Multi-component film
Patent Information
- Application Number
- CN202380028971.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-21
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-05
AI Technical Summary
The multi-layer sheet manufacturing process of existing dental orthodontics is complex and costly, and has limited customization characteristics, making it difficult to meet the characteristics requirements of different needs.
Using a multicomponent membrane structure, customizes the physical properties of the polymer, such as flexural modulus and tear characteristics, by changing material selection and film or layer thickness, for the manufacture of thermoforming with improved durability and customizable modulus Products.
It realizes high durability and customization of thermoformed products such as dental orthodontics, meets different application needs, and improves the performance and flexibility of products.
Smart Images

Figure BDA0005051507190000311 
Figure BDA0005051507190000321 
Figure BDA0005051507190000322
Abstract
Description
Technical Field
[0001] The present invention is generally in the field of thermoplastic polymers. In particular, the present invention relates to polymer films for use in making three-dimensional thermoformed articles such as dental braces aligners. Background Art
[0002] Traditionally, metal braces have been used to reposition teeth to improve function or appearance. In recent years, metal braces have been replaced in many cases by plastic braces. Braces are thermoformed appliances that fit over the patient's teeth and are designed to gradually move them to the desired position. The braces must be hard enough to exert an initial force on the teeth, be able to maintain sufficient force over a period of time, and be durable (resistant to cracking).
[0003] Aligners can be manufactured from a single-layer plastic sheet, but multi-layer sheets (composed of two or more different plastic layers) can allow greater freedom to tailor properties to specific needs. However, multi-layer sheet manufacturing processes may be more difficult or cost-intensive than single-layer counterparts, and there may also be limited ability to tailor the properties of the sheet.
[0004] It would be beneficial to provide films or sheets having improved or wider range of tailored properties than current single or multi-layer sheets. Summary of the invention
[0005] It has been found that multi-component (e.g., monolayer) films (comprising two or more different polymers) can allow greater freedom to tailor properties to specific needs. In embodiments, monolayer films can be provided that allow greater freedom to tailor properties to meet specific needs without increasing the complexity of multilayer film extrusion. In other embodiments, multilayer films can be provided that allow greater freedom to tailor properties to specific needs than multilayer films utilizing essentially a single polymer layer.
[0006] It has also been discovered that blending different polymers (in the same film / layer) in a structure having one major (or majority) polymer domain and appropriately selected minority components enables the physical properties of the overall structure (e.g., flexural modulus, tear properties, and stress relaxation) to be tailored for specific applications.
[0007] The invention is set forth in the appended claims. The present invention generally relates to film structures having improved durability and customizable modulus properties that can be used in many applications, including thermoformed articles for the dental braces market. By varying the material selection and thickness of the film or layer, the modulus can be customized to suit the needs of the end user. These structures can be prepared by extrusion, lamination, or other methods known to those skilled in the art.
[0008] In one aspect, a film structure comprising a multi-component composition is provided. In an embodiment, the multi-component composition comprises at least two different polymer components (A) and (B). In an embodiment, the polymer component (A) is present in an amount of 50 to 99 wt%, or greater than 50 to 99 wt%, and the polymer component (B) is present in an amount of 1 to 50 wt%, or 1 to less than 50 wt%. In an embodiment, the film is a single-layer structure. In other embodiments, the film is a multilayer structure comprising one or more layers, wherein the one or more layers comprise a multi-component composition. DETAILED DESCRIPTION
[0009] The term "film" used herein includes films and sheets and is intended to have its generally accepted meaning in the art.
[0010] As used herein, the singular forms "a", "an", "the", "said" include the plural forms unless the context clearly dictates otherwise. The term "comprising" or "including" is intended to be synonymous with the term "comprising", which means that at least the described compound, element, particle, method step, etc. is present in the composition, article or method, but does not exclude the presence of other compounds, materials, method steps, etc., even if other such compounds, materials, particles, method steps, etc. have the same functions as those described, unless explicitly excluded in the claims.
[0011] In one aspect, a film comprising a multi-component composition is provided, the multi-component composition comprising at least two polymer components (A) and (B), wherein the polymer component (A) is present in an amount of greater than 50 to 99 wt %, and the polymer component (B) is present in an amount of 1 to less than 50 wt %. In an embodiment, the polymer component (A) comprises a polyester comprising:
[0012] (a) a dicarboxylic acid component comprising:
[0013] i) 70 to 100 mol % of terephthalic acid residues; and
[0014] ii) 0 to 30 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0015] (b) a diol component comprising:
[0016] i) 10 to 50 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues;
[0017] ii) 0 to 90 mol% of 1,4-cyclohexanedimethanol residues; and
[0018] iii) 0 to 90 mol % of ethylene glycol residues; and having an inherent viscosity of about 0.4 to about 0.9 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.; and
[0019] The polymer component (B) includes a polyester different from the polyester in the polymer component (A).
[0020] In an embodiment, polymer component (B) comprises a polyester comprising: (a) a dicarboxylic acid component comprising 1,4-cyclohexanedicarboxylate residues, and (b) a diol component comprising 1,4-cyclohexanedimethanol residues.
[0021] In an embodiment, polymer component (B) comprises a polyester comprising:
[0022] (a) a dicarboxylic acid component comprising:
[0023] i) 90 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues;
[0024] ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0025] (b) a diol component comprising:
[0026] i) 90 to 100 mol % of 1,4-cyclohexanedimethanol residues, and
[0027] ii) 0 to 10 mol% of modifying diol residues; and
[0028] Having an inherent viscosity of about 0.5 to about 1.2 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
[0029] In another embodiment, polymer component (B) comprises a copolyester comprising:
[0030] A polyester portion and a polyether portion, wherein:
[0031] The polyester portion comprises the residues of an aliphatic diol and an aliphatic dicarboxylic acid or an aliphatic dicarboxylic acid ester, and
[0032] The polyether portion comprises a polyalkylene glycol; and
[0033] The copolyesterethers have an inherent viscosity of about 0.6 to about 1.5 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
[0034] In an embodiment, polymer component (B) comprises a copolyester comprising a dicarboxylic acid component comprising residues of 1,4-cyclohexanedicarboxylate and a diol component comprising residues of 1,4-cyclohexanedimethanol and poly(tetramethylene ether) glycol.
[0035] In one embodiment, polymer component (B) comprises a copolyester comprising:
[0036] (a) a dicarboxylic acid component comprising:
[0037] i) 90 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues;
[0038] ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0039] (b) a diol component comprising:
[0040] i) 95 to 80 mol % of 1,4-cyclohexanedimethanol residues, and
[0041] ii) 5 to 20 mol% of poly(tetramethylene ether) glycol residues; and
[0042] Having an inherent viscosity of about 0.9 to about 1.4 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C. In another embodiment, the inherent viscosity is in the range of about 1.02 to about 1.26.
[0043] In another embodiment, the multi-component composition comprises three polymer components (A), (B) and (C), wherein the polymer components are different. In the embodiment of the three-component composition, the polymer component (A) is present in an amount of greater than 50 to 99 wt%, and the polymer components (B) and (C) are each present in an amount of 1 to less than 50 wt%. In the embodiment of the three-component composition, the polymer component (A) can be a polyester as described above for component (A) in the embodiment of the (at least) two-component composition, and the components (B) and (C) can independently be polyesters or copolyesters as described above for component (B) in the embodiment of the (at least) two-component composition, provided that the components (B) and (C) are different.
