

[0118] Indeed, when extrusion begins, the heat regulator will be turned on, particularly in the melting zone, to allow the material to melt. Then, when the polymer self-heats, the heat regulator is turned off to allow the temperature in the extruder to increase.

[0119] In a preferred embodiment, step (c) of extruding the initial polyethylene-containing material comprises extruding at a mechanical specific energy greater than or equal to 0.45 kWh / kg, preferably greater than or equal to 0.5 kWh / kg; more preferably greater than or equal to 0.6 kWh / kg.

[0120] High rotational screw speeds are preferred, but the exact value of the high rotational screw speed depends on the "extruder diameter". For example, when considering a twin-screw extruder with a diameter D of 18 mm, a high rotational screw speed is considered to be above 500 rpm, preferably above 800 rpm. For example, when considering a twin-screw extruder with a diameter D = 58 mm, a high rotational screw speed is considered to be above 250 rpm, preferably above 350 rpm.

[0121] Non-limiting examples of suitable extruder screws having specific screw profiles are described in Figure 1 Shown in FIG. 1 are PTE1 and PTE2.

[0122] The heat treatment of the material in step c) is preferably carried out at a maximum barrel temperature in the range of 300 to 460° C., preferably in the range of 310 to 450° C., more preferably in the range of 320 to 430° C., even more preferably in the range of 330 to 410° C., and most preferably in the range of 340 to 390° C. The maximum barrel temperature is the highest temperature among the temperatures applied or measured along the extruder.

[0123] For example, step (c) of extruding the initial polyethylene-containing material comprises heat treatment in one or more hot zones of the extruder at a temperature of at least 305°C; preferably at a temperature of at least 315 or at least 320°C; more preferably at a temperature of at least 330°C; even more preferably at a temperature of at least 340°C, and most preferably at a temperature of at least 350°C, or at a temperature of at least 355°C, or at a temperature of at least 360°C.

[0124] For example, step (c) of extruding the initial polyethylene-containing material comprises a heat treatment in one or more hot zones of the extruder at a temperature of at most 460°C; preferably, at most 450°C; more preferably, at most 440°C; even more preferably, at most 440°C; most preferably, at most 430°C; even most preferably, at most 420°C, or at most 410°C, or at most 405°C, or at most 400°C, or at most 395°C, or at most 390°C.

[0125] For example, step (c) of extruding the initial polyethylene-containing material comprises heat treatment in one or more hot zones of the extruder at a temperature in the range of 300 to 460°C; preferably at a temperature in the range of 310 to 450°C; more preferably at a temperature in the range of 320 to 430°C; even more preferably at a temperature in the range of 330 to 410°C, and most preferably at a temperature in the range of 340 to 390°C, or at a temperature in the range of 320 to 460°C.

[0126] The temperature of the heat treatment is the maximum barrel temperature.

[0127] One skilled in the art can adjust the extrusion conditions to impart sufficient energy to obtain a polyethylene composition having a melt index (MI2 T) within a target range.

[0128] The screw speed can be adjusted according to the target maximum barrel temperature and the capacity of the extruder. Higher screw speeds allow for higher increases in polymer temperature. For example, the screw speed range is 100 to 1200 rpm; preferably 110 rpm to 1200 rpm; more preferably 150 rpm to 1100 rpm; even more preferably 200 rpm to 1000 rpm; most preferably 300 rpm to 900 rpm; and even most preferably 320 to 800 rpm or 350 to 1200 rpm.

[0129] In a twin-screw extruder with a screw diameter of 18 mm, the preferred screw speed is higher than 500 rpm; in a twin-screw extruder with a screw diameter of 58 mm, the preferred screw speed is higher than 250 rpm.

[0130] For example, step (c) of extruding the initial polyethylene-containing material comprises extruding with a residence time in the range of 10 seconds to 10 minutes; preferably with a residence time in the range of 20 seconds to 5 minutes; more preferably with a residence time in the range of 10 to 180 seconds, or 10 to 120 seconds, or 20 to 100 seconds, or 30 to 80 seconds.

[0131] Initial polyethylene-containing material and step b) of providing an initial polyethylene-containing material

[0132] The process according to the present disclosure comprises a step b) of providing an initial polyethylene-containing material comprising at least 50 wt.-% polyethylene, based on the total weight of the initial polyethylene-containing material.

[0133] The initial polyethylene-containing material may be an original polyethylene-containing material, a recycled polyethylene-containing material, or a mixture of an original polyethylene-containing material and a recycled polyethylene-containing material. In some embodiments, the initial polyethylene-containing material is a recycled polyethylene-containing material. As used herein, the term "recycled polyethylene composition" encompasses both post-consumer resins (PCR) and post-industrial resins (PIR).

