High flow polypropylene composition for injection molding applications

By adjusting the elastomer phase performance of the heterophase polypropylene copolymer and adding a granular inorganic nucleating agent, the problem of insufficient balance of high flowability and impact performance of heterophase polypropylene copolymer in automotive applications in the prior art is solved, and the problem of insufficient balance of high flowability and impact performance in automobile applications is achieved. The high performance balance of polypropylene compositions is suitable for injection molded automotive products.

CN118900851AActive Publication Date: 2024-11-05北欧化工公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380028416.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-21
Publication Date
2024-11-05
Estimated Expiration
2043-03-21

Smart Images

  • Figure BDA0005047906640000171
    Figure BDA0005047906640000171
  • Figure BDA0005047906640000211
    Figure BDA0005047906640000211
  • Figure BDA0005047906640000212
    Figure BDA0005047906640000212
Patent Text Reader

Abstract

The present invention relates to a polypropylene composition having a melt flow rate MFR2 of 75 to 250 g / 10 min, comprising a heterophasic propylene copolymer and a particulate inorganic nucleating agent, which is particularly suitable for injection molding applications. The invention also relates to a method for producing said polypropylene composition, to an article comprising said polypropylene composition, and to the use of said polypropylene composition for injection molding articles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polypropylene composition having a melt flow rate (MFR) of 2 The polypropylene copolymer has a molecular weight of 75-250 g / 10 min and is particularly suitable for injection molding applications. The polypropylene copolymer comprises a heterophasic propylene copolymer and a particulate inorganic nucleating agent. Background Art

[0002] Heterophasic propylene copolymers are widely used in the automotive industry due to their excellent combination of stiffness and impact properties. There are currently two development trends in the automotive industry:

[0003] - Weight reduction requires thin-walled structures and the need to keep mineral reinforcements to a low level.

[0004] - Using post-industrial or even post-consumer recycled materials, which have lower MFR and limited impact strength, requires the addition of other components in the final composition.

[0005] To meet these requirements, it is necessary for compositions suitable for automotive applications to have high flow, as manifested by a high melt flow rate, high toughness after processing, as manifested by a low initial coefficient of linear thermal expansion (CLTE), good impact properties, especially at low temperatures, as manifested by high Charpy notched impact strength and instrumented puncture tests, and high stiffness, as manifested by a high tensile modulus.

[0006] The properties of the composition can be adjusted by introducing polymer components which are adapted to the properties of the elastomeric phase of one or more heterophasic polypropylene copolymers (e.g. elastomeric polymers like plastic plastomers) and / or which are adapted to the properties of the matrix phase of one or more heterophasic polypropylene copolymers (e.g. propylene homogeneous or random copolymers).

[0007] However, by adjusting the properties of one or more heterophasic polypropylene copolymers as major components of the composition, more pronounced effects can be obtained.

[0008] WO 2017 / 148970 A1 discloses heterophasic propylene copolymers comprising a multimodal matrix phase that can have a higher melt flow rate. However, the examples show that a high melt flow rate of at least 70 g / 10 min exhibits poor tensile and impact balance properties, especially at low temperatures.

[0009] Therefore, there is a need in the art for new heterophasic polypropylene copolymers suitable as the main component of polypropylene compositions suitable for injection molding applications. It has been found that by carefully adjusting the properties of the heterophasic polypropylene copolymers, in particular the properties of the elastomeric phase, compositions having an excellent balance of properties can be obtained, including high flowability (expressed by high melt flow rate) and high dimensional stability after processing (expressed by low initial linear thermal expansion coefficient (CLTE)), good impact properties (especially at low temperatures, expressed by high Charpy notched impact strength and instrumented puncture test), and high stiffness (expressed by high tensile modulus). These polypropylene compositions are suitable for injection molding applications, in particular automotive applications. Summary of the invention

[0010] Summary of the Invention

[0011] The present invention relates to a polypropylene composition, comprising:

[0012] (A) a heterophasic propylene copolymer in an amount of at least 95.0 wt%, such as from 95.0 to 99.9 wt%, preferably from 96.0 to 99.5 wt%, more preferably from 97.5 to 99.0 wt%; and

[0013] (B) a particulate inorganic nucleating agent, the content of which is up to 1.5 wt%, for example 0.01 to 1.5 wt%, preferably 0.1 to 1.3 wt%, more preferably 0.2 to 1.2 wt%.

[0014] All percentages refer to the total content and are

[0015] The heterophasic propylene copolymer (A) comprises a matrix phase and an elastomeric phase dispersed therein, and the composition has

[0016] (1) Soluble fraction (SF) and crystallite fraction (CF), determined by CRYSTEX QC analysis;

[0017] (2) a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 15.0 wt% to 30.0 wt%, preferably between 17.5 wt% and 27.5 wt%, more preferably between 20.0 wt% and 25.0 wt%;

[0018] (3) The ethylene content in the soluble fraction C2(SF) is quantified by 13 % by weight, preferably in the range of 27.5 to 37.5 wt %, more preferably in the range of 27.5 to 36.5 wt %;

[0019] (4) an intrinsic viscosity of the soluble fraction, iV(SF), measured in decalin at 135° C. according to DIN ISO 1628 / 1, of between 2.0 dl / g and 3.5 dl / g, preferably between 2.3 and 3.0 dl / g, more preferably between 2.5 and 2.9 dl / g;

[0020] (5) the ratio of the ethylene content of the soluble fraction to the crystallized fraction (C2(SF) / C2(CF)) is from 11.0 to 15.0, preferably from 11.5 to 15.0, more preferably from 12.0 to 15.0; and

[0021] (6) Melt flow rate (MFR) 2 (230°C, 2.16 kg, ISO 1133) is 75 to 250 g / 10 min, preferably 80 to 200 g / 10 min, more preferably 85 to 180 g / 10 min.

[0022] Furthermore, the present invention relates to a process for the preparation of the above or following polypropylene composition, wherein a heterophasic polypropylene copolymer (A) is polymerized in the presence of a Ziegler-Natta catalyst system in a multistage process comprising at least two polymerization reactors connected in series and the heterophasic polypropylene copolymer (A) is then blended with a particulate inorganic nucleating agent (B).

[0023] Furthermore, the present invention relates to an article, preferably a molded article, more preferably an injection molded article, still more preferably an injection molded automotive article comprising the above or below polypropylene composition.

[0024] Finally, the present invention relates to the use of the polypropylene composition as described above or below in injection moulded articles, preferably automotive articles.

[0025] definition

[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those of ordinary skill in the art to which the present invention belongs. Although methods and materials similar or equivalent to those described herein can be used to practice and test the present invention, preferred methods and materials are described herein. When describing and claiming the present invention, the following terms will be used according to the following definitions. Unless explicitly stated, the use of words such as "a", "an" refers to one or more.

[0027] A polymer blend is a mixture of two or more polymer components. Generally, a blend can be prepared by mixing two or more polymer components. A suitable mixing procedure known in the art is post-polymerization blending.

[0028] Post-polymerization blending may be dry blending of the polymer components (eg, polymer powders and / or composite polymer pellets), or may be melt blending, for example, by melt mixing the polymer components.

[0029] Propylene homopolymer is a polymer mainly composed of propylene monomer units. Due to the presence of impurities, especially in commercial polymerization processes, propylene homopolymer may contain up to 0.1 mol% of comonomer units, preferably up to 0.05 mol% of comonomer units, most preferably up to 0.01 mol% of comonomer units.

[0030] Polypropylene is a polymer consisting of propylene-derived units, the propylene content of which exceeds 50 mol%.

[0031] Polyethylene refers to a polymer consisting of ethylene-derived units, the ethylene content of which exceeds 50 mol%.

[0032] The term "elastomer" refers to a natural or synthetic polymer that has elastic properties. The term "plastomer" refers to a natural or synthetic polymer that combines the properties of an elastomer and a plastic, such as rubber-like properties and the processing capabilities of a plastic. Ethylene-based plastomers are plastomers composed of ethylene-derived units with an ethylene content of more than 50% by weight.

[0033] The presence of a multiphase nature can be readily determined by the number of glass transition points (e.g. in dynamic mechanical analysis (DMA)) and / or high resolution microscopy (e.g. scanning electron microscopy (SEM), transmission electron microscopy (TEM) or atomic force microscopy (AFM)).

[0034] "Multimodal", like "bimodal" or "trimodal", describes a probability distribution with multiple relative maxima. In particular, the term "modality of a polymer" refers to the form of its molecular weight distribution (MWD) curve, i.e. the appearance of a plot of the polymer weight fraction as a function of its molecular weight. If a polymer is produced in a sequential step process, i.e. using reactors coupled in a series configuration and using different conditions in each reactor, the different polymer fractions produced in the different reactors each have their own molecular weight distribution, which may differ significantly from each other. The molecular weight distribution curve obtained for the final polymer can be viewed as a superposition of the molecular weight distribution curves of the individual polymer fractions and will therefore show a distinct maximum or at least be significantly broader than the curves of the individual fractions. Polymers with such a molecular weight distribution curve are called bimodal, trimodal or multimodal, respectively.

[0035] The molecular weight distribution (MWD) curve of a polymer polymerized in a single polymerization stage or in a sequential step process using comparable polymerization conditions in each reactor generally shows a single maximum. Such polymers are considered to be unimodal.

[0036] The term "XCS" refers to the xylene cold soluble fraction (XCS wt %) measured at 25°C according to ISO 16152. The term "XCI" refers to the xylene cold insoluble fraction (XCI wt %) measured at 25°C according to ISO 16152.

[0037] Reactor blends are blends produced in two or more reactors coupled in series or in a reactor with two or more reaction chambers. Reactor blends can also be produced by blending in solution. Reactor blends are distinct from compounds produced by melt extrusion.

[0038] Unless otherwise indicated, "%" means weight percent (wt%). DETAILED DESCRIPTION

[0039] Composition

[0040] In a first aspect, the present invention relates to a polypropylene composition comprising:

[0041] (A) a heterophasic propylene copolymer in an amount of at least 95.0 wt%, such as from 95.0 to 99.9 wt%, preferably from 96.0 to 99.5 wt%, more preferably from 97.5 to 99.0 wt%; and

[0042] (B) a particulate inorganic nucleating agent, the content of which is up to 1.5 wt%, for example 0.01 to 1.5 wt%, preferably 0.1 to 1.3 wt%, more preferably 0.2 to 1.2 wt%.