[0044] In a three component composition embodiment, polymer component (A) comprises a polyester comprising:
[0045] (a) a dicarboxylic acid component comprising:
[0046] i) 70 to 100 mol % of terephthalic acid residues; and
[0047] ii) 0 to 30 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0048] (b) a diol component comprising:
[0049] i) 10 to 50 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues;
[0050] ii) 0 to 90 mol% of 1,4-cyclohexanedimethanol residues; and
[0051] iii) 0 to 90 mol% of ethylene glycol residues; and
[0052] having an inherent viscosity of about 0.4 to about 0.9 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.; and
[0053] The polymer components (B) and (C) each contain a polyester different from the polyester in the polymer component (A), provided that the components (B) and (C) are different from each other.
[0054] In a three component composition embodiment, polymer component (B) comprises a polyester comprising:
[0055] (a) a dicarboxylic acid component comprising:
[0056] i) 90 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues;
[0057] ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0058] (b) a diol component comprising:
[0059] i) 90 to 100 mol % of 1,4-cyclohexanedimethanol residues, and
[0060] ii) 0 to 10 mol% of modifying diol residues; and
[0061] Having an inherent viscosity of about 0.5 to about 1.2 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
[0062] In a three component composition embodiment, polymer component (C) comprises a copolyester comprising:
[0063] (a) a dicarboxylic acid component comprising:
[0064] i) 90 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues;
[0065] ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0066] (b) a diol component comprising:
[0067] i) 95 to 80 mol % of 1,4-cyclohexanedimethanol residues, and
[0068] ii) 5 to 20 mol% of poly(tetramethylene ether) glycol residues; and
[0069] Having an inherent viscosity of about 0.9 to about 1.4 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C. In another embodiment, the inherent viscosity is in the range of about 1.02 to about 1.26.
[0070] In other embodiments (for any of the embodiments described in this application), polymer component (A) is a polyester comprising:
[0071] (a) a dicarboxylic acid component comprising:
[0072] i) 70 to 100 mol % of terephthalic acid residues; and
[0073] ii) 0 to 30 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0074] (b) a diol component comprising:
[0075] i) 10 to 40 mol % of isosorbide residues;
[0076] ii) 0 to 90 mol% of 1,4-cyclohexanedimethanol residues; and
[0077] iii) 0 to 90 mol% of ethylene glycol residues; and
[0078] Having an inherent viscosity of about 0.4 to about 1.2 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
[0079] In another embodiment (for any embodiment described in this application), polymer component (A) is a polyester comprising:
[0080] (a) a dicarboxylic acid component comprising:
[0081] i) 90 to 100 mol % of terephthalic acid residues;
[0082] ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0083] (b) a diol component comprising:
[0084] i) 10 to 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues;
[0085] ii) 60 to 90 mol% of 1,4-cyclohexanedimethanol residues; and
[0086] Having an inherent viscosity of about 0.5 to about 0.9 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C. In another embodiment, polymer component (A) has an inherent viscosity of about 0.6 to 0.8 dL / g.
[0087] In other embodiments (for any of the embodiments described in this application), polymer component (A) is a polyester comprising:
[0088] (a) a dicarboxylic acid component comprising:
[0089] i) 90 to 100 mol % of terephthalic acid residues;
[0090] ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0091] (b) a diol component comprising:
[0092] i) 10 to 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues;
[0093] ii) 60 to 90 mol% of ethylene glycol residues; and
[0094] Having an inherent viscosity of about 0.4 to about 0.9 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C. In another embodiment, the inherent viscosity of the polymer component (A) is about 0.5 to 0.7 dL / g.
[0095] In other embodiments (for any of the embodiments described in this application), suitable polymer components (B) or (C) are copolyesters comprising:
[0096] (a) a dicarboxylic acid component comprising:
[0097] i) 90 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues;
[0098] ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0099] (b) a diol component comprising:
[0100] i) 15 to 65 mol% of 1,4-cyclohexanedimethanol residues, and
[0101] ii) 85 to 35 mol% of ethylene glycol residues; and
[0102] Having an inherent viscosity of about 0.4 to about 0.8 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C. In this embodiment, the total number of moles of the diol component totals 100 mol%, and may further consist of 0 to 15 mol% of diethylene glycol residues. In an embodiment, the 1,4-cyclohexanedicarboxylic acid residues may contain trans-1,4-cyclohexanedicarboxylic acid isomers in an amount greater than 50 mol%, or greater than 75 mol%, or greater than 90 mol%, based on the total amount of 1,4-cyclohexanedicarboxylic acid residues present in the polyester.
[0103] Examples of materials that can be used for polymer component (A) can include Tritan available from Eastman Chemical Company. TM MP100, TX1000, TX1500, TX2000, TX1800, MX710, MX711, MX810 and MX730 copolyesters. Examples of materials that can be used for polymer component (B) or (C) can include Neostar 19972 copolyester available from Eastman Chemical Company, or Ecdel TM Elastomer 9966 or 9967.
[0104] The term "polyester" as used herein is intended to include "copolyesters" and, unless otherwise expressly stated, is understood to refer to a synthetic polymer prepared by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxy compounds and / or polyfunctional hydroxy compounds. Typically, the difunctional carboxylic acid can be a dicarboxylic acid and the difunctional hydroxy compound can be a dihydric alcohol, such as a diol. As used herein, the term "diol" includes, but is not limited to, diols, glycols and / or polyfunctional hydroxy compounds. As used herein, the term "residue" refers to any organic structure introduced into a polymer from the corresponding monomer by polycondensation and / or esterification. As used herein, the term "repeat unit" refers to an organic structure having a dicarboxylic acid residue and a diol residue bonded by a carbonyloxy group. Thus, for example, a dicarboxylic acid residue can be derived from a dicarboxylic acid monomer or its associated acyl halide, ester, salt, anhydride or a mixture thereof. As used herein, the term "dicarboxylic acid" is intended to include dicarboxylic acids and any derivatives of dicarboxylic acids, including their associated acyl halides, esters, half-esters, salts, half-salts, anhydrides, mixed anhydrides, or mixtures thereof, which can be used in a reaction process with a diol to prepare a polyester. As used herein, the term "terephthalic acid" is intended to include terephthalic acid itself and its residues and any derivatives of terephthalic acid, including their associated acyl halides, esters, half-esters, salts, half-salts, anhydrides, mixed anhydrides, and / or mixtures thereof or residues thereof, which can be used in a reaction process with a diol to prepare a polyester.
[0105] In one embodiment, terephthalic acid can be used as a starting material. In another embodiment, dimethyl terephthalate can be used as a starting material. In another embodiment, a mixture of terephthalic acid and dimethyl terephthalate can be used as a starting material and / or intermediate material.
[0106] The polyester used in the present invention can generally be prepared from dicarboxylic acids and diols, which react in substantially equal proportions and are introduced into the polyester polymer as their respective residues. Therefore, the polyester of the present invention can contain substantially equal molar amounts of acid residues (100 mol%) and diol (and / or polyfunctional hydroxy compound) residues (100 mol%), so that the total mole number of repeating units is equal to 100 mol%. The molar percentages provided herein can be based on the total mole number of acid residues, the total mole number of diol residues, or the total mole number of repeating units. For example, based on the total acid residues, a polyester containing 30 mol% of isophthalic acid means that the polyester contains 30 mol% of isophthalic acid residues in a total of 100 mol% of acid residues. Therefore, there are 30 moles of isophthalic acid residues in every 100 moles of acid residues. In another example, a polyester containing 30 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol based on total diol residues means that the polyester contains 30 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol out of a total of 100 mol% of diol residues. Thus, there are 30 moles of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues for every 100 moles of diol residues.