[0134] Suitable polyethylenes include, but are not limited to, homopolymers of ethylene, copolymers of ethylene and higher α-olefin comonomers. Therefore, preferably, the polyethylene in the initial polyethylene-containing material is one or more polyethylene homopolymers, one or more polyethylene copolymers, and any mixtures thereof.

[0135] The term "copolymer" refers to a polymer made by connecting two different types of monomers in the same polymer chain. Preferred comonomers are alpha-olefins having 3 to 20 carbon atoms or 3 to 10 carbon atoms. More preferred comonomers are selected from propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, and any mixture thereof. Even more preferred comonomers are selected from 1-butene, 1-hexene, 1-octene, and any mixture thereof. The most preferred comonomer is 1-hexene.

[0136] The term "homopolymer" refers to a polymer made by joining only one monomer in the absence of a comonomer. Thus, ethylene homopolymers are substantially free of any comonomer. "Substantially free" means that no comonomer is intentionally added during the production of the polyethylene, but may still be present up to 0.2 wt%, preferably up to 0.1 wt%, and most preferably up to 0.05 wt%, relative to the total weight of the polyethylene.

[0137] The initial polyethylene-containing material is selected to contain at least 50% polyethylene by weight based on the total weight of the initial polyethylene-containing material. Preferably, the initial polyethylene-containing material is selected to contain at least 55% polyethylene by weight based on the total weight of the initial polyethylene-containing material; preferably, at least 60%; preferably, at least 70%; preferably, at least 80%; preferably, at least 90%; preferably, at least 95% polyethylene by weight.

[0138] In one embodiment, the initial polyethylene-containing material is a virgin material and consists of polyethylene (ie, comprises 100 wt. % polyethylene).

[0139] In one embodiment, the initial polyethylene-containing material is a recycled polyethylene-containing material. The recycled polyethylene-containing material may contain one or more polymers different from polyethylene.

[0140] In one embodiment, and in particular wherein the initial polyethylene-containing material is a recycled polyethylene-containing material; the initial polyethylene-containing material comprises at least one polymer different from polyethylene in an amount ranging from 0 to 50 wt. % based on the total weight of the initial polyethylene-containing material; wherein the at least one polymer different from polyethylene is selected from polypropylene (PP), polyacrylate (PA), polyethylene terephthalate (PET), polystyrene (PS), polylactic acid (PLA), and any mixture thereof.

[0141] Preferably, the initial polyethylene-containing material comprises at least one polymer different from polyethylene in an amount ranging from 0 to 40 wt.-%; preferably 0.1 to 20 wt.-%; more preferably 0.2 to 10 wt.-%; and even more preferably 0.5 to 5 wt.-%, based on the total weight of the initial polyethylene-containing material.

[0142] For example, PCR polyethylene typically contains a small fraction of polypropylene (eg, less than 5 wt %).

[0143] In one embodiment, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a high load melt index (HLMI R) of at least 1.0 g / 10 min; preferably at least 1.2 g / 10 min; more preferably at least 1.5 g / 10 min, when measured at 190°C under a load of 21.6 kg according to ISO 1133-2011.

[0144] In one embodiment, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a melt index (MI2 R) of at least 0.10 g / 10 min; preferably at least 0.15 g / 10 min; more preferably at least 0.2 g / 10 min; even more preferably at least 0.5 g / 10 min, most preferably at least 0.8 g / 10 min, and even most preferably at least 0.9 g / 10 min, or at least 1.0 g / 10 min, when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg.

[0145] For example, the initial polyethylene-containing material is selected to have a melt index ranging from a high load melt index (HLMI R) of at least 1.0 g / 10 minutes when measured at 190°C under a load of 21.6 kg according to ISO 1133-2011 to a melt index (MI2 R) of at most 3.0 g / 10 minutes when measured at 190°C under a load of 2.16 kg according to ISO 1133-2011.

[0146] In one embodiment, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a melt index (MI2R) of at most 3.0 g / 10 min; preferably at most 2.8 g / 10 min; more preferably at most 2.5 g / 10 min; even more preferably at most 2.2 g / 10 min, most preferably at most 2.0 g / 10 min, and even most preferably at most 1.8 g / 10 min, or at most 1.6 g / 10 min, when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg.

[0147] For example, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a molecular weight of at least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012. 3 density.

[0148] In one embodiment, the initial polyethylene-containing material is selected to have a high load melt index (HLMI R) of at least 1.0 g / 10 minutes when measured according to ISO 1133-2011 at 190°C under a load of 21.6 kg, a melt index (MI2R) of at most 0.45 g / 10 minutes when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg, and a melt index (MI2R) of at least 0.940 g / cm2 when measured according to ISO 1183-1:2012 at 23°C. 3 density.