[0043] wherein all percentages refer to the total content, the heterophasic propylene copolymer (A) comprises a matrix phase and an elastomeric phase dispersed therein, and

[0044] The composition has

[0045] (1) Soluble fraction (SF) and crystallite fraction (CF) determined by CRYSTEX QC analysis;

[0046] (2) According to CRYSTEX QC analysis, in the range of 15.0 wt% to 30.0 wt%, preferably 17.5 wt%

[0047] % to 27.5 wt%, more preferably 20.0 wt% to 25.0 wt% of the soluble fraction (SF);

[0048] (3) By quantitative 13 an ethylene content of the soluble fraction C2(SF) in the range of 25.0 to 40.0 wt.-%, preferably in the range of 27.5 to 37.5 wt.-%, more preferably in the range of 27.5 to 36.5 wt.-%, determined by FT-IR spectroscopy calibrated with C-NMR spectroscopy;

[0049] (4) an intrinsic viscosity of the soluble fraction iV (SF) of between 2.0 and 3.5 dl / g, preferably between 2.3 and 3.0 dl / g, more preferably between 2.5 and 2.9 dl / g, measured in decalin at 135° C. according to DIN ISO 1628 / 1;

[0050] (5) a ratio of the ethylene content of the soluble fraction to the crystallizate fraction (C2(SF) / C2(CF)) of 11.0 to 15.0, preferably 11.5 to 15.0, more preferably 12.0 to 15.0; and

[0051] (6) a melt flow rate (MFR) of 75 to 250 g / 10 min, preferably 80 to 200 g / 10 min, more preferably 85 to 180 g / 10 min 2 (230℃, 2.16kg, ISO 1133).

[0052] The composition suitable for automotive applications according to the present invention has one or more of the following characteristics:

[0053] The melt flow rate MFR of the composition 2 (230°C, 2.16 kg, ISO 1133) is 75 to 250 g / 10 min, preferably 80 to 200 g / 10 min, more preferably 85 to 180 g / 10 min.

[0054] The composition can be characterized by CRYSTEX QC analysis. In the CRYSTEX QC analysis, a crystallite fraction (CF) and a soluble fraction (SF) can be obtained, which can be quantified and analyzed according to the content of monomers and comonomers and the intrinsic viscosity (iV). Thus, the crystallite fraction (CF) represents the crystallite part of the polypropylene composition, such as the matrix phase of a heterophasic propylene copolymer. The soluble fraction (SF) represents the amorphous part of the polypropylene composition, such as the elastomeric phase of a heterophasic propylene copolymer.

[0055] The composition has a soluble fraction (SF) and a crystallizate fraction (CF) as determined by CRYSTEX QC analysis.

[0056] In the CRYSTEX QC analysis, the composition exhibits one or more of the following properties:

[0057] (1) a crystallizate fraction (CF) content determined according to CRYSTEX QC analysis in the range of 70.0 to 85.0 wt %, preferably in the range of 72.5 to 82.5 wt %, more preferably in the range of 75.0 to 80.0 wt %;

[0058] (2) The soluble fraction (SF) content determined by CRYSTEX QC analysis is between 15.0 wt% and 30.0 wt%

[0059] The range is preferably 17.5 wt% to 27.5 wt%, and more preferably 20.0 wt% to 25.0 wt%.

[0060] within the range.

[0061] The crystallizate fraction (CF) preferably has all of the following properties:

[0062] (1) Through quantitative 13 The ethylene content (C2(CF)) determined by FT-IR spectroscopy calibrated with C-NMR spectroscopy is in the range of 1.5 to 3.0 wt%, preferably in the range of 1.8 to 2.8 wt%, more preferably in the range of 2.0 to 2.7 wt%.

[0063] within the scope; and / or

[0064] (2) The intrinsic viscosity (iV(CF)) measured in decalin at 135° C. according to DIN ISO 1628 / 1 is 0.7 to 1.7 dl / g, preferably 0.8 to 1.5 dl / g, more preferably 0.9 to 1.4 dl / g.

[0065] The soluble fraction (SF) preferably has all of the following properties:

[0066] (1) Through quantitative 13 Ethylene content determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy (C2(SF))

[0067] In the range of 25.0 to 40.0 wt%, preferably in the range of 27.5 to 37.5 wt%, more preferably in the range of 27.5 to 36.5 wt%; and / or

[0068] (2) Intrinsic viscosity (iV(CF)) measured in decalin at 135°C according to DIN ISO 1628 / 1: 2.0

[0069] dl / g to 3.5 dl / g, preferably 2.3 to 3.0 dl / g, more preferably 2.5 to 2.9 dl / g.

[0070] The polypropylene composition preferably comprises units derived from ethylene in a total amount of 5.5 to 12.5 wt%, preferably 6.0 to 12.0 wt%, more preferably 6.5 to 11.5 wt%, as determined by quantitative 13 FT-IR spectroscopy calibrated by C-NMR spectroscopy.

[0071] The ratio of the intrinsic viscosities of the soluble fraction and the crystallizate fraction (iV(SF) / iV(CF)) is preferably in the range of 2.2 to 3.0, more preferably in the range of 2.4 to 2.9, still more preferably in the range of 2.6 to 2.8.

[0072] The ratio of the ethylene content of the soluble fraction to the crystallizate fraction (C2(SF) / C2(CF)) is in the range of 11.0 to 15.0, preferably in the range of 11.5 to 15.0, more preferably in the range of 12.0 to 15.0.

[0073] Preferably, the polymer component in the polypropylene composition consists of propylene units and ethylene units only.

[0074] Although not measured, the content of units derived from propylene (C3) in the soluble fraction (SF) and the content of units derived from ethylene (C2) in the soluble fraction (SF) added together are preferably up to 100 wt%.

[0075] The content of units derived from propylene (C3) in the soluble fraction (SF) is preferably in the range of 60.0 to 75.0 wt%, more preferably in the range of 62.5 to 72.5 wt%, still more preferably in the range of 63.5 to 72.5 wt%.

[0076] Although it cannot be measured directly, the content of units derived from propylene (C3) in the crystallizate fraction (CF) and the content of units derived from ethylene (C2) in the crystallizate fraction (CF) added together preferably amounts to at most 100 wt.-%.

[0077] The content of units derived from propylene (C3) in the crystallizate fraction (CF) is preferably in the range of 97.0 to 98.5 wt.-%, more preferably in the range of 97.2 to 98.2 wt.-%, still more preferably in the range of 98.0 to 98.3 wt.-%.

[0078] The total content of units derived from propylene (C3) of the polypropylene composition is preferably from 87.5 to 94.5 wt%, more preferably from 88.0 to 94.0 wt%, still more preferably from 88.5 to 93.5 wt%.

[0079] Especially the properties of the soluble fraction (SF) preferably result in a specific morphology of the elastomeric phase dispersed in the matrix phase of the heterophasic polypropylene copolymer.The elastomeric phase can be identified as particles in the matrix phase, for example under microscopic observation.

[0080] The particles of the elastomeric phase dispersed in the matrix phase preferably have a number average particle size of 1150 to 1325 nm, preferably 1175 to 1300 nm, more preferably 1200 to 1275 nm.

[0081] The melting temperature Tm of the polypropylene composition is preferably between 155 and 175 °C, more preferably between 157 and 172 °C, still more preferably between 160 and 170 °C.

[0082] Furthermore, the crystallization temperature Tc of the polypropylene composition is preferably between 120 and 140 °C, more preferably between 122 and 137 °C, still more preferably between 125 and 135 °C.

[0083] Further, the heat deformation temperature HDTB of the polypropylene composition is preferably between 92 and 110°C, more preferably between 93 and 108°C, still more preferably between 95 and 105°C.

[0084] The polypropylene composition according to the present invention preferably shows an excellent balance of properties in terms of flowability (melt flow rate as stated above), impact properties and especially mechanical properties (like tensile properties).

[0085] The tensile modulus of the polypropylene composition is preferably from 1250 to 1600 MPa, more preferably from 1300 to 1550 MPa, still more preferably from 1300 to 1520 MPa.

[0086] Furthermore, the tensile elongation at break of the polypropylene composition is preferably between 4.0% and 25.0%, more preferably between 4.5% and 20.0%, still more preferably between 4.7% and 17.5%.

[0087] Furthermore, the Charpy notched impact strength of the polypropylene composition at 23°C (CNIS at 23°C) is preferably in the range of 2.5 to 6.4 kJ / m 2 between 2.7 and 6.0 kJ / m 2 between.

[0088] Furthermore, the Charpy notched impact strength of the polypropylene composition at -20°C (CNIS at -20°C) is preferably in the range of 2.0 to 5.5 kJ / m 2 More preferably, between 2.3 and 5.0 kJ / m 2 between.

[0089] Still more preferably, the composition has good impact strength in an instrumented puncture test:

[0090] (1) The composition has a puncture energy measured at 23°C of 4.5 to 20.0 J, preferably 5.0 to 15.0 J.

[0091] (2) The puncture energy of the composition measured at -20°C is 3.5 to 15.0 J, preferably 4.0 to 12.0 J.

[0092] The polypropylene composition comprises the heterophasic propylene copolymer (A) in an amount of at least 95.0 wt%, such as 95.0 to 99.9 wt%, preferably 96.0 to 99.5 wt%, more preferably 97.5 to 99.0 wt%, based on the total weight of the polypropylene composition.

[0093] The heterophasic polypropylene copolymer (A) preferably has all of the following properties:

[0094] (1) Melt flow rate (MFR) 2 (230°C, 2.16 kg, ISO 1133) is 75 to 250 g / 10 min, preferably 80 to 200 g / 10 min, more preferably 85 to 180 g / 10 min; and / or

[0095] (2) Through quantitative 13 The total content of units derived from ethylene (C2), determined by FT-IR spectroscopy calibrated with C-NMR spectroscopy, is from 5.5 to 12.5 wt%, preferably from 6.0 to 12.0 wt%, more preferably from 6.5 to 11.5 wt%; and / or

[0096] (3) a melting temperature Tm of 155 to 175°C, preferably 157 to 172°C, more preferably 160 to 170°C, as determined by differential scanning calorimetry (DSC) according to ISO 11357 / Part 3 / Method C2; and / or

[0097] (4) a crystallization temperature Tc of 120 to 140°C, preferably 122 to 137°C, more preferably 125 to 135°C, as determined by differential scanning calorimetry (DSC) according to ISO 11357 / Part 3 / Method C2; and / or

[0098] (5) Xylene cold soluble fraction (XCS) measured at 25°C according to ISO 16152, first edition, 2005-07-01

[0099] A content, based on the total weight of the heterophasic propylene copolymer (A), of 12.5 to 30.0 wt%, preferably of 15.0 to 27.5 wt%, more preferably of 17.5 to 25.0 wt%; and / or

[0100] (6) The ethylene content of the XCS fraction (C2(XCS)) is 22.5 to 50.0 wt%, preferably 25.0 to 47.5 wt%, more preferably 27.5 to 45.0 wt%, using quantitative13 C-NMR spectroscopy calibrated FT-

[0101] IR spectroscopy; and / or

[0102] (7) The intrinsic viscosity iV(XCS) of the XCS fraction, measured in decalin at 135° C. according to DIN ISO 1628 / 1, is from 3.0 to 4.5 dl / g, preferably from 3.1 to 4.2 dl / g, more preferably from 3.2 to 4.0 dl / g.

[0103] Further, the polypropylene composition further comprises a particulate inorganic nucleating agent (B) in an amount up to 1.5 wt%, such as 0.01 to 1.5 wt%, preferably 0.1 to 1.3 wt%, more preferably 0.2 to 1.2 wt%, based on the total weight of the polypropylene composition.

[0104] The particulate inorganic nucleating agent (B) is preferably talc.

[0105] The median particle size d of the granular inorganic nucleating agent (B) before mixing 50 It is 0.5 to 7.5 μm, preferably 1.0 to 5.0 μm.