[0107] For the desired polyester, the molar ratio of cis / trans 2,2,4,4-tetramethyl-1,3-cyclobutanediol may be different from the respective pure form or from the mixture thereof. In certain embodiments, the mole percentage of cis- and / or trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol is greater than 50 mol% cis and less than 50 mol% trans; or greater than 55 mol% cis and less than 45 mol% trans; or 30 to 70 mol% cis and 70 to 30% trans; or 40 to 60 mol% cis and 60 to 40 mol% trans; or 50 to 70 mol% trans and 50 to 30% cis or 50 to 70 mol% cis and 50 to 30% trans; or 60 to 70 mol% cis and 30 to 40 mol% trans; or greater than 70 mol% cis and less than 30 mol% trans; wherein the sum of the mole percentages of cis- and trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol is equal to 100 mol%. The molar ratio of cis / trans 1,4-cyclohexanedimethanol may vary within the range of 50 / 50 to 0 / 100, for example between 40 / 60 and 20 / 80.
[0108] In certain embodiments, for the polymer component (A) polyester, terephthalic acid or its ester, such as dimethyl terephthalate, or a mixture of terephthalic acid and its ester, constitutes most or all of the dicarboxylic acid component used to form the polyester used in the present invention. In certain embodiments, the terephthalic acid residue can constitute a part or all of the dicarboxylic acid component used to form the polyester in a concentration of at least 70 mol%, such as at least 80 mol%, at least 90 mol%, at least 95 mol%, at least 99 mol% or 100 mol%. In certain embodiments, a higher amount of terephthalic acid can be used to prepare a polyester with higher impact strength. In one embodiment, dimethyl terephthalate is a part or all of the dicarboxylic acid component used to prepare the polyester used in the present invention. As used herein, the terms "terephthalic acid" and "dimethyl terephthalate" are used interchangeably unless otherwise explicitly indicated.
[0109] In addition to terephthalic acid, the dicarboxylic acid component of the copolyester that can be used for polymer component (A) can include up to 30mol%, up to 20mol%, up to 10mol%, up to 5mol% or up to 1mol% of one or more modified aromatic dicarboxylic acids. Another embodiment contains 0mol% of modified aromatic dicarboxylic acid. Therefore, if present, it is expected that the amount of one or more modified aromatic dicarboxylic acids can be within the scope of any of these aforementioned endpoint values, including, for example, 0.01 to 30mol%, 0.01 to 20mol%, 0.01 to 10mol%, 0.01 to 5mol% and 0.01 to 1mol%. In one embodiment, the modified aromatic dicarboxylic acids that can be used for the present invention include but are not limited to those with up to 20 carbon atoms, and they can be linear, para-oriented or symmetrical. Examples of modified aromatic dicarboxylic acids that can be used in the present invention include, but are not limited to, isophthalic acid, 4,4'-biphenyl dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, and trans-4,4'-stilbene dicarboxylic acid, and esters thereof. In one embodiment, the modified aromatic dicarboxylic acid is isophthalic acid.
[0110] The carboxylic acid component of the polyester that can be used for polymer component (A) can be further modified with up to 10mol%, for example, up to 5mol% or up to 1mol% of one or more aliphatic dicarboxylic acids containing up to 20 carbon atoms, for example malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid and dodecanedioic acid dicarboxylic acids. Some embodiments can also contain 0.01 or more mol%, for example, 0.1 or more mol%, 1 or more mol%, 5 or more mol%, or 10 or more mol% of one or more modified aliphatic dicarboxylic acids. Another embodiment contains 0mol% of modified aliphatic dicarboxylic acids. Therefore, if present, it is expected that the amount of one or more modified dicarboxylic acids can be within the scope of any of these aforementioned endpoint values, including, for example, 0.01 to 10mol% and 0.1 to 10mol%. The total mol% of the dicarboxylic acid component is 100mol%.
[0111] The ester of terephthalic acid and other modified dicarboxylic acids or their corresponding ester and / or salt can replace dicarboxylic acid and use. Suitable examples of dicarboxylic acid esters include but are not limited to dimethyl ester, diethyl ester, dipropyl ester, diisopropyl ester, dibutyl ester and diphenyl ester. In one embodiment, the ester is selected from at least one of the following: methyl ester, ethyl ester, propyl ester, isopropyl ester and phenyl ester.
[0112] 1,4-cyclohexanedimethanol may be cis, trans or a mixture thereof, for example, in a cis / trans ratio of 60:40 to 40:60. In another embodiment, trans-1,4-cyclohexanedimethanol may be present in an amount of 60 to 80 mol%.
[0113] In an embodiment, the diol component of the polyester of polymer component (A) above may contain up to 35 mol% of one or more modifying diols which are not 2,2,4,4-tetramethyl-1,3-cyclobutanediol or 1,4-cyclohexanedimethanol.
[0114] Modified glycols that can be used for polyesters may refer to glycols other than 2,2,4,4,-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol, and may contain 2-16 carbon atoms. Examples of suitable modified glycols include, but are not limited to, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, p-xylene glycol, isosorbide, or mixtures thereof. In one embodiment, the modified glycol is ethylene glycol. In another embodiment, the modified glycol is 1,3-propylene glycol and / or 1,4-butanediol. In another embodiment, ethylene glycol is excluded as a modified glycol. In another embodiment, 1,3-propylene glycol and 1,4-butanediol are excluded as modified glycols. In another embodiment, 2,2-dimethyl-1,3-propanediol is excluded as a modified glycol.
[0115] In embodiments, the polyesters described herein (in embodiments of polymer component (A)) may also include 0 to 10 mol%, e.g., 0.01 to 5 mol%, 0.01 to 1 mol%, 0.05 to 5 mol%, 0.05 to 1 mol%, or 0.1 to 0.7 mol% of one or more residues of a branching monomer or branching agent having 3 or more carboxyl substituents, hydroxyl substituents, or a combination thereof (also referred to herein as a branching agent), based on the total mole percent of diol or diacid residues. In embodiments, the polyesters described herein (in embodiments of polymer components (B) and / or (C)) may also include a branching agent in an amount of 0 to 10 mol%, e.g., 0.01 to 5 mol%, 0.01 to 1 mol%, 0.05 to 5 mol%, 0.05 to 1 mol%, or 0.1 to 0.7 mol%, based on the total mole percent of diol or diacid residues.
[0116] In certain embodiments, branching monomers or agents may be added before and / or during and / or after polymerization of the polyester.Thus, the polyesters useful in the present invention may be linear or branched.
[0117] Examples of branching monomers or branching agents include, but are not limited to, polyfunctional acids or polyfunctional alcohols, such as trimellitic acid, trimellitic anhydride, pyromellitic dianhydride, trimethylolpropane, glycerol, pentaerythritol, citric acid, tartaric acid, 3-hydroxyglutaric acid, and the like. In one embodiment, the branching monomer residues may contain 0.1 to 0.7 mol% of one or more residues selected from the following: trimellitic anhydride, pyromellitic dianhydride, glycerol, sorbitol, 1,2,6-hexanetriol, pentaerythritol, trimethylolethane and / or trimesic acid. The branching monomer or branching agent may be added to the polyester reaction mixture in the form of a concentrate or blended with the polyester, such as described in U.S. Pat. Nos. 5,654,347 and 5,696,176, the disclosure of which regarding branching monomers is incorporated herein by reference.
[0118] In certain embodiments, the Tg of the polyester containing TMCD that can be used for polymer component (A) can be about 70 to 150°C, or 90 to 130°C, or 100 to 120°C. In certain embodiments, the Tg of the polyester containing 1,4-cyclohexane dicarboxylate that can be used for polymer component (B) can be about 30 to 110°C, or 50 to 90°C, or 60 to 80°C. In certain embodiments, the Tg of the polyester containing a polyether moiety that can be used for polymer component (B) or (C) can be about -80-50°C, or -60-20°C, or -50-20°C. The glass transition temperature (Tg) of the polyester can be measured using a TADSC 2920 purchased from Thermal Analyst Instrument at a scanning rate of 20°C / min.