[0149] For example, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a molecular weight of at least 0.940 g / cm2 when measured at 23°C according to ISO 1183-1:2012. 3 ; preferably, at least preferably, at least 0.945 g / cm 3 More preferably, at least 0.948 g / cm 3 ; even more preferably at least 0.950 g / cm 3 ; and most preferably at least 0.951 g / cm 3 density.

[0150] For example, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a molecular weight of at most 0.965 g / cm 3 ; Preferably, at most 0.962g / cm 3 ; and more preferably, at most 0.960 g / cm 3 density.

[0151] For example, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a molecular weight in the range of 0.940 g / cm 3 Up to 0.965g / cm 3 ; Preferably, the range is 0.942g / cm 3 Up to 0.964g / cm 3 More preferably, the range is 0.945 g / cm 3 Up to 0.962g / cm 3; and even more preferably, in the range of 0.948 g / cm 3 Up to 0.960g / cm 3 density.

[0152] For example, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a melt index ranging from a high load melt index (HLMI R) of at least 1.0 g / 10 min when measured at 190°C under a load of 21.6 kg according to ISO 1133-2011 to a melt index (MI2 R) of at most 0.45 g / 10 min when measured at 190°C under a load of 2.16 kg according to ISO 1133-2011.

[0153] For example, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a high load melt index (HLMI R) of at least 1.0 g / 10 min; preferably at least 1.2 g / 10 min; more preferably at least 1.5 g / 10 min, when measured according to ISO 1133-2011 at 190°C under a load of 21.6 kg.

[0154] For example, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a melt index (MI2 R) of at most 0.45 g / 10 min; preferably, at most 0.42 g / 10 min; more preferably at most 0.40 g / 10 min; even more preferably in the range of at most 0.35 g / 10 min, when measured according to ISO 1133-2005 at 190°C under a load of 2.16 kg.

[0155] In another embodiment, the initial polyethylene-containing material is selected to have a melt index (MI2 R) in the range of 0.8 to 1.5 g / 10 minutes when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg, and in the range of 0.910 g / cm2 when measured according to ISO 1183-1:2012 at 23°C. 3 To less than 0.940g / cm 3 ; The preferred range is 0.910g / cm 3 Up to 0.935g / cm 3 , and the more preferred range is 0.910 g / cm 3 Up to 0.930g / cm 3 density.

[0156] Preferably, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a molecular weight of at least 0.910 g / cm3 ; preferably, at least preferably, at least 0.912 g / cm 3 More preferably, at least 0.915 g / cm 3 ; and even more preferably at least 0.916 g / cm 3 density.

[0157] For example, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a molecular weight of less than 0.940 g / cm2 when measured at 23°C according to ISO 1183-1:2012. 3 ; Preferably, at most 0.935g / cm 3 More preferably, at most 0.930 g / cm 3 ; Even more preferably, at most 0.928 g / cm 3 ; and most preferably, at most 0.925 g / cm 3 density.

[0158] For example, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a molecular weight in the range of 0.910 g / cm 3 To less than 0.940g / cm 3 ; Preferably, the range is 0.910g / cm 3 Up to 0.935g / cm 3 More preferably, the range is 0.910 g / cm 3 Up to 0.930g / cm 3 ; Even more preferably in the range of 0.912 g / cm 3 Up to 0.928g / cm 3 ; Most preferably, the range is 0.915g / cm 3 Up to 0.925g / cm 3 ; and even more preferably, in the range of 0.916 g / cm 3 Up to 0.925g / cm 3 density.

[0159] For example, when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a melt index (MI2R) in the range of 0.8 to 1.5 g / 10 minutes; preferably, in the range of 0.8 to 1.4 g / 10 minutes; more preferably in the range of 0.9 to 1.3 g / 10 minutes; even more preferably in the range of 1.0 to 1.2 g / 10 minutes.

[0160] In some embodiments, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has an Mz / Mw of at least 4.0; preferably, ranging from 4.0 to 50.0; preferably, 5.0 to 25.0; preferably, 7.0 to 15.0, when determined by gel permeation chromatography.

[0161] In some embodiments, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a complex viscosity at 0.1 rad / s at 190°C in the range of 20,000 to 80,000 Pa·s; preferably, in the range of 22,000 to 70,000 Pa·s; more preferably, in the range of 25,000 to 60,000 Pa·s; and even more preferably, in the range of 30,000 to 50,000 Pa·s.

[0162] In some embodiments, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a Mw / Mn in the range of 5.0 to 30.0; preferably in the range of 6.0 to 20.0; preferably in the range of 7.0 to 15.0, when determined by gel permeation chromatography.

[0163] In some embodiments, the initial polyethylene-containing material or the polyethylene in the initial polyethylene-containing material has a complex viscosity ratio of 10 or more; preferably, a complex viscosity ratio of at least 11; more preferably, a complex viscosity ratio of at least 12.