[0106] Furthermore, the top-cut particle size d of the particulate inorganic nucleating agent (B) before mixing is 95 It is 2.0 to 20.0 μm, preferably 3.0 to 15.0 μm.

[0107] The composition further comprises additives, and the additive content is up to 3.0 wt%, preferably in the range of 0.1 to 3.0 wt%, and more preferably in the range of 0.5 to 2.5 wt%, based on the total weight of the composition.

[0108] Typically, the additives may be selected from antioxidants, anti-slip agents, nucleating agents (other than the particulate inorganic nucleating agent (B)), scratch inhibitors, scorch inhibitors, metal deactivators, UV stabilizers, acid scavengers, lubricants, antistatic agents, pigments, etc., and combinations thereof. These additives are well known in the polymer industry and the skilled artisan will be familiar with their use. Any additive present may be added as a separate raw material or may be added as a mixture with a carrier polymer, i.e. in a so-called masterbatch.

[0109] The polypropylene composition may comprise further components than the heterophasic polypropylene copolymer (A), the particulate inorganic nucleating agent (B) and optional additives, such as minor amounts of other polymer components, such as up to 3.0 wt%.

[0110] However, it is preferred that the polypropylene composition consists of the heterophasic propylene copolymer (A), the particulate inorganic nucleating agent (B) and optional additives.

[0111] Technology

[0112] In another aspect, the present invention relates to a process for the preparation of a polypropylene composition as defined above or below, wherein the heterophasic polypropylene copolymer (A) is polymerized in the presence of a Ziegler-Natta catalyst system in a multistage process of at least two polymerization reactors connected in series and the heterophasic polypropylene copolymer (A) is blended with a particulate inorganic nucleating agent.

[0113] In a multistage process, a propylene homopolymer is prepared in at least one first polymerization step and a propylene ethylene copolymer is prepared in the presence of the propylene homopolymer or produced by blending the propylene homopolymer with the propylene ethylene copolymer after polymerization of the propylene homopolymer and the propylene ethylene copolymer in at least one subsequent polymerization step.

[0114] In a particularly preferred embodiment the propylene homopolymer matrix is ​​produced in at least a slurry phase reactor and subsequently the propylene ethylene copolymer is produced in at least a gas phase reactor.

[0115] Thus, the heterophasic propylene copolymer can usually be produced in a reactor cascade of at least 2 reactors, preferably at least 3 reactors, more preferably at least 4 reactors, wherein the first reactor is preferably a liquid bulk reactor of loop design and all subsequent reactors are gas phase reactors, preferably of fluidized bed design. The number of subsequent reactors is generally not more than 6, preferably not more than 5. Preferably, the heterophasic propylene copolymer is produced in a cascade of 4 reactors.

[0116] The preferred multi-stage process is provided by Borealis (called The "loop-gas phase" process is a process developed by the German Patent Office (Kunstofftechnik) and is described in the patent literature, for example, in EP 0 887 379, WO 92 / 12182, WO 2004 / 000899, WO 2004 / 111095, WO 99 / 24478, WO 99 / 24479 or WO 00 / 68315.

[0117] Another suitable slurry-gas phase process is Basell's Craftsmanship.

[0118] Preferably, the components produced in the first two reactors are crystallizable propylene homopolymers, while the components produced in the subsequent third and fourth reactors are amorphous propylene ethylene copolymers having a higher ethylene comonomer content.

[0119] In case the propylene homopolymer and / or propylene ethylene copolymer is polymerized in multiple polymerization reactors, for example in two subsequent polymerization reactors, preferably the polymerization conditions should be adjusted in order to produce comparable propylene homopolymer fractions and / or propylene ethylene copolymer fractions.

[0120] Preferably the propylene homopolymer is unimodal.

[0121] Further preferably, the propylene ethylene copolymer is unimodal.

[0122] In a preferred embodiment, the process comprises the following steps:

[0123] a) polymerizing propylene in a first polymerization reactor in the presence of a Ziegler-Natta catalyst system to obtain a first propylene homopolymer fraction;

[0124] b) transferring the polymerization mixture containing the Ziegler-Natta catalyst system and the first propylene homopolymer fraction from the first polymerization reactor to the second polymerization reactor;

[0125] c) polymerizing propylene in the presence of a Ziegler-Natta catalyst system in a second polymerization reactor to produce a second propylene homopolymer fraction;

[0126] d) transferring the polymerization mixture containing the Ziegler-Natta catalyst system, the first propylene homopolymer fraction and the second propylene homopolymer fraction from the second polymerization reactor to a third polymerization reactor;

[0127] e) polymerizing propylene and ethylene in the presence of a Ziegler-Natta catalyst system in a third polymerization reactor to produce a first propylene-ethylene copolymer fraction;

[0128] f) transferring the polymerization mixture comprising the Ziegler-Natta catalyst system, the first propylene homopolymer fraction and the second propylene homopolymer fraction and the first propylene-ethylene copolymer fraction from the third polymerization reactor to a fourth polymerization reactor;

[0129] g) polymerizing propylene and ethylene in the presence of a Ziegler-Natta catalyst system in a fourth polymerization reactor to produce a second propylene-ethylene copolymer fraction;

[0130] h) withdrawing a polymerization mixture comprising the Ziegler-Natta catalyst system, the first propylene homopolymer fraction and the second propylene homopolymer fraction and the first propylene-ethylene copolymer fraction and the second propylene-ethylene copolymer fraction from the fourth polymerization reactor;

[0131] i) obtaining a heterophasic propylene copolymer (A) comprising a first propylene homopolymer fraction and a second propylene homopolymer fraction and a first propylene-ethylene copolymer fraction and a second propylene-ethylene copolymer fraction;

[0132] j) blending the heterophasic polypropylene copolymer (A) with a particulate inorganic nucleating agent (B).

[0133] Preferably the first polymerisation reactor is a slurry phase reactor, such as a loop reactor.

[0134] Preferably the operating temperature in the first polymerisation reactor, preferably a loop reactor, is between 62 and 85 °C, more preferably in the range of 65 to 82 °C, still more preferably in the range of 67 to 80 °C.

[0135] Typically, the pressure in the first polymerisation reactor, preferably in a loop reactor, is between 20 and 80 bar, preferably between 30 and 70 bar, for example between 35 and 65 bar.

[0136] Preferably a propylene homopolymer is produced in the first polymerization reactor, preferably a loop reactor. Accordingly, the first propylene polymer fraction is preferably a first propylene homopolymer fraction.

[0137] Preferably, hydrogen is added to the first polymerization reactor to control the molecular weight, i.e. the melt flow rate MFR 2 .

[0138] Preferably, in the first polymerization reactor, preferably a loop reactor, the ratio of hydrogen to propylene (H2 / C3) is controlled in the range of 20 to 50 mol / kmol, more preferably in the range of 30 to 40 mol / kmol.

[0139] Due to the high hydrogen content the melt flow rate of the first propylene polymer fraction is very high.

[0140] Preferably, the melt flow rate MFR of the first propylene polymer fraction is 2 (230° C., 2.16 kg, ISO 1133) is in the range of 50 to 1000 g / 10 min, preferably in the range of 150 to 850 g / 10 min, more preferably in the range of 300 to 700 g / 10 min.

[0141] The second polymerization reactor is preferably a first gas phase reactor, such as a first fluidized bed gas phase reactor.

[0142] Preferably, the operating temperature of the second polymerisation reactor, preferably the first gas phase reactor, is in the range of 75 to 95 °C, more preferably in the range of 78 to 92 °C.

[0143] Typically, the pressure of the second polymerization reactor, preferably the first gas phase reactor, is in the range of 5 to 50 bar, preferably in the range of 15 to 40.

[0144] In the second polymerization reactor, preferably the first gas phase reactor, a propylene homopolymer is produced. Hence, the second propylene polymer fraction is preferably a second propylene homopolymer fraction.

[0145] It is preferred to add hydrogen to the second polymerization reactor to control the molecular weight, i.e. the melt flow rate MFR 2 .

[0146] It is preferred that the ratio of hydrogen to propylene (H2 / C3) in the second polypropylene reactor (preferably the first gas phase reactor) is in the range of 150 to 500 mol / kmol, more preferably in the range of 200 to 350 mol / kmol.

[0147] Due to the high hydrogen content the melt flow rate of the first propylene polymer fraction and the second propylene polymer fraction is very high.

[0148] Preferably, the melt flow rate MFR of the combined first propylene polymer fraction and the second propylene polymer fraction is 2 (230° C., 2.16 kg, ISO 1133) is in the range of 50 to 1000 g / 10 min, preferably in the range of 150 to 850 g / 10 min, more preferably in the range of 300 to 700 g / 10 min.

[0149] The third polymerization reactor is preferably a second gas phase reactor, such as a second fluidized bed gas phase reactor.

[0150] Preferably, the operating temperature of the third polymerization reactor, preferably the second gas phase reactor, is in the range of 65 to 85° C., more preferably in the range of 68 to 82° C. Typically, the operating temperature of the third polymerization reactor is lower than the operating temperature of the second polymerization reactor.

[0151] Typically, the pressure of the third polymerization reactor, preferably the second gas phase reactor, is in the range of 5 to 40 bar, preferably in the range of 10 to 30.

[0152] The propylene ethylene copolymer is produced in the third polymerization reactor, preferably the second gas phase reactor. Thus, the third propylene polymer fraction is the first propylene ethylene homopolymer fraction.

[0153] The ratio of ethylene to propylene (C2 / C3 ratio) in the third polymerization reactor (preferably the second gas phase reactor) is controlled in the range of 200 to 500 mol / kmol, more preferably in the range of 250 to 475 mol / kmol.

[0154] Since the content ratio of ethylene to propylene (C2 / C3 ratio) is high, the third propylene polymer fraction is preferably an elastic block copolymer having a propylene-rich portion and an ethylene-rich portion.

[0155] Preferably, hydrogen is added to the third polymerization reactor to control the molecular weight, i.e., the melt flow rate MFR 2 .

[0156] Preferably, in the third polymerization reactor, the ratio of hydrogen to ethylene (H2 / C2 ratio) is controlled within the range of 20 to 100 mol / kmol, more preferably within the range of 30 to 75 mol / kmol.

[0157] Preferably the melt flow rate MFR of the first, second and third propylene polymer fractions combined is 2 (230° C., 2.16 kg, ISO 1133) is in the range of 30 to 500 g / 10 min, preferably in the range of 65 to 350 g / 10 min, more preferably in the range of 75 to 250 g / 10 min.

[0158] The fourth polymerization reactor is preferably a third gas phase reactor, such as a third fluidized bed gas phase reactor.

[0159] Preferably, the operating temperature in the fourth polymerization reactor (preferably the third gas phase reactor) is in the range of 65 to 85° C., more preferably in the range of 68 to 82° C. Typically, the operating temperature of the fourth polymerization reactor is lower than the operating temperature of the second polymerization reactor.

[0160] Typically, the pressure of the fourth polymerization reactor (preferably the third phase reactor) is in the range of 5 to 40 bar, preferably in the range of 10 to 30.