[0119] In addition, the multi-component composition useful in the present invention may also contain 0.01 to 25 wt % or 0.01 to 20 wt % or 0.01 to 15 wt % or 0.01 to 10 wt % or 0.01 to 5 wt % of common additives, such as colorants, dyes, slip agents or release agents and / or stabilizers, including but not limited to heat stabilizers or hydrolysis stabilizers, based on the total weight of the polyester composition.
[0120] In certain embodiments where the polymer component (A) comprises a copolyester containing TMCD and CHDM residues, the diol component for the polyester may include, but is not limited to, at least one of the following range combinations: 10 to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 to 90 mol% of 1,4-cyclohexanedimethanol; 10 to 35 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 65 to 90 mol% of 1,4-cyclohexanedimethanol; 10 to less than 35 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 65 to 90 mol% of 1,4-cyclohexanedimethanol; 10 to 30 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 65 to 90 mol% of 1,4-cyclohexanedimethanol. Tetramethyl-1,3-cyclobutanediol and 70 to 90 mol % of 1,4-cyclohexanedimethanol; 10 to 25 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 75 to 90 mol % of 1,4-cyclohexanedimethanol; 11 to 25 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 to 89 mol % of 1,4-cyclohexanedimethanol; 12 to 25 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 to 88 mol % of 1,4-cyclohexanedimethanol; and 13 to 25 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 to 87 mol % of 1,4-cyclohexanedimethanol.
[0121] In other embodiments, the diol component for the polyester may include, but is not limited to, at least one of the following range combinations: 15 to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 to 85 mol% of 1,4-cyclohexanedimethanol; 15 to 35 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 65 to 85 mol% of 1,4-cyclohexanedimethanol; 15 to 30 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 70 to 85 mol% of 1,4-cyclohexanedimethanol. % of 1,4-cyclohexanedimethanol; 15 to 25 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 to 85 mol % of 1,4-cyclohexanedimethanol; 15 to 20 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 to 80 mol % of 1,4-cyclohexanedimethanol; and 17 to 23 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 77 to 83 mol % of 1,4-cyclohexanedimethanol.
[0122] In other embodiments in which the polymer component (A) includes a copolyester containing TMCD and CHDM residues, the diol component for the polyester may include, but is not limited to, at least one of the following range combinations: 20 to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 to 80 mol% of 1,4-cyclohexanedimethanol; 20 to 35 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 65 to 80 mol% of 1,4-cyclohexanedimethanol; 20 to 30 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 70 to 80 mol% of 1,4-cyclohexanedimethanol; and 20 to 25 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 to 80 mol% of 1,4-cyclohexanedimethanol.
[0123] In other embodiments where the polymer component (A) comprises a copolyester containing TMCD and CHDM residues, the diol component for the polyester may include, but is not limited to, at least one of the following range combinations: 25 to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 to 75 mol% of 1,4-cyclohexanedimethanol; 25 to 35 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 65 to 75 mol% of 1,4- cyclohexanedimethanol; and 25 to 30 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 70 to 75 mol % of 1,4-cyclohexanedimethanol; 30 to 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 to 70 mol % of 1,4-cyclohexanedimethanol; 30 to 35 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 65 to 70 mol % of 1,4-cyclohexanedimethanol.
[0124] In certain embodiments, when polymer component (A) comprises a copolyester comprising TMCD and CHDM residues, the copolyester may contain less than 15 mol% ethylene glycol residues, such as 0.01 to less than 15 mol% ethylene glycol residues. In embodiments, the polyesters useful in the present invention contain less than 10 mol%, or less than 5 mol%, or less than 4 mol%, or less than 2 mol%, or less than 1 mol% ethylene glycol residues, such as 0.01 to less than 10 mol%, or 0.01 to less than 5 mol%, or 0.01 to less than 4 mol%, or 0.01 to less than 2 mol%, or 0.01 to less than 1 mol% ethylene glycol residues. In one embodiment, the copolyesters useful in the present invention contain no ethylene glycol residues.
[0125] In certain embodiments where polymer component (A) comprises a copolyester containing isosorbide and CHDM residues, the diol component for the polyester may include, but is not limited to, at least one of the following range combinations: 10 to 40 mol% of isosorbide, 20 to 80 mol% of 1,4-cyclohexanedimethanol, and 10 to 40 mol% of EG; 10 to 35 mol% of isosorbide, 25 to 80 mol% of 1,4-cyclohexanedimethanol, and 10 to 40 mol% of EG; 10 to less than 35 mol% of isosorbide, greater than 25 to 80 mol% of 1,4-cyclohexanedimethanol, and 10 to 40 mol% of EG; 10 to 30 mol% of isosorbide; 1,4-cyclohexanedimethanol and 10 to 40 mol % EG; 10 to 25 mol % of isosorbide, 35 to 80 mol % of 1,4-cyclohexanedimethanol and 10 to 40 mol % EG; 11 to 25 mol % of isosorbide, 35 to 79 mol % of 1,4-cyclohexanedimethanol and 10 to 40 mol % EG; 12 to 25 mol % of isosorbide, 35 to 78 mol % of 1,4-cyclohexanedimethanol and 10 to 40 mol % EG; and 13 to 25 mol % of isosorbide, 35 to 77 mol % of 1,4-cyclohexanedimethanol and 10 to 40 mol % EG.
[0126] In other embodiments, the diol component for the polyester may include, but is not limited to, at least one of the following range combinations: 15 to 40 mol% isosorbide, 20 to 75 mol% 1,4-cyclohexanedimethanol, and 10 to 40 mol% EG; 15 to 35 mol% isosorbide, 25 to 75 mol% 1,4-cyclohexanedimethanol, and 10 to 40 mol% EG; 15 to 30 mol% isosorbide, 30 to 75 mol% 1,4-cyclohexanedimethanol, and 10 to 40 mol% EG; 15 to 25 mol% isosorbide, 35 to 75 mol% 1,4-cyclohexanedimethanol, and 10 to 40 mol% EG; Cyclohexanedimethanol and 10 to 40 mol% EG; 15 to 20 mol% isosorbide, 40 to 75 mol% 1,4-cyclohexanedimethanol and 10 to 40 mol% EG; 17 to 23 mol% isosorbide, 37 to 73 mol% 1,4-cyclohexanedimethanol and 10 to 40 mol% EG; 15 to 30 mol% isosorbide, 40 to 75 mol% 1,4-cyclohexanedimethanol and 10 to 30 mol% EG; 20 to 30 mol% isosorbide, 40 to 65 mol% 1,4-cyclohexanedimethanol and 15 to 30 mol% EG.
[0127] In other embodiments, the diol component for the polyester may include, but is not limited to, at least one of the following range combinations: 10 to 30 mol% of isosorbide, 40 to 75 mol% of 1,4-cyclohexanedimethanol, and 30 to 45 mol% of EG; 20 to 30 mol% of isosorbide, 40 to 65 mol% of 1,4-cyclohexanedimethanol, and 20 to 30 mol% of EG; 20 to 35 mol% of isosorbide, 40 to 55 mol% of 1,4-cyclohexanedimethanol, and 20 to 30 mol% of EG.
[0128] In embodiments where polymer component (A) comprises a copolyester comprising TMCD and EG residues, the polyester may comprise a copolyester comprising: (a) diacid residues comprising from about 90 to 100 mol % TPA residues and from 0 to about 10 mol % IPA residues; and (b) diol residues comprising at least 60 mol % EG residues and up to 40 mol % TMCD residues, wherein the copolyester comprises a total of 100 mol % of the diacid residues and a total of 100 mol % of the diol residues.
[0129] In an embodiment, the copolyester comprises diol residues comprising 10 to 40 mol% TMCD residues and 60 to 90 mol% EG residues. In an embodiment, the copolyester comprises diol residues comprising 20 to 37 mol% TMCD residues and 63 to 80 mol% EG residues. In one embodiment, the copolyester comprises diol residues comprising 22 to 35 mol% TMCD residues and 65 to 78 mol% EG residues.