[0164] In one embodiment, the initial polyethylene-containing material further has a tan δ (G" / G' measured at 0.1 rad / sec at 190°C) of at most 3.0; preferably at most 2.6.

[0165] In one embodiment, the initial polyethylene-containing material further has a tan δ (G" / G' measured at 0.1 rad / sec at 190°C) ranging from 0.5 to 3.0; preferably, 0.8 to 2.6.

[0166] The polyethylene composition obtained and step d) collecting the polyethylene composition

[0167] Step d) comprises recovering the polyethylene composition as a treated initial polyethylene-containing material.

[0168] For example, when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg, the polyethylene composition has a melt index (MI2 T) in the range of 3.0 to 60.0 g / 10 minutes. For example, when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg, the polyethylene composition has a melt index (MI2 T) in the range of 3.5 to 40.0 g / 10 minutes; preferably, in the range of 4.0 to 20.0 g / 10 minutes; more preferably, in the range of 4.5 to 15.0 g / 10 minutes; even more preferably in the range of 5.0 to 10.0 g / 10 minutes.

[0169] The polyethylene composition corresponds to the treated initial material; wherein the melt index is increased. However, unexpectedly, the treatment performed also provides other characteristics to the polyethylene composition, making it particularly suitable for injection molding.

[0170] In particular, the polyethylene composition is found to have a ratio of the complex viscosity at a frequency of 0.01 rad / s to the complex viscosity at a frequency of 100 rad / s of at most 10; preferably, at most 9.0; more preferably, at most 8.5; even more preferably, at most 8.0; and most preferably, at most 7.0, said ratio being measured at 190°C.

[0171] In one embodiment, the polyethylene composition has a complex viscosity at 0.1 rad / s at 190°C of at most 20,000 Pa·s; preferably at most 18,000 Pa·s; more preferably at most 15,000 Pa·s; even more preferably at most 12,000 Pa·s; most preferably at most 10,000 Pa·s; and even most preferably at most 9,000 Pa.s; or at most 8,000 Pa.s, or at most 5,000 Pa.s.

[0172] In one embodiment, the polyethylene composition has a complex viscosity at 0.1 rad / s at 190°C in the range of 200 to 20,000 Pa.s; preferably 250 to 18,000 Pa.s; more preferably 300 to 15,000 Pa.s; even more preferably 400 to 12,000 Pa.s; most preferably 410 to 10,000 Pa.s; and even most preferably 410 to 9,000 Pa.s; or 400 to 8,000 Pa.s, or 400 to 5,000 Pa.s.

[0173] Preferably, the polyethylene composition has a Mz / Mw, when determined by size exclusion chromatography, of at most 7.0; preferably at most 6.0; preferably at most 5.0.

[0174] For example, the polyethylene composition further has a Mw / Mn, when determined by size exclusion chromatography, ranging from 2.5 to 10.0; preferably from 2.6 to 8.0; more preferably from 2.7 to 6.0; even more preferably from 2.8 to 5.0 or 2.9 to 4.5.

[0175] For example, the polyethylene composition further has a tan δ (G" / G') at 0.1 rad at 190°C of above 2.5; preferably at least 3.0; more preferably at least 5.0, and even more preferably at least 10.0.

[0176] The polyethylene composition has a density that is higher than the density of the initial polyethylene-containing material.

[0177] For example, the polyethylene composition has a hardness of at least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012. 3 For example, when measured at 23°C according to ISO 1183-1:2012, the polyethylene composition has a density of at least 0.912 g / cm 3 ; preferably, at least preferably, at least 0.915 g / cm 3 More preferably, at least 0.918 g / cm 3 ; even more preferably at least 0.920 g / cm 3 ; and most preferably, at least 0.930 g / cm 3 density.

[0178] In one embodiment, the polyethylene composition has a molecular weight of at most 0.965 g / cm2 when measured at 23°C according to ISO 1183-1:2012. 3 ; Preferably, at most 0.962g / cm 3 ; and more preferably, at most 0.960 g / cm 3 ; and even more preferably, at most 0.958 g / cm 3 density.

[0179] For example, when measured according to ISO 1183-1:2012 at 23°C, the polyethylene composition has a range of 0.920 g / cm 3 Up to 0.965g / cm 3 ; Preferably, the range is 0.930g / cm 3 Up to 0.960g / cm 3 density.