[0161] In the fourth polymerization reactor, preferably the third gas phase reactor, propylene ethylene copolymer is produced. Thus, the fourth propylene polymer fraction is the second propylene ethylene copolymer fraction.

[0162] The ratio of ethylene to propylene (C2 / C3 ratio) in the fourth polymerization reactor (preferably the third gas phase reactor) is in the range of 150 to 650 mol / kmol, more preferably in the range of 250 to 500 mol / kmol.

[0163] Since the content ratio of ethylene to propylene (C2 / C3 ratio) is high, the fourth propylene polymer fraction is preferably an elastic block copolymer of a propylene-rich portion and an ethylene-rich portion.

[0164] Preferably, hydrogen is added to the fourth polymerization reactor to control the molecular weight, i.e., the melt flow rate MFR 2 .

[0165] Preferably, the ratio of hydrogen to propylene (H2 / C3 ratio) in the fourth polypropylene reactor (preferably the third gas phase reactor) is in the range of 50 to 250 mol / kmol, more preferably in the range of 80 to 175 mol / kmol.

[0166] Preferably the melt flow rate MFR of the first, second, third and fourth propylene polymer fractions combined is2 (230° C., 2.16 kg, ISO 1133) is in the range of 75 to 250 g / 10 min, preferably in the range of 80 to 200 g / 10 min, more preferably in the range of 85 to 180 g / 10 min.

[0167] Furthermore, the total comonomer content, preferably ethylene (C2) content, of the combined first, second, third and fourth propylene polymer fractions is in the range of 5.5 to 12.5 wt%, preferably in the range of 6.0 to 12.0 wt%, more preferably in the range of 6.5 to 11.5 wt%, based on the total weight of the combined first, second, third and fourth propylene polymer fractions, as determined by quantitative 13 FT-IR spectroscopy calibrated by C-NMR spectroscopy.

[0168] The combined first, second, third and fourth propylene polymer fractions preferably form a heterophasic propylene copolymer.

[0169] The preparation of the first, second, third and fourth propylene polymer fraction may comprise, besides the (main) polymerization stage in at least four polymerization reactors, a prepolymerization in a prepolymerization reactor upstream of the first polymerization reactor.

[0170] The polypropylene is produced in a prepolymerization reactor. The prepolymerization is preferably carried out in the presence of a Ziegler-Natta catalyst system. According to this embodiment, the Ziegler-Natta catalyst system is introduced into the prepolymerization step. However, this does not exclude the option of further adding a cocatalyst in a subsequent stage, for example in the first reactor. In one embodiment, if prepolymerization is used, all components of the Ziegler-Natta catalyst system are added only in the prepolymerization reactor.

[0171] The prepolymerization reaction is usually carried out at a temperature of 0 to 60°C, preferably between 15 and 50°C, more preferably between 20 and 45°C.

[0172] The pressure in the prepolymerization reactor is not critical but must be high enough to keep the reaction mixture in the liquid phase. Thus, the pressure may be from 20 to 100 bar, for example from 30 to 70 bar.

[0173] In a preferred embodiment, the prepolymerization is carried out as a bulk slurry polymerization in liquid propylene, ie the liquid phase comprises mainly propylene, optionally containing inert components dissolved therein.

[0174] Other components may also be added during the prepolymerization stage. Thus, hydrogen may be added during the prepolymerization stage to control the molecular weight of the polypropylene, as is well known in the art. In addition, antistatic additives may be used to prevent the particles from adhering to each other or to the walls of the reactor.

[0175] Precise control of prepolymerization reaction conditions and reaction parameters is well known in the art.

[0176] Due to the defined process conditions in the prepolymerization, a mixture of the Ziegler-Natta catalyst system and the polypropylene produced in the prepolymerization reactor is preferably obtained. Preferably, the Ziegler-Natta catalyst system is (finely) dispersed in the polypropylene. In other words, the Ziegler-Natta catalyst system introduced in the prepolymerization reactor is split into smaller fragments, which are evenly distributed in the growing polypropylene. The size of the introduced Ziegler-Natta catalyst system and the obtained fragments are not necessarily relevant for the present invention and are within the scope of expert knowledge.

[0177] As mentioned above, if prepolymerization is used, after prepolymerization, the mixture of Ziegler-Natta catalyst system and polypropylene produced in the prepolymerization reactor is transferred to the first polymerization reactor. Typically, the total amount of polypropylene produced in the first, second and third propylene polymer fractions produced in the prepolymerization reactor is quite low, typically not more than 5.0 wt%, preferably not more than 4.0 wt%, more preferably in the range of 0.5 to 4.0 wt%, for example in the range of 1.0 to 3.0 wt%.

[0178] Without using prepolymerization, propylene and other ingredients (such as Ziegler-Natta catalyst system) are directly introduced into the first polymerization reactor.

[0179] The residence time of the polymerization mixture in the different polymerization stages is adjusted in order to obtain the amounts of the first, second, third and fourth polymer fractions in the combined first, second, third and fourth polymer fractions.

[0180] Preferably, the content of the first propylene polymer fraction is between 35 and 55 wt%, more preferably between 40 and 50 wt%, based on the total weight of the combined first, second, third and fourth propylene polymer fractions. The amount of polypropylene generated in the prepolymerization reactor, if any, is usually added to the amount of the first propylene polymer fraction.

[0181] Preferably, the second propylene polymer fraction is present in an amount of 25 to 45 wt%, more preferably 30 to 40 wt%, based on the total weight of the first, second, third and fourth propylene polymer fractions combined.

[0182] Preferably, the third propylene polymer fraction is present in an amount of 5 to 20 wt%, more preferably 10 to 15 wt%, based on the total weight of the first, second, third and fourth propylene polymer fractions combined.

[0183] Preferably, the fourth propylene polymer fraction is present in an amount of 3 to 15 wt%, preferably 5 to 10 wt%, based on the total weight of the first, second, third and fourth propylene polymer fractions combined.

[0184] According to the present invention the heterophasic propylene copolymer (A) is obtainable by a multistage polymerization process as described above in the presence of a Ziegler-Natta catalyst system.

[0185] As stated above in the specific process for the preparation of the heterophasic propylene copolymer (A) it is preferred to use a specific Ziegler-Natta catalyst.

[0186] Therefore, the Ziegler-Natta catalyst system is described in detail.

[0187] The catalyst used in the present invention is a solid Ziegler-Natta catalyst comprising a compound of an IUPAC Group 4 to 6 transition metal (such as titanium), a compound of a Group 2 metal (such as magnesium), and an internal donor (preferably a non-phthalic acid compound, more preferably a non-phthalic acid ester, and even more preferably a diester of a non-phthalic acid dicarboxylic acid), as described in more detail below. Thus, the catalyst is completely free of unwanted phthalic acid compounds. In addition, the solid catalyst does not contain any external support material, such as silica or MgCl 2 , but self-supporting.

[0188] Ziegler-Natta catalysts (ZN-C) can be further defined according to how they are obtained.

[0189] The Ziegler-Natta catalyst (ZN-C) is preferably obtained by a process comprising the following steps:

[0190] a)

[0191] a 1 ) providing a solution of at least one Group 2 metal alkoxide (Ax) which is the reaction product of a Group 2 metal compound and a monohydric alcohol (A) and which comprises, in addition to hydroxyl moieties, at least one ether moiety, optionally present in an organic liquid reaction medium; or

[0192] a 2 ) a solution of at least one Group 2 metal alkoxide (Ax') which is the reaction product of a Group 2 metal compound and an alcohol mixture of a monohydric alcohol (A) and a monohydric alcohol (B) of formula ROH, optionally in an organic liquid reaction medium; or

[0193] a 3 ) providing a solution of a mixture of a Group 2 alkoxide (Ax) and a Group 2 metal alkoxide (Bx), compound (Bx) being the reaction product of a Group 2 metal compound and a monohydric alcohol (B), optionally in an organic liquid reaction medium; or

[0194] a 4 ) provides a solution of a Group 2 alkoxy compound having the formula M(OR 1 ) m (OR 2 ) m (OR 2 ) m X 2-n-m Or the Group 2 alkoxy compound M(OR 1 ) n’ X 2-n’ and M(OR 1 ) m 'X 2-m’ A mixture of wherein M is a Group 2 metal, X is a halogen, and R 1 and R 2 C 2 to C 16 Different alkyl groups of carbon atoms, with 0≤n<2, 0≤m<2, n+m+(2-nm)=2, provided that n and m are both not equal to 0, 0<n'≤2 and 0<m'≤2; and

[0195] b) adding the solution obtained in step a) to at least one compound of a transition metal of Groups 4 to 6, and

[0196] c) obtaining solid catalyst component particles.

[0197] An internal electron donor, preferably a non-phthalic acid internal donor, is added in any step prior to step c).

[0198] The internal donor or a precursor thereof is preferably added to the solution in step a).

[0199] According to the above procedure, the Ziegler-Natta catalyst can be obtained by precipitation or by emulsion (liquid / liquid two-phase system)-solidification method, depending on the physical conditions, in particular the temperature used in steps b) and c).

[0200] In both methods (precipitation or emulsion-solidification), the catalyst is chemically identical.

[0201] In the precipitation method, the solution of step a) is combined with at least one transition metal compound in step b), and the entire reaction mixture is maintained at at least 50°C, more preferably in the range of 55°C to 110°C, more preferably in the range of 70°C to 100°C, to ensure complete precipitation of the catalyst components in the form of solid particles (step c).

[0202] In the emulsion-solidification process of step b), the solution of step a) is generally added to at least one transition metal compound at a relatively low temperature, for example between -10 and below 50° C., preferably between -5 and 30° C. While the emulsion is stirred, the temperature is generally maintained between -10 and below 40° C., preferably between -5 and 30° C. The droplets of the dispersed phase of the emulsion form the active catalyst composition. Solidification of the droplets (step c) is suitably carried out by heating the emulsion to a temperature of 70 to 150° C., preferably 80 to 110° C.

[0203] The present invention preferably uses a catalyst prepared by an emulsion-solidification method.

[0204] In a preferred embodiment, step a) uses a 2 ) or a 3 ), that is, a solution of (Ax') or a solution of a mixture of (Ax) and (Bx).

[0205] Preferably, the Group 2 metal is magnesium.

[0206] The magnesium alkoxides (Ax), (Ax') and (Bx) can be prepared in situ in the first step (step a) of the catalyst preparation process by reacting a magnesium compound with the above-mentioned alcohol, or the magnesium alkoxides can be separately prepared magnesium alkoxides, or they can even be commercially available as ready-made magnesium alkoxides and directly used in the catalyst preparation process of the present invention.

[0207] Illustrative examples of alcohol (A) are monoethers of diols (ethylene glycol monoether). Preferred alcohols (A) are C 2 to C 4 Ethylene glycol monoethers, wherein the ether portion contains 2 to 18 carbon atoms, preferably 4 to 12 carbon atoms. Preferred examples are 2-(2-ethylhexyloxy)ethanol, 2-butoxyethanol, 2-hexyloxyethanol and 1,3-propylene glycol-monobutyl ether, 3-butoxy-2-propanol, among which 2-(2-ethylhexyloxy)ethanol and 1,3-propylene glycol-monobutyl ether, and 3-butoxy-2-propanol are particularly preferred.