[0130] In certain embodiments where the polymer component (A) comprises a copolyester comprising TMCD and EG residues, the copolyester comprises: a) a dicarboxylic acid component comprising: (i) 90-100 mol % terephthalic acid residues; and (ii) from about 0 to about 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: (i) from about 10 to about 27 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues; and (ii) from about 90 to about 73 mol% of ethylene glycol residues; and wherein the total mol% of the dicarboxylic acid components is 100 mol%, and wherein the total mol% of the diol components is 100 mol%; and wherein the inherent viscosity (IV) of the polyester is from about 0.50 to 0.8 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.25 g / 50 ml at 25°C; and the L* color value of the polyester is 90 or more as measured by the L*a*b* color system of ASTM D 6290-98 and ASTM E308-99 measured on polymer particles crushed to a 1 mm sieve. In an embodiment, the L* color value of the polyester is greater than 90 as measured by the L*a*b* color system of ASTM D 6290-98 and ASTM E308-99 measured on polymer particles crushed to a 1 mm sieve.
[0131] In certain embodiments, the diol component of the copolyester comprises: (i) from about 15 to about 25 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues; and (ii) from about 85 to about 75 mol % of ethylene glycol residues; or (i) from about 20 to about 25 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues; and (ii) from about 80 to about 75 mol % of ethylene glycol residues; or (i) from about 21 to about 24 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues; and (ii) from about 86 to about 79 mol % of ethylene glycol residues.
[0132] In embodiments where polymer component (A) comprises a copolyester comprising TMCD and EG residues, the copolyester has at least one property selected from the group consisting of a Tg of about 90°C to about 110°C as measured by a TA 2100 thermal analyzer at a scan rate of 20°C / min, a flexural modulus greater than about 2000 MPa (290,000 psi) at 23°C as defined by ASTM D790, and an Izod notched impact strength greater than about 25 J / m (0.47 ft-lb / in) at 23°C using a 1 / 8 inch thick bar according to ASTM D256. In one embodiment, the copolyester has a color value of 90 or greater, or greater than 90, as determined by subjecting polymer particles crushed to a 1 mm screen to the L*a*b* color system of ASTM D6290-98 and ASTM E308-99.
[0133] In one embodiment where the polymer component (A) comprises a copolyester comprising TMCD and EG residues, the copolyester further comprises: (II) a catalyst / stabilizer component comprising: (i) titanium atoms in the range of 10-50 ppm based on the weight of the polymer, (ii) optionally, manganese atoms in the range of 10-100 ppm based on the weight of the polymer, and (iii) phosphorus atoms in the range of 10-200 ppm based on the weight of the polymer. In one embodiment, the 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues are a mixture comprising greater than 50 mol% of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol residues and less than 50 mol% of trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol residues.
[0134] In certain embodiments where the polymer component (A) comprises a copolyester containing TMCD and CHDM residues, the diol component for the copolyester may include, but is not limited to, at least one of the following range combinations: about 10 to about 30 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 90 to about 70 mol% of ethylene glycol; about 10 to about 27 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 90 to about 73 mol% of ethylene glycol; about 15 to about 26 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 85 to about 74 mol % of ethylene glycol; about 18 to about 26 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 82 to about 77 mol % of ethylene glycol; about 20 to about 25 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 80 to about 75 mol % of ethylene glycol; about 21 to about 24 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 79 to about 76 mol % of ethylene glycol; or about 22 to about 24 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 78 to about 76 mol % of ethylene glycol.
[0135] In certain embodiments where polymer component (A) includes a copolyester comprising residues of TMCD and EG, the copolyester may exhibit at least one of the following inherent viscosities, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.25 g / 50 ml at 25° C.: 0.50 to 0.8 dL / g; 0.55 to 0.75 dL / g; 0.57 to 0.73 dL / g; 0.58 to 0.72 dL / g; 0.59 to 0.71 dL / g; 0.60 to 0.70 dL / g; 0.61 to 0.69 dL / g; 0.62 to 0.68 dL / g; 0.63 to 0.67 dL / g; 0.64 to 0.66 dL / g; or about 0.65 dL / g.
[0136] In certain embodiments where polymer component (A) comprises a copolyester comprising TMCD and EG residues, the Tg of the copolyester may be selected from the following ranges: 85 to 100°C; 86 to 99°C; 87 to 98°C; 88 to 97°C; 89 to 96°C; 90 to 95°C; 91 to 95°C; 92 to 94°C.
[0137] In other embodiments, when polymer component (A) comprises a copolyester comprising TMCD and EG residues, the copolyester comprises diol residues comprising 30 to 42 mol% TMCD residues and 58 to 70 mol% EG residues. In one embodiment, the copolyester comprises diol residues comprising 33 to 38 mol% TMCD residues and 62 to 67 mol% EG residues.
[0138] In certain embodiments where the polymer component (A) comprises a copolyester comprising TMCD and EG residues, the copolyester comprises: a) a dicarboxylic acid component comprising: (i) 90-100 mol % terephthalic acid residues; and (ii) from about 0 to about 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: (i) from about 30 to about 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues; and (ii) from about 70 to about 60 mol% of ethylene glycol residues; and wherein the total mol% of the dicarboxylic acid components is 100 mol% and wherein the total mol% of the diol components is 100 mol%; and wherein the inherent viscosity (IV) of the polyester is from about 0.50 to 0.70 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.25 g / 50 ml at 25°C; and the L* color value of the polyester is 90 or more as measured by the L*a*b* color system of ASTM D 6290-98 and ASTM E308-99 measured on polymer particles crushed to a 1 mm sieve. In an embodiment, the L* color value of the polyester is greater than 90 as measured by the L*a*b* color system of ASTM D 6290-98 and ASTM E308-99 measured on polymer particles crushed to a 1 mm sieve.
[0139] In certain embodiments where the polymer component (A) comprises a copolyester comprising TMCD and EG residues, the diol component comprises: (i) from about 32 to about 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues, and (ii) from about 68 to about 60 mol % of ethylene glycol residues; or (i) from about 34 to about 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues, and (ii) from about 66 to about 60 mol % of ethylene glycol residues; or (i) greater than 34 to about 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues, and (i i) less than 66 to about 60 mol % ethylene glycol residues; or (i) 34.2 to about 40 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues, and (ii) 65.8 to about 60 mol % ethylene glycol residues; or (i) about 35 to about 39 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues, and (ii) about 65 to about 61 mol % ethylene glycol residues; or (i) about 36 to about 37 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues, and (ii) about 64 to about 63 mol % ethylene glycol residues.
[0140] In certain embodiments where polymer component (A) includes a copolyester containing TMCD and EG residues, the copolyester has at least one property selected from the group consisting of: a Tg of about 100°C to about 110°C as measured by a TA 2100 thermal analyzer at a scan rate of 20°C / min, a flexural modulus equal to or greater than about 2000 MPa (290,000 psi), or greater than 2200 MPa (319,000 psi) at 23°C as defined by ASTM D790, an Izod notched impact strength of about 30 J / m (0.56 ft-lb / in) to about 80 J / m (1.50 ft-lb / in) at 23°C using a 1 / 8 inch thick bar according to ASTM D256, and a loss in inherent viscosity of less than 5% after being held at a temperature of 293°C (560°F) for 2 minutes. In one embodiment, the polyester composition has an L* color value of 90 or greater, or greater than 90, as measured by the L*a*b* color system of ASTM D 6290-98 and ASTM E308-99 on polymer particles crushed into a 1 mm sieve.