[0180] In one embodiment, the polyethylene composition has a hardness of at least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012. 3; preferably, at least preferably, at least 0.912 g / cm 3 More preferably, at least 0.915 g / cm 3 ; and even more preferably, at least 0.916 g / cm 3 For example, when measured at 23°C according to ISO 1183-1:2012, the polyethylene composition has a density of at most 0.930 g / cm 3 ; Preferably, at most 0.928g / cm 3 ; and more preferably, at most 0.925 g / cm 3 For example, when measured at 23°C according to ISO 1183-1:2012, the polyethylene composition has a density in the range of 0.910 g / cm 3 To less than 0.940g / cm 3 ; Preferably, the range is 0.910g / cm 3 Up to 0.935g / cm 3 More preferably, the range is 0.910 g / cm 3 Up to 0.930g / cm 3 Even more preferably, the range is 0.912 g / cm 3 Up to 0.928g / cm 3 ; Most preferably, the range is 0.915g / cm 3 Up to 0.925g / cm 3 ; and even more preferably, in the range of 0.916 g / cm 3 Up to 0.925g / cm 3 density.

[0181] In one embodiment, the polyethylene composition has a hardness of at least 0.940 g / cm2 when measured at 23°C according to ISO 1183-1:2012. 3 ; preferably, at least preferably, at least 0.945 g / cm 3 More preferably, at least 0.948 g / cm 3 Even more preferably, at least 0.950 g / cm 3 ; and most preferably, at least 0.951 g / cm 3 For example, when measured at 23°C according to ISO 1183-1:2012, the polyethylene composition has a density of at most 0.965 g / cm 3 ; Preferably, at most 0.962g / cm 3 ; and more preferably, at most 0.960 g / cm 3For example, when measured at 23°C according to ISO 1183-1:2012, the polyethylene composition has a density in the range of 0.940 g / cm 3 Up to 0.965g / cm 3 ; Preferably, the range is 0.942g / cm 3 Up to 0.964g / cm 3 More preferably, the range is 0.945 g / cm 3 Up to 0.962g / cm 3 ; and even more preferably, in the range of 0.948 g / cm 3 Up to 0.960g / cm 3 density.

[0182] In one embodiment, the polyethylene composition recovered in step (d) has one or more selected from the group consisting of:

[0183] - At least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012 3 density; and / or

[0184] - a melt index MI2 ranging from 3.0 to 60.0 g / 10 min when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg; and / or

[0185] - an unsaturation index greater than 2,000, wherein the unsaturation index is the product of the units of vinyl unsaturation per 1,000 carbon atoms and the Mn in Daltons when determined by ASTM D6248-98:2004; and / or

[0186] - A complex viscosity at 0.1 rad / s at 190° C. of at most 20,000 Pa·s.

[0187] In a preferred embodiment, the polyethylene composition recovered in step (d) has:

[0188] - At least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012 3 density;

[0189] - a melt index MI2 ranging from 3.0 to 60.0 g / 10 minutes when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg;

[0190] - an unsaturation index greater than 2,000, wherein the unsaturation index is the product of the units of vinyl unsaturation per 1,000 carbon atoms and the Mn in Daltons when determined by ASTM D6248-98:2004; and

[0191] - A complex viscosity at 0.1 rad / s at 190° C. of at most 20,000 Pa·s.

[0192] For example, the polyethylene composition further has a VOC content that is lower than the VOC content of the initial polyethylene-containing material.

[0193] VOC is the amount of volatile organic compounds (VOC) in ppm, where the volatile compounds are defined as having chains of 12 carbon atoms or less. This reduction in VOC is beneficial, but it takes a very significant reduction in such levels to eliminate odor.

[0194] The present disclosure encompasses an article produced from the polyethylene composition as defined above, wherein the article is an injection molded article; preferably, the article is selected from a bottle or a container.

[0195] For example, the article is produced using 40 wt% to 100 wt% of the original polyethylene-containing material that is recycled polyethylene-containing, and has a lower VOC content than the original polyethylene-containing material.

[0196] Test Method

[0197] Polyethylene Melt flow index MI2 Determined according to ISO 1133-2011 at 190°C under a load of 2.16 kg.

[0198] Polyethylene HLMI Determined according to ISO 1133-2011 at 190°C under a load of 21.6 kg.

[0199] Mn, Mw, Mz, Mw / Mn and Mz / Mw : Molecular weight (M) was determined by size exclusion chromatography (SEC) n (number average molecular weight), M w(weight average molecular weight) and molecular weight distribution D (Mw / Mn). Briefly, GPC-IR5 from Polymer Char was used: 10 mg of polyethylene sample was dissolved in 10 ml of trichlorobenzene at 160°C for 1 hour. Injection (sample injection) volume: about 400 μl, automatic sample preparation, and injection temperature: 160°C. Column temperature: 145°C. Detector temperature: 160°C. Two Shodex AT-806MS (ShowaDenko) and one Styragel HT6E (Waters) columns were used, with a flow rate of 1 ml / min (eluent: trichlorobenzene). Detector: infrared detector (2800-3000cm -1 Calibration: narrow standard of polystyrene (PS) (commercially available). The molecular weight Mi of each fraction i of the eluted polyethylene was calculated based on the Mark-Houwink relationship (log 10 (M PE ) = 0.965909 x log 10 (M PS )–0.28264)(in M PE =1000 at the low molecular weight end cutoff).