[0208] An exemplary monohydric alcohol (B) has the formula ROH, wherein R is a linear or branched C 6 -C 10 The most preferred monohydric alcohol is 2-ethyl-1-hexanol or octanol.

[0209] Preferably, a mixture of magnesium alkoxides (Ax) and (Bx) or a mixture of alcohols (A) and (B) is used and employed in a molar ratio of Bx:Ax or B:A of 8:1 to 2:1, more preferably 5:1 to 3:1.

[0210] The magnesium alkoxide may be the reaction product of an alcohol as defined above and a magnesium compound selected from dialkylmagnesium, alkylmagnesium alkoxide, magnesium glycolate, alkoxymagnesium halide and alkylmagnesium halide. The alkyl groups may be similar or different C 1 -C 20 Alkyl, preferably C 2 -C 10 Alkyl. When used, typical alkyl-alkoxy magnesium compounds are ethyl butoxy magnesium, butyl pentoxy magnesium, octyl butoxy magnesium and octyl octoxy magnesium. Dialkyl magnesium is preferably used. The most preferred dialkyl magnesium is butyl octyl magnesium or butyl ethyl magnesium.

[0211] It is also possible that the magnesium compound can react with alcohol (A) and alcohol (B) in addition to the reaction with the formula R" (OH) m If a polyol is used, it is preferably an alcohol, wherein R" is a linear, cyclic or branched C2 to C10 hydrocarbon residue and m is an integer from 2 to 6.

[0212] The magnesium alkoxide of step a) can be selected from dialkoxymagnesium, diaryloxymagnesium, alkoxymagnesium halide, aryloxymagnesium halide, alkylmagnesium alkoxide, arylalkoxymagnesium and alkylaryloxymagnesium. In addition, mixtures of dihalide and dialkoxymagnesium can also be used.

[0213] The solvent used to prepare the catalyst can be selected from aromatic and aliphatic straight chain, branched and cyclic hydrocarbons having 5 to 20 carbon atoms, preferably 5 to 12 carbon atoms, or mixtures thereof. Suitable solvents include benzene, toluene, cumene, xylene, pentane, hexane, heptane, octane and nonane. Hexane and pentane are particularly preferred.

[0214] As mentioned above, the magnesium compound is provided as a 10 to 50 wt% solution in the above mentioned solvents. Typical commercially available magnesium compounds, especially dialkyl magnesium solutions, are 20-40 wt% solutions in toluene or heptane.

[0215] The preparation reaction of the magnesium alkoxide compound can be carried out at a temperature of 40° C. to 70° C. The most suitable temperature depends on the magnesium compound and alcohol used.

[0216] The transition metal compound of Groups 4 to 6 is preferably a titanium compound, most preferably a titanium halide such as TiCl 4 .

[0217] The non-phthalic acid internal donor used to prepare the catalyst of the present invention is preferably selected from non-phthalic acid carboxylic acid (dies), 1,3-diethers, and their derivatives and mixtures. Particularly preferred donors are diesters of monounsaturated dicarboxylic acids, in particular esters belonging to the classes of malonates, maleates, succinates, citrates, glutarates, cyclohexene-1,2-dicarboxylates and benzoates, and any derivatives and / or mixtures thereof. Preferred examples are substituted maleates and citraconates, and most preferred are citraconates.

[0218] In the emulsion process, the two-phase liquid-liquid system can be formed by simple stirring and optionally adding (further) solvents and additives, such as turbulence minimizing agents (TMAs) and / or emulsifiers and / or emulsion stabilizers (such as surfactants), which are used in a manner known in the art to promote the formation and / or stabilization of the emulsion. Preferably, the surfactant is an acrylic acid or methacrylic acid polymer. Particularly preferred are unbranched C 12 To C 20 (Meth)acrylates, such as poly(hexadecyl)-methacrylate and poly(octadecyl)-methacrylate and mixtures thereof. If a turbulence minimizing agent (TMA) is used, it is preferably selected from α-olefin polymers of α-olefin monomers having 6 to 20 carbon atoms, such as polyoctene, polynonene, polydecene, polyundecene or polydodecene or mixtures thereof. Most preferably, polydecene.

[0219] The solid particles obtained by precipitation or emulsion-solidification can be washed at least once, preferably at least twice, more preferably at least three times with aromatic and / or aliphatic hydrocarbons, preferably with toluene, heptane or pentane. The catalyst can be further dried, for example by evaporation or flushing with nitrogen, or it can be slurried into an oily liquid without any drying step.

[0220] The final Ziegler-Natta catalyst is preferably in the form of particles, generally having an average particle size ranging from 5 to 200 μm, preferably from 10 to 100 μm. The particles are compact and have low porosity, with a surface area of ​​less than 20 g / m 2 , more preferably less than 10g / m 2 The content of titanium in the catalyst composition is usually 1 to 6 wt%, magnesium is 10 to 20 wt% and the donor is 10 to 40 wt%.

[0221] Detailed preparation methods of the catalyst are disclosed in WO 2012 / 007430, EP2610271, EP261027 and EP2610272, which are incorporated herein by reference.

[0222] Ziegler-Natta catalysts are usually used together with an alkylaluminum cocatalyst and preferably with an external donor.

[0223] In the present polymerization process, an external donor is preferably present as a further component. Suitable external donors include certain silanes, ethers, esters, amines, ketones, heterocyclic compounds and mixtures thereof. Particular preference is given to using silanes. Most preferably, silanes having the following general formula are used:

[0224]

[0225] Where R a , R b and R c represents a hydrocarbon radical, in particular an alkyl or cycloalkyl radical, wherein p and q are numbers from 0 to 3, their sum p+q being equal to or less than 3. a , R b and R c Can be selected independently of each other and can be the same or different. A specific example of such a silane is (tert-butyl) 2 Si(OCH 3 ) 2 ,(cyclohexyl)(methyl)Si(OCH 3 ) 2 ,(phenyl) 2 Si(OCH 3 ) 2 and (cyclopentyl) 2 Si(OCH 3 ) 2 , or has the following general formula:

[0226] Si(OCH 2 CH 3 ) 3 (NR 3 R 4 )

[0227] Where R 3 and R 4 The groups may be the same or different and represent a hydrocarbon group having 1 to 12 carbon atoms.

[0228] R 3 and R 4 is independently selected from a linear aliphatic hydrocarbon group having 1 to 12 carbon atoms, a branched aliphatic hydrocarbon group having 1 to 12 carbon atoms, and a cyclic aliphatic hydrocarbon group having 1 to 12 carbon atoms. 3 and R 4 Independently selected from methyl, ethyl, n-propyl, n-butyl, octyl, decyl, isopropyl, isobutyl, isopentyl, tert-butyl, tert-pentyl, neopentyl, cyclopentyl, cyclohexyl, methylcyclopentyl and cycloheptyl.

[0229] More preferably, R 3and R 4 are the same, and more preferably, R 3 and R 4 All are ethyl groups.

[0230] Preferably the external donor is a dicyclopentyldimethoxysilane donor (D-donor) or a cyclohexylmethyldimethoxysilane donor (C-donor).

[0231] In addition to the Ziegler-Natta catalyst, a cocatalyst must be used, and an optional external donor can be used. The cocatalyst is preferably a compound of the 13th group of the periodic table (IUPAC), such as an organoaluminum, such as an aluminum compound, such as an aluminum alkyl, an aluminum halide or an aluminum alkyl halide compound. Therefore, in a specific embodiment, the cocatalyst is a trialkylaluminum, such as triethylaluminum (TEAL), dialkylaluminum chloride or alkylaluminum dichloride or a mixture thereof. In a specific embodiment, the cocatalyst is triethylaluminum (TEAL).

[0232] Preferably, the ratio of cocatalyst (Co) to external donor (ED) [Co / ED] and / or the ratio of cocatalyst (Co) to transition metal (TM) [Co / TM] should be carefully selected.

[0233] therefore,

[0234] (a) the molar ratio of the cocatalyst (Co) to the external donor (ED) [Co / ED] must be in the range of 10 to 50, preferably in the range of 15 to 40, more preferably in the range of 15 to 35; and optionally

[0235] (b) the molar ratio of the co-catalyst (Co) to the titanium compound (TC) [Co / TC] must be in the range of 50 to 350,

[0236] It is preferably in the range of 75 to 300, and more preferably in the range of 100 to 275.

[0237] The first heterophasic propylene copolymer (A) of the instant invention is preferably produced in the presence of:

[0238] (a) a Ziegler-Natta catalyst comprising a transition metal compound (TC) of Group 4 to 6 of IUPAC, a Group 2 metal compound and an internal donor, wherein the internal donor is a non-phthalic acid compound, preferably a non-phthalic acid ester, more preferably a diester of a non-phthalic acid dicarboxylic acid;

[0239] (b) an optional co-catalyst (Co), and

[0240] (c) Optional external donor (ED).

[0241] Preferably, the internal donor (ID) is selected from optionally substituted malonates, maleates, succinates, glutarates, cyclohexene-1,2-dicarboxylates, benzoates and their derivatives and / or mixtures thereof, the internal donor (ID) is preferably a citrate. Additionally or alternatively, the molar ratio of the cocatalyst (Co) to the external donor (ED) [Co / ED] is from 10 to 50.

[0242] Preferably, in the polymerization process of heterophasic polypropylene copolymer (A), additional nucleating agent is introduced into the composition. Additional nucleating agent is preferably a polymeric nucleating agent, which is preferably prepared by polymerizing vinyl compounds. In the presence of Ziegler-Natta catalyst system and the vinyl compound (preferably vinylcyclohexane (VCH) polymer) obtained, by first polymerizing vinyl compounds (preferably vinyl cycloalkane) and additional nucleating agent is introduced into the heterophasic polypropylene copolymer (A), then using the catalyst system to produce the heterophasic polypropylene copolymer (A). In the polymerization process of heterophasic polypropylene copolymer (A), the above-mentioned polymerizing nucleating agent is introduced into the heterophasic polypropylene copolymer (A), which is called BNT technology.

[0243] For BNT technology, reference is made to international patent applications WO 99 / 24478 and WO 99 / 24479, in particular WO 00 / 68315. According to this technology, a catalyst system, preferably a Ziegler-Natta procatalyst, can be modified by polymerizing a vinyl compound in the presence of a catalyst system comprising a special Ziegler-Natta catalyst, an external donor and a cocatalyst, wherein the vinyl compound has the formula: CH 2 =CH-CHR 1 R 2 .

[0244] Among them, R 1 and R 2 Together with the carbon atoms to which they are attached, they form an optionally substituted saturated or unsaturated or aromatic ring or condensed ring system, wherein the ring or condensed ring portion contains 4 to 20 carbon atoms, preferably a 5-membered to 12-membered saturated or unsaturated or aromatic ring or condensed ring, or independently represent a straight chain or branched C 4 -C 30 Alkanes, C 4 -C 20 Cycloalkanes or C 4 -C 20 Preferably, R 1 and R 2Together with the C atoms to which they are attached, they form a five-membered or six-membered saturated or unsaturated or aromatic ring, or are independently represented by a lower alkyl group consisting of 1 to 4 carbon atoms. Preferably, the vinyl compounds used to prepare the polymeric nucleating agent used in the present invention are especially vinyl cycloalkanes, especially vinyl cyclohexane (VCH), vinyl cyclopentane and vinyl-2-methylcyclohexane, 3-methyl-1-butene, 3-ethyl-1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene or mixtures thereof. VCH is a particularly preferred monomer.