[0141] In one embodiment where polymer component (A) comprises a copolyester containing TMCD and EG residues, the copolyester comprises a diol component having at least 30 mol% TMCD residues (based on the diol) and a catalyst / stabilizer component comprising: (i) titanium atoms in the range of 10-60 ppm based on the weight of the polymer, (ii) manganese atoms in the range of 10-100 ppm based on the weight of the polymer, and (iii) phosphorus atoms in the range of 10-200 ppm based on the weight of the polymer. In one embodiment, the 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues are a mixture comprising greater than 50 mol% cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol residues and less than 50 mol% trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol residues.
[0142] In certain embodiments, the diol component for the copolyester includes, but is not limited to, at least one of the following range combinations: about 30 to about 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 60 to 70 mol% of ethylene glycol; about 32 to about 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 60 to 68 mol% of ethylene glycol; about 32 to about 38 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 64 to 68 mol% of ethylene glycol; about 33 to about 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 60 to 67 mol% of ethylene glycol; about 34 to about 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol alcohol and about 60 to 66 mol % ethylene glycol; greater than 34 to about 40 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 to less than 66 mol % ethylene glycol; 34.2 to 40 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 60 to 65.8 mol % ethylene glycol; about 35 to about 39 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 61 to 65 mol % ethylene glycol; about 35 to about 38 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 62 to 65 mol % ethylene glycol; or about 36 to about 37 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and about 63 to 64 mol % ethylene glycol.
[0143] In certain embodiments where polymer component (A) comprises a copolyester comprising TMCD and EG residues, the polyester may exhibit at least one of the following inherent viscosities, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.25 g / 50 ml at 25° C.: 0.50 to 0.70 dL / g; 0.55 to 0.65 dL / g; 0.56 to 0.64 dL / g. L / g; 0.56 to 0.63 dL / g; 0.56 to 0.62 dL / g; 0.56 to 0.61 dL / g; 0.57 to 0.64 dL / g; 0.58 to 0.64 dL / g; 0.57 to 0.63 dL / g; 0.57 to 0.62 dL / g; 0.57 to 0.61 dL / g; 0.58 to 0.60 dL / g or about 0.59 dL / g.
[0144] In certain embodiments where polymer component (A) comprises a copolyester comprising TMCD and EG residues, such copolyester may contain less than 10 mol%, or less than 5 mol%, or less than 4 mol%, or less than 3 mol%, or less than 2 mol%, or less than 1 mol%, or no CHDM residues.
[0145] In embodiments, the polyesters used in embodiments of polymer composition (A) described herein may exhibit at least one of the following inherent viscosities, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.: 0.10 to 1.2 dL / g; 0.10 to 1.1 dL / g; 0.10 to 1 dL / g; 0.10 to less than 1 dL / g; 0.10 to 0.98 dL / g; 0.10 to 0.95 dL / g; 0.10 to 0.90 dL / g; 0.10 to 0.85 dL / g; 0.10 to 0.80 dL / g; 0.10 to 0.75 dL / g; 0.10 to less than 0.75 dL / g; 0.10 to 0.72 dL / g; 0.10 to 0.70 dL / g; 0.10 to less than 0.70 dL / g; 0.10 to 0.68 dL / g; 0.10 to less than 0.68 dL / g; 0.10 to 0.65 dL / g; 0.20 to 1.2 dL / g; 0.20 to 1.1 dL / g; 0.20 to 1 dL / g; 0.2 0 to less than 1 dL / g; 0.20 to 0.98 dL / g; 0.20 to 0.95 dL / g; 0.20 to 0.90 dL / g; 0.20 to 0.85 dL / g; 0.20 to 0.80 dL / g; 0.20 to 0.75 dL / g; 0.20 to less than 0.75 dL / g; 0.20 to 0.72 dL / g; 0.20 to 0.70 dL / g; 0.20 to less than 0.70 dL / g; 0.20 to 0.68 dL / g; 0.20 to less than 0.68 dL / g; 0.20 to 0.65 dL / g; 0.35 to 1.2 dL / g; 0.35 to 1.1 dL / g; 0.35 to 1 dL / g; 0.35 to less than 1 dL / g; 0 .35 to 0.98 dL / g; 0.35 to 0.95 dL / g; 0.35 to 0.90 dL / g; 0.35 to 0.85 dL / g; 0.35 to 0.80 dL / g; 0.35 to 0.75 dL / g; 0.35 to less than 0.75 dL / g; 0.35 to 0.72 dL / g; 0.35 to 0.70 dL / g g; 0.35 to less than 0.70 dL / g; 0.35 to 0.68 dL / g; 0.35 to less than 0.68 dL / g; 0.35 to 0.65 dL / g; 0.40 to 1.2 dL / g; 0.40 to 1.1 dL / g; 0.40 to 1 dL / g; 0.40 to less than 1 dL / g; 0.40 to 0.98 dL / g; 0.40 to 0.95 dL / g; 0.40 to 0.90 dL / g; 0.40 to 0.85 dL / g; 0.40 to 0.80 dL / g; 0.40 to 0.75 dL / g; 0.40 to less than 0.75 dL / g; 0.40 to 0.72 dL / g; 0.40 to 0.70 dL / g; 0.40 to less than 0.70 dL / g; 0.40 to 0.68 dL / g; 0.40 to less than 0.68 dL / g; 0.40 to 0.65 dL / g; greater than 0.42 to 1.2 dL / g; greater than 0.42 to 1.1 dL / g; greater than 0.42 to 1 dL / g; greater than 0.42 to less than 1 dL / g; greater than 0.42 to 0.98 dL / g; greater than 0.42 to 0.95 dL / g; greater than 0.42 to 0.90 dL / g; greater than 0.42 to 0.85 dL / g; greater than 0.42 to 0.80 dL / g; greater than 0.42 to 0.75 dL / g; greater than 0.42 to less than 0.75 dL / g; greater than 0.42 to 0.72 dL / g; greater than 0.42 to less than 0.70 dL / g; greater than 0.42 to 0.68 dL / g; greater than 0.42 to less than 0.68 dL / g; and greater than 0.42 to 0.65 dL / g. .