[0200] The average molecular weight used to establish molecular weight / property relationships is the number average (M n ), weight average (M w ) and z average (M z ) molecular weight. These averages are defined by the following expressions and are calculated from the M i Sure:

[0201]

[0202] Here N i and W i are the number and weight of molecules with molecular weight Mi, respectively. The third representation (rightmost) in each case defines how these averages were obtained from the SEC chromatogram. i is the height of the SEC curve at the i-th elution fraction (from the baseline), and M i is the molecular weight of the species eluting in that increment.

[0203] Then Molecular weight distribution (MWD) is calculated as Mw / Mn.

[0204] 13 C-NMR analysisThe signal intensity in the spectrum is proportional to the total number of carbon atoms contributed in the sample using a 400MHz or 500MHz Bruker NMR spectrometer. These conditions are well known to those skilled in the art and include, for example, sufficient relaxation time, etc. In practice, the intensity of the signal is obtained from its integral (i.e., the corresponding area). The data are obtained using proton decoupling, 2000 to 4000 scans per spectrum of a 10 mm room temperature probe (room temperature through) or 240 scans per spectrum of a 10 mm cryoprobe, a pulse repetition delay of 11 seconds, and a spectral width of 25000Hz (+ / -3000Hz). The sample is prepared by: a sufficient amount of polymer is dissolved in 1,2,4-trichlorobenzene (TCB, 99%, spectral grade) at 130°C and occasionally stirred to homogenize the sample, followed by the addition of hexadeuterated benzene (C6D6, spectral grade) and a small amount of hexamethyldisiloxane (HMDS, 99.5+%), wherein HMDS serves as an internal standard. As an example, about 200 mg to 600 mg of polymer was dissolved in 2.0 mL of TCB, followed by the addition of 0.5 mL of C6D6 and 2 to 3 drops of HMDS.

[0205] After data acquisition, the chemical shifts were referenced to the signal of the internal standard HMDS, which was assigned a value of 2.03 ppm.

[0206] The comonomer content in the polyethylene was determined by the method described by GJ Ray et al. (Macromolecules, 1977, 10, (4), 773-778) by precipitating the pellets. 13 The content of MgCl2O3 was determined by C-NMR analysis.

[0207] Crystallization temperature (Tc) and Melting temperature (Tm) According to ISO 11357-3:2018, it is measured on a DSCQ2000 instrument from TA Instruments. To eliminate the thermal history, the sample is first heated to 220°C and kept at 220°C for 3 minutes. The polymer is then cooled to a maximum of 20°C at -20°C / min and kept at 20°C for 3 minutes. The crystallization temperature is determined during this cooling step. The crystallization temperature Tc corresponds to the temperature of the extreme value of the spectrum, which presents the heat flux associated with the polymer as a function of the temperature during its cooling. The polymer is then melted at 20°C / min to a maximum of 220°C, and the melting temperature is determined during this heating step. The melting temperature corresponds to the temperature of the extreme value of the spectrum, which presents the heat flux associated with the polymer as a function of the temperature during its melting.

[0208] Measured according to the method of standard ISO 1183-1:2012 (immersion method) at a temperature of 23°C density .

[0209] Complex Shear Modulus and Viscosity :Complex shear modulus G*(w)=G'(w)+jG”(w)(J 2 = -1, G'(w): storage modulus and G"(w): loss modulus) were measured using DHR-2 (stress-controlled rheometer from TA Instruments). The rheometer was set at 190°C under nitrogen flow from 100 to 0.01 rad.s -1 The frequency sweep was performed in the linear domain (1% strain) to prevent thermo-oxidative degradation. The geometry used was a 25 mm diameter parallel plate with a 2 mm gap. The samples (25 mm diameter, 2 mm thickness) used for these experiments were previously obtained using an injection press (Babyplast model).

[0210] Complex viscosity η * (ω) is calculated according to the following formula of linear viscoelasticity:

[0211]

[0212] Example

[0213] The following non-limiting examples illustrate the present disclosure.

[0214] PE1 = Polyethylene HDPE 5502 commercialized by TotalEnergies. Density according to ISO 1183-1:2012 is 0.954 g / cm 3 ; MI2 according to ISO 1133-2011 (190° C., 2.16 kg) is 0.25 g / 10 min; HLMI according to ISO 1133-2011 (190° C., 21.6 kg) is 22 g / 10 min. The polyethylene is produced using a chromium-based catalyst.