[0245] The polymerized vinyl compound acts as an α-nucleating agent. In the catalyst modification step, the weight ratio of the vinyl compound to the solid catalyst component is preferably at most 5 (5:1), preferably at most 3 (3:1), more preferably from 0.5 (1:2) to 2 (2:1). The most preferred vinyl compound is cyclohexene (VCH).

[0246] When additional nucleating agent is introduced into the heterophasic propylene copolymer (A) during the polymerization, the amount of additional nucleating agent present in the heterophasic propylene copolymer (A) is preferably not more than 500 ppm, more preferably not more than 200 ppm, yet more preferably in the range of 1.0 to 200 ppm, most preferably in the range of 5.0 to 100 ppm, based on the heterophasic propylene copolymer (A) and the additional nucleating agent, preferably based on the total weight of the polypropylene composition.

[0247] The polypropylene composition is prepared by blending the heterophasic polypropylene copolymer (A) and the particulate inorganic nucleating agent (B) with optional additives. Therefore, the blending conditions are preferably within the usual range for blending such polypropylene compositions and can be easily adjusted by a person skilled in the art.

[0248] Products

[0249] In another aspect, the present invention relates to an article, preferably a molded article, more preferably an injection molded article, still more preferably an injection molded automotive article comprising the polypropylene composition described above or below.

[0250] The article preferably comprises the polypropylene composition in an amount between 25 wt% and 100 wt%.

[0251] In one embodiment, the article preferably comprises the polypropylene composition in an amount of 90 to 100 wt%, preferably 95 to 100 wt%.

[0252] In the above embodiment, the article has the same properties as the polypropylene composition described above or below.

[0253] The articles preferably exhibit high post-processing dimensional stability as evidenced by a low initial coefficient of linear thermal expansion (CLTE).

[0254] The article has a linear thermal expansion coefficient (CLTE 23-80°C, MD) in the temperature range of +23 to +80°C in the machine direction at a heating rate of 1°C / min and is lower than 130 μm / m°C, preferably between 115 and 129 μm / m°C.

[0255] Furthermore, the product has a linear thermal expansion coefficient (CLTE 23-80°C, TD) in the transverse direction within a temperature range of +23 to +80°C at a heating rate of 1°C / min and is lower than 140 μm / m°C, preferably between 125 and 139 μm / m°C.

[0256] Furthermore, the product has a linear thermal expansion coefficient (CLTE-30-80°C, MD) in the machine direction within a temperature range of -30 to +80°C at a heating rate of 1°C / min and is lower than 115 μm / m°C, preferably between 100 and 114 μm / m°C.

[0257] Furthermore, the linear thermal expansion coefficient of the product in the transverse direction within the temperature range of -30 to +80°C (CLTE-30-80°C, TD) at a heating rate of 1°C / min is lower than 125 μm / m°C, preferably between 110 and 124 μm / m°C.

[0258] Due to the excellent balance of properties, the product meets the conditions of automotive products. The product has a wide range of uses and can be used in automotive interior and exterior applications.

[0259] use

[0260] In yet another aspect, the present invention relates to the use of the polypropylene composition as described above or below for injection moulded articles, preferably automotive articles.

[0261] Experimental Section

[0262] The following examples include certain aspects and embodiments of the invention described in the claims. However, it should be understood by those skilled in the art that the following description is illustrative only and should not be considered in any way as limiting the present invention.

[0263] Test Method

[0264] a) CRYSTEX

[0265] Determination of the crystals fraction and the soluble fraction and their respective properties (IV and ethylene content)

[0266] The crystallites fraction (CF) and soluble fraction (SF) of the polypropylene (PP) composition, as well as the comonomer content and intrinsic viscosity of the respective fractions, were analyzed using a CRYSTEX instrument from Polymer Char (Valencia, Spain). Detailed information on the technique and the method can be found in the literature (Ljiljana Jeremic, Andreas Albrecht, Martina Sandholzer and Markus Gahleitner (2020) Rapid characterization of high impact ethylene-propylene copolymer compositions by crystallization-extraction separation: comparability with standard separation methods, International Journal of Polymer Analysis and Characterization, 25:8, 581-596).

[0267] The crystals fraction and the amorphous fraction were separated by temperature cycling of dissolution at 160° C., crystallization at 40° C. and redissolution in 1,2,4-trichlorobenzene at 160° C. SF and CF were quantified using an integrated infrared detector (IR4), the ethylene content (C2) was determined, and the intrinsic viscosity (iV) was determined using an online 2-capillary viscometer.

[0268] The IR4 detector is a multi-wavelength detector that measures infrared absorption in two different bands (CH 3 Stretching vibration (center at about 2960cm -1 ) and CH stretching vibration (2700-3000cm -1 ) for the determination of concentration and ethylene content in ethylene-propylene copolymers. The IR4 detector was calibrated with a series of 8 EP copolymers with known ethylene contents ranging from 2 wt% to 69 wt% (by 13 C-NMR measurement), the concentration of each copolymer was between 2 and 13 mg / ml. In order to take into account both the concentration and ethylene content at various polymer concentrations expected during the Crystex analysis, the following calibration formula was used:

[0269] Concentration = a + b * Abs(CH) + c * (Abs(CH)) 2 +d*(Abs(CH 3 ))+e*(Abs(CH 3 )) 2 +f*

[0270] Abs(CH)*Abs(CH 3 )(Formula 1)

[0271]

[0272] The constants a to e in Formula 1 and the constants a to f in Formula 2 are determined by using least squares regression analysis. CH3 / 1000C is converted to ethylene content (wt%) by the following formula:

[0273]

[0274] By means of the XS calibration, the amounts of the soluble fraction (SF) and the crystallisate fraction (CF) are related to the amount of "xylene cold solubles" (XCS) and the "xylene cold insolubles" (XCI) fraction, determined according to ISO 16152, standard gravimetric method. The XS calibration was achieved by testing various EP copolymers with an XS content in the range of 2-31 wt%. The determined XS calibration is linear:

[0275] wt% XS=1,01*wt% SF (Formula 4)

[0276] The intrinsic viscosity (iV) of the parent EP copolymer and its soluble and crystalline fractions were determined using an online 2-capillary viscometer and correlated to the corresponding iV determined in decalin according to the ISO 1628-3 standard method. Various EP PP copolymers with iV = 2-4 dL / g were used for calibration. The determined calibration curve was linear:

[0277]

[0278] The sample to be analyzed was weighed at a concentration of 10 mg / ml to 20 mg / ml. To avoid injection of gels and / or polymers such as PET and PA that may not dissolve in TCB at 160°C, the weighed sample was filled into a stainless steel mesh MW 0.077 / D0.05 mm.

[0279] After 1,2,4-TCB containing 250 mg / l 2,6-tert-butyl-4-methylphenol (BHT) as an antioxidant was automatically injected into the vial, the sample was dissolved at 160°C until completely dissolved, usually for 60 minutes under constant stirring at 400 rpm. To avoid sample degradation, the polymer solution was covered with a nitrogen atmosphere during the dissolution process.

[0280] A specified volume of sample solution is injected into a chromatographic column filled with an inert carrier, where the sample is crystallized and the soluble fraction is separated from the crystalline part. This process is repeated twice. During the first injection, the entire sample is measured at high temperature to determine the iV [dl / g] and C2 [wt%] of the PP component. During the second injection, the soluble fraction (at low temperature) and the crystallized fraction (at high temperature) in the crystallization cycle are measured (wt% SF, wt% C2, iV).

[0281] b) Xylene cold soluble fraction (XCS, wt%)

[0282] According to ISO 16152 standard, first edition, 2005-07-01, the xylene cold soluble fraction (XCS) is determined at 25° C. The remaining insoluble part is the xylene cold insoluble (XCI) fraction.

[0283] c) Intrinsic viscosity

[0284] The intrinsic viscosity is measured in accordance with DIN ISO 1628 / 1, October 1999, at 135°C in decalin.

[0285] d) Charpy notched impact strength

[0286] According to ISO 179-1eA, at +23°C and -20°C, for 80x 10x4mm prepared according to EN ISO 1873-2 3 The measurements were carried out on injection moulded specimens after conditioning the specimens at 23°C for 96 hours.

[0287] e) Tensile properties

[0288] According to ISO 527-2 standard (crosshead speed = 1 mm / min; test speed 50 mm / min, 23 ° C), the tensile modulus, yield tensile elongation and break tensile elongation tests were carried out using injection molded specimens 1B (dog bone shape, thickness 4 mm) prepared according to EN ISO 1873-2. The test was carried out after the specimens were conditioned at 23 ° C for 96 hours.

[0289] f) Instrument puncture test

[0290] According to ISO 6603-2:2000, 60x 60x 3mm at 23℃ and -30℃ 3 Injection molded plaques were subjected to instrumented penetration testing. The tests were conducted after conditioning the samples at 23°C, -20°C and -30°C for 96 hours.

[0291] g) Comonomer content

[0292] Poly(propylene-co-ethylene)--ethylene content--infrared spectroscopy

[0293] Quantitative infrared (IR) spectroscopy was used to quantify the ethylene content of poly(ethylene-co-propylene) copolymers by calibration with a primary method. The calibration was performed using a set of 13In-house non-commercial calibration standards of known ethylene content were used for quantitative determination of C solution state nuclear magnetic resonance (NMR) spectroscopy. The calibration procedure was performed using conventional methods described in the literature. The calibration set consists of 38 calibration standards with ethylene contents ranging from 0.2-75.0 wt% tested or produced on a full scale under various conditions. The calibration set was chosen to reflect the typical variety of copolymers encountered in the final quantitative infrared spectroscopy. Quantitative IR spectra were measured in the solid state using a Bruker Vertex 70 FTIR spectrometer. The spectra were measured on 300 μm thick 25x25 mm square films prepared under compression molding at 180-210 °C and 4-6 MPa. For samples with very high ethylene content (>50 mol%), 100 μm thick films were used. Standard transmission FT-IR spectroscopy was used using 5000-500 cm -1 The spectral range is 6 mm, the spectral resolution is 2 cm -1 , 16 background scans, 16 spectral scans, an interferogram zero filling factor of 64, and a Blackmann-Harris 3-phase telephoto. Quantitative analysis was performed using the data corresponding to (CH 2 ) >2 The structural unit is 730 and 720cm -1 (A Q ) at CH 2 The total area of ​​the shaking deformation was carried out (integration method G, limit values ​​762 and 694 cm -1 The quantitative band was normalized to 4323 cm corresponding to the CH structural unit. -1 The CH band area (A R )(Integration method G, limit value 4650, 4007cm -1 ). Then the secondary calibration curve was used to normalize the absorbance (A Q / A R ) to predict ethylene content in weight percent. The calibration curve has been previously constructed by regressing the normalized absorbance measured on the calibration set and the main comonomer content.