[0146] For certain embodiments, the polyesters described herein for embodiments comprising 1,4-cyclohexanedicarboxylate polymer compositions (B) or (C) may exhibit at least one of the following inherent viscosities, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.: 0.45 to 1.50 dL / g; 0.45 to 1.40 dL / g; 0.45 to 1.30 dL / g; 0.45 to 1.25 dL / g; 0.45 to 1.20 dL / g; 0.45 to 1.15 dL / g; 0.45 to 1.10 dL / g; 0.45 to 1.05 dL / g; 0.45 to less than 1 dL / g; 0.50 to 1.50 dL / g; 0.50 to 1.40 dL / g; 0.50 to 1.30 dL / g; 0.50 to less than 1.25 dL / g; 0.60 to 1.30 dL / g; 0.60 to 1.20 dL / g; 0.60 to 1.10 dL / g; 0.70 to 1.30 dL / g; 0.70 to 1.20 dL / g; 0.70 to 1.10 dL / g; 0.80 to less than 1.5 dL / g; 0.80 to 1.45 dL / g; 0.80 to 1.40 dL / g; 0.80 to less than1.40dL / g; 0.80 to 1.35dL / g; 0.80 to less than 1.3dL / g; 0.80 to 1.25dL / g; 0.80 to 1.20dL / g; 0.80 to 1.15dL / g; 0.80 to 1.10dL / g; 0.80 to less than 1.10dL / g; 0.80 to 1.05dL / g; 0.80 to 1.0 0dL / g; 0.80 to 0.95dL / g; 0.80 to 0.90dL / g; 0.85 to 1.50dL / g; 0.85 to 1.40dL / g; 0.85 to less than 1.40dL / g; 0.85 to 1.35dL / g; 0.85 to 1.30dL / g; 0.85 to less than 1.30dL / g; 0.85 to 1.25dL / g; 0 .85 to less than 1.25 dL / g; 0.85 to 1.20 dL / g; 0.85 to 1.15 dL / g; 0.85 to 1.10 dL / g; 0.85 to 1.05 dL / g; 0.85 to less than 1.0 dL / g; 0.90 to 1.50 dL / g; 0.90 to 1.40 dL / g; 0.90 to 1.30 dL / g; 0.90 to 1.2 5dL / g; 0.90 to 1.20dL / g; 0.90 to 1.15dL / g; 0.90 to 1.10dL / g; 0.90 to 1.05dL / g; 0.90 to 1.10dL / g; 1.0 to less than 1.50dL / g; 1.0 to 1.4dL / g; 1.0 to less than 1.3dL / g; 1.0 to less than 1.25dL / g; 1.0 to 1.20dL / g; 1.0 to 1.10 dL / g; 1.05 to 1.25 dL / g; 1.05 to less than 1.25 dL / g; 1.05 to 1.20 dL / g; 1.05 to 1.15 dL / g; 1.05 to 1.10 dL / g; greater than 0.80 dL / g to 1.50dL / g; greater than 0.80dL / g to 1.40dL / g; greater than 0.80dL / g to less than 1.30dL / g; greater than 0.85dL / g to 1.30dL / g; greater than 0.85dL / g to 1.25dL / g; greater than 0.85dL / g to 1.20dL / g; greater than 0.85dL / g to 1.15dL / g; greater than 0.85dL / g to 1.10dL / g; greater than 0.85dL / g to 1.05dL / g; greater than 0.85dL / g to 1.0dL / g; greater than 0.90dL / g to 1.30dL / g; greater than 0.95dL / g to 1.30dL / g; greater than 1.0dL / g to 1.30dL / g. .
[0147] In certain embodiments, the acid component for the polymer component (B) or (C) comprising 1,4-cyclohexanedicarboxylic acid ester includes, but is not limited to, at least one of the following range combinations: about 90 to about 100 mol% of 1,4-cyclohexanedicarboxylic acid residues; and about 0 to 10 mol% of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; about 90 to 98 mol% of 1,4-cyclohexanedicarboxylic acid residues and about 2 to 10 mol% of modified aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; about 90 to 95 mol% of 1,4-cyclohexanedicarboxylic acid residues and about 5 to 10 mol% of modified aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; about 90 to 93 mol% of 1,4-cyclohexanedicarboxylic acid residues and about 7 to 10 mol % of modified aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; about 92 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues and about 0 to 8 mol % of modified aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; about 95 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues and about 0 to 5 mol % of modified aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; about 98 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues and about 0 to 2 mol % of modified aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; or about 100 mol % of 1,4-cyclohexanedicarboxylic acid residues and no modified aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms.
[0148] In certain embodiments, the diol component for the polymer component (B) or (C) comprising 1,4-cyclohexane dicarboxylate includes, but is not limited to, at least one of the following range combinations: about 90 to about 100 mol % of 1,4-cyclohexanedimethanol residues and about 0 to 10 mol % of modifying diol residues; about 90 to about 98 mol % of 1,4-cyclohexanedimethanol residues and about 2 to 10 mol % of modifying diol residues; about 90 to about 95 mol % of 1,4-cyclohexanedimethanol residues and about 5 to 10 mol % of modifying diol residues; about 90 to about 100 mol % of 1,4-cyclohexanedimethanol residues and about 0 .... 93 mol % of 1,4-cyclohexanedimethanol residues and about 7 to 10 mol % of modifying diol residues; about 92 to about 100 mol % of 1,4-cyclohexanedimethanol residues and about 0 to 8 mol % of modifying diol residues; about 95 to about 100 mol % of 1,4-cyclohexanedimethanol residues and about 0 to 5 mol % of modifying diol residues; about 98 to about 100 mol % of 1,4-cyclohexanedimethanol residues and about 0 to 2 mol % of modifying diol residues; or about 100 mol % of 1,4-cyclohexanedimethanol residues and no modifying diol residues.
[0149] In an embodiment, the inherent viscosity (IV) of component (B) or (C) comprising 1,4-cyclohexanedicarboxylate is in the range of 0.70 to 1.5 dL / g, or 0.75 to 1.3 dL / g, or 0.8 to 1.2 dL / g, 0.8 to 1.1 dL / g, or 0.85 to 1.1 dL / g, or 0.85 to 1.0 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C. In embodiments, component (B) or (C) comprising 1,4-cyclohexanedicarboxylate has a glass transition temperature (Tg) of less than 110°C, or less than 100°C, or less than 90°C, or less than 80°C, or in the range of 30°C to 100°C, or 40°C to 90°C, 50°C to 80°C, or 60°C to 75°C as determined by DSC. In an embodiment, component (B) or (C) comprising 1,4-cyclohexanedicarboxylate has an elongation at break of at least 50%, or at least 75%, or at least 100%, or in the range of 50% to 300%, or 100% to 200%, as measured in accordance with ASTM D 638; and / or a flexural modulus in the range of 500 to 2000 MPa, or 750 to 1500 MPa, or 800 to 1200 MPa, as measured in accordance with ASTM D 790; and / or a tear strength of at least 10 N, or at least 50 N, or at least 100 N, or in the range of 10 N to 200 N, or 10 N to 150 N, or 10 N to 100 N, as measured in accordance with ASTM D 1004.
[0150] In an embodiment, the polymer component (B) or (C) may include a polyester ether or a copolyester ether (COPE), such as (PCCE) commercially available from Eastman Chemical Company. The term "polyester" used herein with respect to component (B) or (C) includes copolyester ethers. The copolyester ether may be derived from a dicarboxylic acid component comprising and / or consisting essentially of 1,4-cyclohexanedicarboxylic acid or an ester-forming derivative thereof such as dimethyl 1,4-cyclohexanedicarboxylate. Both the acid and the ester are sometimes referred to herein as DMCD. The diol component consists essentially of 1,4-cyclohexanedimethanol (CHDM) and polytetramethylene ether glycol (PTMG). The copolyester ether may also include a branching agent, such as, based on the acid or diol component, from about 0.1 to about 1.5 mol % of a multifunctional branching agent having at least 3 carboxyl or hydroxyl groups.
[0151] In an embodiment, the dibasic acid component of the copolyester ether comprises residues of 1,4-cyclohexanedicarboxylic acid or dimethyl 1,4-cyclohexanedicarboxylate having a trans isomer content of at least 70%, or at least 80%, or at least 85%. In an embodiment, the dibasic acid component of the copolyester ether may consist essentially of DMCD and may have a trans isomer content of at least 70%, or at least 80%, or at least 85%.
[0152] In an embodiment, the polyester ether useful for the core or inner layer may contain residues of 1,4-cyclohexanedicarboxylic acid or its esters in an amount of 70 to 100 wt%, or 80 to 100 wt%, or 90 to 100 wt%, or 95 to 100 wt%, or 98 to 100 wt%, based on a total of 100 wt% of the acid residues and a total of 100 wt% of the glycol residues. The polyester ether may contain residues of 1,4-cyclohexanedimethanol and polytetramethylene ether glycol.