[0215] The storage modulus (G') at 0.1 radian and at 190°C was measured to be 1,855 Pa, and the loss modulus (G") at 0.1 radian and at 190°C was measured to be 2,798 Pa; resulting in a tan delta (G" / G') of 1.5.

[0216] From a melt index point of view, PE1 was chosen because it represents the melt index of a recycled polyethylene flux, which makes sense to convert to an injection (recycled) grade.

[0217] Example 1: Machining

[0218] The extruder used in the experiments was a Leistritz ZSE 18HPe. The screw design was modified from the standard configuration as follows Figure 1The PTE1 and PTE2 screw designs shown in . Both the PTE1 and PTE2 screw designs include two left-handed screw sections, one in the Z2 zone and one in the Z5 zone. Z2 is the melting zone and Z5 is the mixing zone. Both the PTE1 and PTE2 screws are designed with a section with a kneading block in Z4 (i.e. placed between the two left-handed screw sections).

[0219] In the first experiment, extrusion was performed at different screw speeds, with a fixed flow rate of 1.5 kg / h and a temperature profile as shown in Table 1. These temperatures correspond to the values ​​applied during the start-up of the test. When progressing to stable conditions, the barrel temperature exceeds these targets due to the conversion of mechanical heat in the barrel into polymer heat. When the temperature in a zone exceeds the target by more than 10°C, the temperature regulation in that zone will be turned off, and the temperature of the zone can increase and stabilize to a higher value.

[0220] Table 1

[0221]

[0222] Figure 2 The results on MI2 are provided in (polymer analysis was performed when stable conditions were reached), where it can be seen that it was already possible to increase the initial MI2 of 0.2 g / 10 min up to about 10 g / 10 min (a factor of 50). The polyethylene composition obtained exhibited an unsaturation index of about 13,700.

[0223] In the second experiment, extrusion was performed at different screw speeds, with a fixed flow rate of 2.5 kg / h and the temperature profiles shown in Table 2. Here, these temperatures also correspond to the values ​​applied during the start-up of the test. When progressing to stable conditions, the barrel temperature exceeds these targets due to the conversion of mechanical heat in the barrel into polymer heat. When the temperature in a zone exceeds the target by more than 10°C, the temperature regulation in this zone will be turned off, and the temperature of the zone can increase and stabilize to a higher value.

[0224] Table 2

[0225]

[0226] MI2 results are available at Figure 3 In the example (polymer analysis was performed when stable conditions were reached), it can be seen that it was already possible to increase the initial MI2 of 0.2 g / 10 min up to about 16 g / 10 min (factor 80). The polyethylene composition obtained exhibited an unsaturation index of about 13,500.

[0227] Example 2: Thermal Processing

[0228] A series of experiments were then carried out in which heat treatment was performed by heating the material at temperatures increasing from 320°C to 390°C. The experiments were carried out at screw speeds of 400 and 800 rpm. Figure 4 The complex viscosities obtained on the treated samples are reported in and compared with the starting material HDPE 5502. From the results it can be seen that a significant reduction in the complex viscosity is obtained. The complex viscosity ratio of HDPE 5502 (about 13) drops below 8 for all samples treated at 340°C or higher.

[0229] Figure 5 The increase in tan δ (G" / G') obtained for the treated material is shown.

Claims

1. A process for treating an initial polyethylene-containing material to produce a polyethylene composition, characterized in that It includes the following steps: a) providing a twin screw extruder with a heat regulating device; b) providing an initial polyethylene-containing material comprising at least 50 wt. % polyethylene, based on the total weight of the initial polyethylene-containing material; c) extruding the initial polyethylene-containing material to obtain a polyethylene composition; wherein the extrusion is performed with a residence time of less than 20 minutes; and d) collecting the polyethylene composition; wherein the extrusion step (c) comprises heat treating the initial polyethylene-containing material at a temperature of at least 300°C by self-heating of the material in one or more hot zones of the extruder, wherein the one or more hot zones have a total length equal to or greater than 6D, wherein D is the screw diameter, wherein the extrusion is carried out with a mechanical specific energy greater than or equal to 0.4 kWh / kg, wherein the screw profile comprises at least one hot zone having a succession of kneading block elements followed by left-handed elements over a length of at least 4D, wherein D is the screw diameter, wherein the heat regulating device is set to an initial applied barrel temperature in the range between 240 and 320°C and is closed when the barrel temperature in the zone spontaneously exceeds the applied barrel temperature by at least 3°C ​​without the need for external heat application.