[0294] Poly(propylene-co-ethylene)-ethylene content- 13 C NMR spectroscopy

[0295] against 1 H and 13 C, using a Bruker Advance III 400 NMR spectrometer, recording the solution state at 400.15 MHz and 100.62 MHz, respectively. 13 C{ 1 H}NMR quantitative spectroscopy. 13All spectra were recorded using a 10 mm extended temperature probe at 125°C using nitrogen for all atmospheres. Approximately 200 mg of material was mixed with chromium acetylacetonate (Cr(acac) 3 ) were dissolved in 3 ml of 1,2-tetrachloroethane-d 2 (TCE-d 2 ) to obtain a 65 mM relaxation agent solution in a solvent (Singh, G., Kothari, A., Gupta, V., Polymer Testing 28 5 (2009), 475).

[0296] To ensure the homogeneity of the solution, after preliminary sample preparation in a heating block, the NMR tube was further heated in a rotating oven for at least 1 hour. After the magnet was inserted, the tube was rotated at a speed of 10 Hz. This device was chosen mainly to obtain high resolution and accurate quantitative ethylene content. Standard single pulse excitation without NOE was used, with the best top cone angle, a 1 s cycle delay and a double-stage WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D. Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 1128). A total of 6144 (6k) transients were collected for each spectrum. 13 C{ 1 H} quantitative NMR spectra are processed, integrated and the relevant quantitative properties are determined from the integral. All chemical shifts are indirectly referenced to the central methylene of the ethylene block (EEE) at 30.00 ppm using the chemical shift of the solvent. Even without this structural unit, this method can be similarly referenced. Characteristic signals corresponding to ethylene incorporation are observed (Cheng, HN, Macromolecules 17 (1984), 1950), and the comonomer fraction is calculated as the fraction of ethylene in the polymer relative to all monomers in the polymer:

[0297]

[0298] Through the penetration 13 C{ 1The comonomer fraction was quantified using the method of Wang et al. (Wang, WJ, Zhu, S., Macromolecules 33 (2000), 1157) by integrating multiple signals over the entire spectral region of the {H} spectrum. This method was chosen for its robustness and ability to account for the presence of regional defects when needed. The integration region was fine-tuned to improve applicability over the entire range of comonomer content encountered. For systems where only isolated ethylene was observed in the PPEPP sequence, the method of Wang et al. was modified to reduce the impact of non-zero integrals at sites known to be absent. This approach reduces the overestimation of ethylene content in such systems by reducing the number of sites used to determine the absolute ethylene content:

[0299] E=0.5(S ββ +S βγ +S βδ +0.5(S αβ +S αγ ))

[0300] Using this set of sites, the corresponding integral equation becomes

[0301] E=0.5(I H +I G +0.5(I C +I D ))

[0302] The same symbols as in the article by Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157) are used. The calculation formula for the absolute propylene content is not modified. The molar percentage of the incorporated comonomer is calculated based on the mole fraction:

[0303] E(mol%)=100*f E

[0304] Calculate the weight percent of comonomer incorporated based on the mole fraction:

[0305] E(wt%)=100*(f E *28.06) / ((f E *28.06)+((1-f E )*42.08))

[0306] h)MFR

[0307] Melt flow rate (MFR 2) is measured at 230°C (polypropylene-based materials) or 190°C (polyethylene-based materials) using a load of 2.16 kg. Melt flow rate refers to the amount of polymer (in grams) that the test equipment extrudes in 10 minutes at a temperature of 230°C (or 190°C) under a load of 2.16 kg according to ISO 1133 standard.

[0308] i) Density

[0309] Density was measured according to ISO 1183-187. Sample preparation was done by compression molding according to ISO 1872-2:2007 standard.

[0310] j)DSC analysis, melting temperature (Tm) and crystallization temperature (Tc)

[0311] The measurements were performed on 5 to 7 mg samples using a TA Instrument Q200 Differential Scanning Calorimetry (DSC). The DSC was run in a heating / cooling / heating cycle at a scan rate of 10°C / min in the temperature range of -30 to +225°C according to ISO 11357 / Part 3 / Method C2. The crystallization temperature (T c ) and crystallization enthalpy (H c ) is determined by the cooling step, while the melting temperature (T m ) and melting enthalpy (H m ) is determined by the second heating step.

[0312] k) Heat Deformation Temperature (HDT)

[0313] HDT was prepared in accordance with ISO 1873-2 in 80x10x4 mm 3 Determined on injection molded specimens and stored at +23°C for at least 96 hours before measurement. The test is carried out according to ISO 75, condition B on flat supported specimens with a nominal surface stress of 0.45 MPa.

[0314] l) Coefficient of linear thermal expansion (CLTE)

[0315] The coefficient of linear thermal expansion (CLTE) was determined according to ISO 11359-2:1999 on 20 pieces of 10 mm length cut from the same injection-molded specimens used to determine the tensile modulus. The measurements were carried out in the temperature range of -30 to +80°C and in the temperature range of 23 to +80°C at a heating rate of 1°C / min in the machine direction.

[0316] m) Particle size of the elastomer phase

[0317] Atomic force microscopy (AFM) images were taken at -40°C from a 60x 60x 1mm 3Photographed on a cryosection surface prepared at the center of an injection molded specimen for instrumented penetration testing (IPT) to provide information on the morphology of the dispersed phase. In injection molding, the cut is made perpendicular to the flow direction and with a 60 x 60 mm 2 The plane of the sample was at an angle of 90°. The Asylum AFM instrument was used in dynamic tapping mode to distinguish the crystalline PP matrix phase from the softer elastomeric phase. Based on the AFM phase images, the particle size distribution of the dispersed phase was analyzed to provide the number average particle size D for each sample. mean .

[0318] experiment

[0319] a) Preparation of HECO A1-A6

[0320] Catalyst system:

[0321] In the polymerization process of HECO A-1 to HECO A-6, the Ziegler-Natta type catalyst (ZN1) used in the inventive example of WO 2016 / 066446 A1 was used, which was prepolymerized with vinylcyclohexane to achieve nucleation with poly(vinylcyclohexane).

[0322] Nucleation with vinylcyclohexane prepolymerization is described in detail in EP 2 960 256 B1 and EP 2 960 279 B1. These documents are incorporated herein by reference.

[0323] Polymerization of HECO A1-A6:

[0324] HECO A1-A6 were prepared in a prepolymerization / loop reactor / gas phase reactor 1 / gas phase reactor 2 / gas phase reactor 3 configuration, respectively, followed by a pelletizing step. The above catalyst system was used in combination with triethylaluminum (TEAL) as cocatalyst and dicyclopentadienyl-dimethoxysilane (donor D) as external donor.

[0325] HECO A1-A5 gives a polymer powder having an elastomeric phase (expressed as XCS content) of more than 30 wt% and a melt flow rate of about 15 to 40 g / 10 min. In order to reduce the elastomeric phase (XCS content) to less than 30 wt% and to increase the melt flow rate, the polymer powder of HECO A1-A5 is diluted with a high flow propylene homopolymer similar to the one produced as matrix material in the loop reactor and in the gas phase reactor 1. Table 1 lists the weights of the same polymer powder and the propylene homopolymer blended in the dilution step and the melt flow rate of the propylene homopolymer.

[0326] The diluted resins of HECO A1-A5 and the polymer powder of HECO A6 were compounded in a co-rotating twin-screw extruder Coperion ZSK 47 at 220°C with 0.15 wt% of an antioxidant (Irganox B215FF from BASF, Germany; a 1:2 mixture of pentaerythritol-tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)-propionate, CAS No. 6683-19-8 and tris(2,4-di-tert-butylphenyl)phosphite, CAS No. 31570-04-4) and 0.05 wt% of calcium stearate (CAS No. 1592-23-0, commercially available from Faci, Italy). Table 2 lists the CRYSTEXQC analysis results and other properties of these copolymers.

[0327] Table 1: Preparation of HECO A1-A6

[0328]

[0329]

[0330] nd = not determined; na = not applicable

[0331] b) Preparation of the compositions of Examples IE1, IE2 and CE1-CE4

[0332] The talc B used was TALC HM2, whose d 50 The d95 is 2.4 μm and d95 is 10.0 μm (sedimentogram measurement), and is commercially available from Imifabi S.PA.

[0333] The final composition was compounded in a Coperion ZSK40 twin screw extruder at 220°C, using polymer and talc B as nucleating agent, as well as antioxidant, calcium stearate and antistatic agent. Table 2 lists the composition of each example.

[0334] Table 2 Composition of the embodiment

[0335]

[0336] c) Properties of the compositions of Examples IE1, IE2 and CE1-CE4

[0337] Table 3 shows the properties of the examples.

[0338] Table 3. CRYSTEX QC analysis and other properties of the compositions of Examples IE1, IE2, and CE1-CE4

[0339]

[0340]

[0341] Inventive Examples IE1 and IE2 show that the ethylene content in the soluble fraction (C2(SF)) is 28.4 wt% and 34.1 wt%, respectively, and the ethylene content ratio in the soluble fraction and the crystallized fraction (C2(SF) / C2(CF)) is 12.3 and 13.6, respectively, thus being significantly different from the comparative examples. The inventive examples also show that the number average particle size (D mean (EPC)) are 1236nm and 1256nm respectively.

[0342] Figure 1 The average particle size of the elastomer phase (D 50 (EPC)) and the relationship between the ethylene content in the soluble fraction (C2(SF)).

[0343] Figure 1 The above figure shows the ethylene content in the soluble fraction (C2(SF)) and the average particle size (D 50 The heterophasic polypropylene copolymers of these examples are closely related to each other when polymerized using the same catalyst system and reactor setup. In all examples IE1, IE2 and CE1-CE3, the reactor conditions were adjusted to produce unimodal polypropylene homopolymer in the loop reactor and GPR1, and unimodal propylene ethylene copolymers in GPR2 and GPR3.

[0344] Considering the relationship between the ethylene content in the soluble fraction (C2(SF)) of Example CE4 and the average particle size (D 50 For CE4, bimodal propylene homopolymer is produced in the loop reactor and GPR1, and unimodal propylene ethylene copolymer is produced in GPR2 and GPR3.

[0345] The figure below shows the relationship between the ethylene content in the xylene cold soluble fraction (C2 (XCS)) and the average particle size of the elastomeric phase (D 50 The relationship between the average particle size of the elastomeric phase in a heterophasic polypropylene copolymer (EPC) was first studied by Grein et al., Rheologica Acta 46 (2007) 1083-1089. mean The relationship between the ethylene content in the (EPC) fraction and the ethylene content in the xylene cold soluble fraction (C2 (XCS)).

[0346] Inventive Examples IE1 and IE2 show an improved balance of properties, with higher tensile modulus, higher Charpy notched impact strength (especially at low temperatures), improved puncture energy (especially at low temperatures), and comparable tensile properties, impact properties, CLTE, and shrinkage.

[0347] These improvements are Figure 2 and Figure 3 It is reflected in.