2. The process according to claim 1, characterized in that The heat treatment is carried out by self-heating of the material and in that the screw profile comprises two or more hot zones, wherein the first hot zone comprises a succession of kneading block elements over a length of at least 4D followed by left-handed elements, wherein D is the screw diameter, and one or more additional hot zones located downstream of the first hot zone are filled mixing zones, each comprising a kneading block element over a length of at least 4D followed by a kneading left-handed element or a left-handed element, wherein D is the screw diameter.

3. The process according to claim 1 or 2, characterized in that The heat treatment is performed by self-heating of the material and the successive kneading block elements of at least one hot zone of the extruder comprise disks having a disk offset of 90 degrees and a disk width of at least 0.3D, where D is the screw diameter.

4. The process according to any one of claims 1 to 3, characterized in that A hot zone of the extruder is or comprises the melt zone of the extruder.

5. The process according to any one of claims 1 to 4, characterized in that The initial polyethylene-containing material is selected to have a high load melt index (HLMI R) of at least 1.0 g / 10 minutes when measured according to ISO 1133-2011 at 190°C under a load of 21.6 kg.

6. The process according to any one of claims 1 to 5, characterized in that The initial polyethylene-containing material is selected to have a melt index (MI2 R) of at most 3.0 g / 10 minutes when measured according to ISO 1133-2011 at 190° C. under a load of 2.16 kg.

7. The process according to any one of claims 1 to 6, characterized in that The initial polyethylene-containing material is selected to have a molecular weight of at least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012. 3 density.

8. The process according to any one of claims 1 to 7, characterized in that The initial polyethylene-containing material is selected to have a high load melt index (HLMI R) of at least 1.0 g / 10 min when measured according to ISO 1133-2011 at 190°C under a load of 21.6 kg, a melt index (MI2 R) of at most 0.45 g / 10 min when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg, and a melt index (MI2 R) of at least 0.940 g / cm2 when measured according to ISO 1183-1:2012 at 23°C. 3 density.

9. The process according to any one of claims 1 to 7, characterized in that The initial polyethylene-containing material is selected to have a melt index (MI2 R) in the range of 0.8 to 1.5 g / 10 min when measured according to ISO 1133-2011 at 190° C. under a load of 2.16 kg, and in the range of 0.910 g / cm2 when measured according to ISO 1183-1:2012 at 23° C. 3 Up to 0.930g / cm 3 density.

10. The process according to any one of claims 1 to 9, characterized in that The ratio of the melt index of the polyethylene composition (MI2 T) to the melt index of the initial polyethylene-containing material (MI2 R) is at least 10.

11. The process according to any one of claims 1 to 10, characterized in that The polyethylene composition recovered in step d) has a melt index (MI2 T) ranging from 3.0 to 60.0 g / 10 min; preferably ranging from 4.0 to 20.0 g / 10 min when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg.

12. The process according to any one of claims 1 to 11, characterized in that The initial polyethylene-containing material comprises at least 80 wt% polyethylene, based on the total weight of the initial polyethylene-containing material.

13. The process according to any one of claims 1 to 12, characterized in that The initial polyethylene-containing material is a recycled polyethylene-containing material.

14. The process according to any one of claims 1 to 13, characterized in that The step (c) of extruding the initial polyethylene-containing material comprises extruding with a residence time ranging from 10 to 180 seconds.

15. The process according to any one of claims 1 to 14, characterized in that The step (c) of extruding said initial polyethylene-containing material comprises a heat treatment at a temperature ranging from 320 to 460°C.

16. The process according to any one of claims 1 to 15, characterized in that The polyethylene composition recovered in step (d) has: - At least 0.910 g / cm2 when measured at 23°C according to ISO 1183-1:2012 3 density; - a melt index MI2 ranging from 3.0 to 60.0 g / 10 minutes when measured according to ISO 1133-2011 at 190°C under a load of 2.16 kg; - an unsaturation index greater than 2,000, wherein the unsaturation index is the product of the units of vinyl unsaturation per 1,000 carbon atoms and the Mn in Daltons when determined by ASTM D6248-98:2004; and - A complex viscosity at 0.1 rad / s at 190° C. of at most 20,000 Pa·s.

17. A method for producing an injection molded product, characterized in that: The method comprises producing a polyethylene composition from an initial polyethylene-containing material according to the process according to any one of claims 1 to 16, and producing an injection molded article using the polyethylene composition obtained by the process; preferably, the initial polyethylene-containing material is a recycled polyethylene-containing material.

Citation Information

Patent Citations

  • High-density polyethylene compositions, method of making the same, articles made therefrom, and method of making such articles

    CN101356225A

  • Oxygen tailoring of polyethylene

    CN104271612A

  • Method for preparing cross-linkable polyethylene modified material

    CN107814996A

  • Process for reducing the weight average molecular weight and melt index ratio of polyethy lenes and polyethylene products

    CN1423663A

  • Polyethylene composition

    JP1988213539A