[0348] Figure 2 The relationship between the Charpy notched impact strength and the tensile modulus at -20°C is shown for IE1, IE2, CE1-CE3 and CE4 as reference examples. It can be seen that at a given tensile modulus, the inventive compositions of Examples IE1 and IE2 have improved Charpy notched impact strength at -20°C.

[0349] Figure 3 The relationship between the instrumented puncture test and the tensile modulus at -20°C for IE1, IE2, CE1-CE3 and CE4 as reference examples is shown. It can be seen that at a given tensile modulus, the instrumented puncture test results at -20°C for the inventive compositions of Examples IE1 and IE2 are improved.

Claims

1. A polypropylene composition comprising: (A) at least 95.0 wt%, e.g. 95.0 to 99.9 wt%, preferably 96.0 to 99.5 wt%, more preferably 97.5 to 99.0 wt% of a heterophasic propylene copolymer; (B) up to 1.5 wt%, e.g., 0.01 to 1.5 wt%, preferably 0.1 to 1.3 wt%, more preferably 0.2 to 1.2 wt% of a particulate inorganic nucleating agent; All percentages refer to the total content, and The heterophasic propylene copolymer (A) comprises a matrix phase and an elastomeric phase dispersed therein, and the composition has - Soluble fraction (SF) and crystallite fraction (CF), determined according to the CRYSTEX QC analytical method; - a content of soluble fraction (SF) determined according to CRYSTEX QC analysis ranging from 15.0 wt% to 30.0 wt%, preferably from 17.5 wt% to 27.5 wt%, more preferably from 20.0 wt% to 25.0 wt%; - By quantitative 13 The ethylene content of the soluble fraction C2(SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy, is between 25.0 and 40.0 wt.-%, preferably between 27.5 and 37.5 wt.-%, more preferably between 27.5 and 36.5 wt.-%; - an intrinsic viscosity of the soluble fraction iV(SF) measured in decalin at 135° C. according to DIN ISO 1628 / 1 of 2.0 to 3.5 dl / g, preferably 2.3 to 3.0 dl / g, more preferably 2.5 to 2.9 dl / g; - the ethylene content ratio of the soluble fraction to the crystallizate fraction (C2(SF) / C2(CF)) is from 11.0 to 15.0, preferably from 11.5 to 15.0, more preferably from 12.0 to 15.0; and - melt flow rate MFR2 (230°C, 2.16 kg, ISO 1133) of 75 to 250 g / 10 min, It is preferably 80 to 200 g / 10 min, more preferably 85 to 180 g / 10 min.

2. The polypropylene composition according to claim 1, wherein The particulate inorganic nucleating agent (B) is talc.

3. The polypropylene composition according to claim 1 or 2, wherein The particulate inorganic nucleating agent (B) has: -Median particle size before mixing d 50 0.5 to 7.5 μm, preferably 1.0 to 5.0 μm; and / or - Top cut particle size d before mixing 95 It is 2.0 to 20.0 μm, preferably 3.0 to 15.0 μm.

4. The polypropylene composition according to any one of claims 1 to 3, having the following characteristics: - a crystallizate fraction (CF) content determined according to CRYSTEX QC analysis in the range of 70.0 to 85.0 wt. %, preferably 72.5 to 82.5 wt. %, more preferably 75.0 to 80.0 wt. %; and / or - Through quantitative 13 The ethylene content C2(CF) in the crystallizide fraction, determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy, is from 1.5 to 3.0 wt. %, preferably from 1.8 to 2.8 wt. %, more preferably from 2.0 to 2.7 wt. %; and / or - the intrinsic viscosity iV(CF) of the crystallizate fraction, measured in decalin at 135° C. according to DIN ISO 1628 / 1, is from 0.7 to 1.7 dl / g, preferably from 0.8 to 1.5 dl / g, more preferably from 0.9 to 1.4 dl / g; and / or - the ratio of the intrinsic viscosities of the soluble fraction to the crystallisate fraction (iV(SF) / iV(CF)) is from 2.2 to 3.0, preferably from 2.4 to 2.9, more preferably from 2.6 to 2.8; and / or - Through quantitative 13 The total content of units derived from ethylene (C2), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy, is from 5.5 to 12.5 wt%, preferably from 6.0 to 12.0 wt%, more preferably from 6.5 to 11.5 wt%.

5. The polypropylene composition according to any one of claims 1 to 4, having the following characteristics: - the particles of the elastomeric phase dispersed in the matrix phase have a number average particle size, as determined in the experimental part, of 1150 to 1325 nm, preferably 1175 to 1300 nm, more preferably 1200 to 1275 nm; and / or - a melting temperature Tm determined by differential scanning calorimetry (DSC) according to ISO 11357 / part 3 / method C2 of 155 to 175°C, preferably 157 to 172°C, more preferably 160 to 170°C; and / or - a crystallization temperature Tc determined by differential scanning calorimetry (DSC) according to ISO 11357 / part 3 / method C2 of 120 to 140°C, preferably 122 to 137°C, more preferably 125 to 135°C; and / or - 80×10×4 mm prepared according to ISO 1873-2 3 The heat deformation temperature HDTB measured on the injection molded specimen is 92 to 110°C, preferably 93 to 108°C, and more preferably 95 to 105°C.

6. The polypropylene composition according to any one of claims 1 to 5, having the following characteristics: - a tensile modulus of 1250 MPa to 1600 MPa, preferably 1300 to 1550 MPa, more preferably 1300 to 1520 MPa; and / or - tensile elongation at break of 4.0% to 25.0%, preferably 4.5% to 20.0%, more preferably 4.7% to 17.5%; All determinations were performed according to ISO 527-2 (crosshead speed = 1 mm / min; test speed 50 mm / min at 23° C.) using injection molded test specimens 1B (dog bone shape, thickness 4 mm) prepared as described in EN ISO 1873-2.

7. The polypropylene composition according to any one of claims 1 to 6, having the following characteristics: - Charpy notched impact strength at 23°C (CNIS at 23°C) of 2.5 to 6.4 kJ / m 2 , preferably 2.7 to 6.0 kJ / m 2 ; and / or -Charpy notched impact strength at -20°C (CNIS at -20°C) of 2.0 to 5.5 kJ / m 2 , preferably 2.3 to 5.0 kJ / m 2 ; All measurements were performed according to ISO 179-1eA at +23°C and -20°C using a 80×10×4 mm 3 Injection molding specimens were carried out.

8. The polypropylene composition according to any one of claims 1 to 7, having the following characteristics: - a puncture energy of 4.5 to 20.0 J, preferably 5.0 to 15.0 J, determined at 23°C by an instrumented puncture test according to ISO 6603-2, and / or The puncture energy determined in an instrumented puncture test according to ISO 6603-2 at -20°C is 3.5 to 15.0 J, preferably 4.0 to 12.0 J.

9. A process for preparing the polypropylene composition according to any one of claims 1 to 8, wherein The heterophasic propylene copolymer (A) is polymerized in the presence of a Ziegler-Natta catalyst system in a multistage process comprising at least two polymerization reactors connected in series and the heterophasic propylene copolymer (A) is blended with the particulate inorganic nucleating agent (B).

10. The method according to claim 9, comprising the steps of: a) polymerizing propylene in a first polymerization reactor in the presence of a Ziegler-Natta catalyst system to obtain a first propylene homopolymer fraction; b) transferring the polymerization mixture comprising the Ziegler-Natta catalyst system and the first propylene homopolymer fraction from the first polymerization reactor to the second polymerization reactor; c) polymerizing propylene in the presence of a Ziegler-Natta catalyst system in a second polymerization reactor to produce a second propylene homopolymer fraction; d) transferring the polymerization mixture comprising the Ziegler-Natta catalyst system, the first propylene homopolymer fraction and the second propylene homopolymer fraction from the second polymerization reactor to a third polymerization reactor; e) polymerizing propylene and ethylene in the presence of a Ziegler-Natta catalyst system in a third polymerization reactor to produce a first propylene-ethylene copolymer fraction; f) transferring the polymerization mixture comprising the Ziegler-Natta catalyst system, the first propylene homopolymer fraction and the second propylene homopolymer fraction and the first propylene-ethylene copolymer fraction from the third polymerization reactor to a fourth polymerization reactor; g) polymerizing propylene and ethylene in the presence of a Ziegler-Natta catalyst system in a fourth polymerization reactor to produce a second propylene-ethylene copolymer fraction; h) withdrawing a polymerization mixture comprising the Ziegler-Natta catalyst system, the first propylene homopolymer fraction and the second propylene homopolymer fraction and the first propylene-ethylene copolymer fraction and the second propylene-ethylene copolymer fraction from the fourth polymerization reactor; i) obtaining a heterophasic propylene copolymer (A) comprising a first propylene homopolymer fraction and a second propylene homopolymer fraction and a first propylene-ethylene copolymer fraction and a second propylene-ethylene copolymer fraction.

11. The method according to claim 9 or 10, wherein: The Ziegler-Natta catalyst system is a solid Ziegler-Natta catalyst system comprising a compound of an IUPAC Group 4 to Group 6 transition metal (such as titanium), a compound of a Group 2 metal (such as magnesium), and an internal donor, wherein the internal donor is preferably a non-phthalic acid compound, more preferably a non-phthalic acid ester, and even more preferably a diester of a non-phthalic dicarboxylic acid.

12. The method according to any one of claims 9 to 11, wherein: The melt flow rate MFR2 (230°C, 2.16kg, ISO 1133) is 250-600g / 10min, preferably 300-575g / 10min, more preferably 375-550g / min.

13. An article, preferably a moulded article, more preferably an injection moulded article, still more preferably an injection moulded automotive article, comprising the polypropylene composition according to any one of claims 1 to 12.

14. The article of claim 13, comprising: - a coefficient of linear thermal expansion in the temperature range of +23 to +80°C in the machine direction at a heating rate of 1°C / min (CLTE 23-80°C, MD) of less than 130 μm / m°C, preferably between 115 and 129 μm / m°C; and / or - a coefficient of linear thermal expansion in the temperature range of +23 to +80°C (CLTE 23-80°C, TD) of less than 140 μm / m°C, preferably between 125 and 139 μm / m°C, at a heating rate of 1°C / min in the transverse direction; and / or - a coefficient of linear thermal expansion in the temperature range of -30 to +80°C in the machine direction at a heating rate of 1°C / min (CLTE-30-80°C, MD) of less than 115 μm / m°C, preferably between 100 and 114 μm / m°C; and / or - a coefficient of linear thermal expansion in the temperature range of -30 to +80°C (CLTE-30-80°C, TD) of less than 125 μm / m°C, preferably between 110 and 124 μm / m°C, at a heating rate of 1°C / min in the transverse direction, All measurements were determined according to ISO 113592:1999.

15. Use of the polypropylene composition according to any one of claims 1 to 8 for injection molded articles, preferably automotive articles.

Citation Information

Patent Citations

  • Heterophasic polypropylene with improved puncture respectively impact strength / stiffness balance

    CN107075205A

  • High flow heterophasic propylene copolymer composition having improved impact properties and thermal stability

    EP3945098A1

  • High flow heterophasic polyolefin compositions having improved stiffness / impact balance

    US20190284379A1

  • Heterophasic polypropylene with improved puncture respectively impact strength / stiffness balance

    WO2016066447A1