[0153] In certain embodiments, the polyester ether may comprise 1 to 50 mol%, or 5 to 50 mol%, or 10 to 50 mol%, or 15 to 50 mol%, or 20 to 50 mol%, or 25 to 50 mol%, or 30 to 50 mol%, or 35 to 50 mol%, or 40 to 50 mol%, or 45 to 50 mol%, or 1 to 45 mol%, or 5 to 45 mol%, or 10 to 45 mol%, or 15 to 45 mol%, or 20 to 45 mol%, or 25 to 45 mol%, or 30 to 45 mol%, or 35 to 45 mol%, or 40 to 45 mol%, or 1 to 40 mol%, or 5 to 40 mol%, or 10 to 40 mol%, or 15 to 40 mol%, or 20 to 40 mol%, or 25 to 40 mol%, or 30 to 40 mol%, or 35 to 40 mol%, or % or 1 to 35 mol%, or 5 to 35 mol%, or 10 to 35 mol%, or 15 to 35 mol%, or 20 to 35 mol%, or 25 to 35 mol%, or 30 to 35 mol%, or 1 to 30 mol%, or 5 to 30 mol%, or 10 to 30 mol%, or 15 to 30 mol%, or 20 to 30 mol% or 25 to 30 mol%, or 1 to 25 mol%, or 5 to 25 mol%, or 10 to 25 mol%, or 15 to 25 mol%, or 20 to 25 mol%, or 1 to 20 mol%, or 5 to 20 mol%, or 10 to 20 mol%, or 15 to 20 mol%, or 1 to 15 mol%, or 5 to 15 mol%, or 10 to 15 mol%, or 1 to 10 mol%, or 5 to 10 mol%, or 1 to 5 mol% of residues of polytetramethylene ether glycol residues.
[0154] In certain embodiments, the polyester ether may comprise residues of polytetramethylene ether glycol residues from 1 mol % to 20 mol %, or from 1 mol % to 15 mol %, or from 1 mol % to 12 mol %, or from 1 mol % to 10 mol %, or from 3 mol % to 12 mol %, or from 5 mol % to 10 wt %, or from 7 mol % to 10 mol %.
[0155] In one embodiment, the polyester portion of the polyester ether comprises the residue of at least one diol of the polyester used in the present invention. In certain embodiments, the polyester portion of the polyester ether comprises the residue of at least one diol selected from ethylene glycol, diethylene glycol, triethylene glycol, isosorbide, propane-1,3-diol, 1,4-butanediol, 2,2-dimethylpropane-1,3-diol (neopentyl glycol), 2,2,4,4,-tetramethyl-1,3-cyclobutanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 3-methyl-pentanediol-(2,4), 2-methylpentanediol-(1, 4), 2,2,4-trimethylpentanediol-(1,3), 2-ethylhexanediol-(1,3), 2,2-diethylpropylene glycol-(1,3), hexanediol-(1,3), 1,4-bis-(hydroxyethoxy)-benzene, 2,2-bis-(4-hydroxycyclohexyl)-propane, 2,4-dihydroxy-1,1,3,3-tetramethyl-cyclobutane, 2,2-bis-(3-hydroxyethoxyphenyl)-propane, 2,2-bis-(4-hydroxypropoxyphenyl)-propane and mixtures thereof. In an embodiment, the balance of the diol component of the polyester ether, other than the polytetramethylene ether glycol (PTMG) residues, is substantially 1,4-cyclohexanedimethanol (CHDM) residues. In an embodiment, the diol component of the polyester ether comprises less than 10 mol%, or less than 5 mol%, or less than 2 mol%, or less than 1 mol% of diol residues other than residues of CHDM and PTMG.
[0156] In embodiments, the polyester ether may comprise from 50 wt% to 95 wt%, or from 55 wt% to 95 wt%, or from 60 wt% to 95 wt%, or from 70 wt% to 95 wt%, or from 75 wt% to 95 wt%, or from 80 wt% to 95 wt% of residues of 1,4-cyclohexanedimethanol residues. In embodiments, the polyester ether is free of residues of ethylene glycol.
[0157] In an embodiment, component (B) or (C) comprises a polyester ether having an inherent viscosity (IV) in the range of 0.70 to 1.5 dL / g, or 0.8 to 1.4 dL / g, or 0.9 to 1.3 dL / g, 1.0 to 1.2 dL / g, or 1.1 to 1.2 dL / g, or 1.14 to 1.18 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C. In an embodiment, the polyester ether has a glass transition temperature (Tg) of less than 0°C, or less than -10°C, or less than -20°C, or less than -30°C, or in the range of -60°C to 0°C, or -50°C to -10°C, -60°C to -20°C, or -50°C to -30°C, as measured by DSC. In embodiments, the polyester ether has an elongation at break of at least 200%, or at least 300%, or at least 350%, or in the range of 200% to 600%, or 300% to 500%, as measured in accordance with ASTM D 638; and / or a flexural modulus in the range of 50 to 250 MPa, or 100 to 200 MPa, as measured in accordance with ASTM D 790; and / or a tear strength of at least 200 N, or at least 250 N, or at least 300 N, or in the range of 200 N to 500 N, or 250 N to 450 N, or 300 N to 400 N, as measured in accordance with ASTM D1004.
[0158] In one embodiment, the copolyester ether contained in component (B) or (C) may have an inherent viscosity of about 0.70 to about 1.5 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C., and may comprise:
[0159] A. a dicarboxylic acid component comprising and / or consisting essentially of 1,4-cyclohexanedicarboxylic acid, and
[0160] B. A diol component consisting essentially of:
[0161] (1) 1,4-cyclohexanedimethanol, and
[0162] (2) from about 1 to about 50 mol %, or 1 to 20 mol %, or 1 to 15 mol %, or 2 to 10 mol % of polytetramethylene ether glycol (PTMG) having a weight average molecular weight of from about 500 to about 2000, based on the moles of the diol component of the polyester ether.
[0163] In one embodiment, the copolyester ether may further comprise (3) about 0.1 to about 1.5 mol %, or 0.1 to 1.0 mol % of a branching agent having at least three COOH or OH functional groups and 3 to 60 carbon atoms, based on the total mol % of the acid or diol component.
[0164] The relative amounts of each component of the polyester-containing polyester (in a multi-component composition) according to various embodiments are described below. For the purposes of this application: "TMCD and CHDM polyester" refers to any embodiment of a polyester described herein that contains both TMCD and CHDM residues in the diol component of the polyester; "TMCD and EG polyester" refers to any embodiment of a polyester described herein that contains both TMCD and EG residues in the diol component of the polyester; "isosorbide polyester" refers to any embodiment of a polyester described herein that contains isosorbide residues in the diol component of the polyester; "1,4-cyclohexanedicarboxylate polyester" refers to any embodiment of a polyester described herein that contains 1,4-cyclohexanedicarboxylate residues in the diacid component of the polyester; and "polyester ether" refers to any embodiment of a polyester described herein that contains a polyester ether in the diol component of the polyester.
[0165] In an embodiment, the multi-component composition includes a polymer component (A) comprising TMCD and CHDM polyester, or TMCD and EG polyester, and a component (B) comprising 1,4-cyclohexanedicarboxylate polyester in an amount of one or more of: 50 to 99 wt% of component (A) and 1 to 50 wt% of component (B), or greater than 50 to 99 wt% of component (A) and 1 to less than 50 wt% of component (B), or 55 to 99 wt% of component (A) and 1 to 45 wt% of component (B). % of component (A) and 1 to 40 wt% of component (B), or 65 to 99 wt% of component (A) and 1 to 35 wt% of component (B), or 70 to 99 wt% of component (A) and 1 to 30 wt% of component (B), or 75 to 99 wt% of component (A) and 1 to 25 wt% of component (B), or 80 to 99 wt% of component (A) and 1 to 20 wt% of component (B), or 55 to 95 wt% of component (A) and 5 to 30 wt% of component (B), 45wt% of component (B), or 60 to 95wt% of component (A) and 5 to 40wt% of component (B), or 65 to 95wt% of component (A) and 5 to 35wt% of component (B), or 70 to 95wt% of component (A) and 5 to 30wt% of component (B), or 75 to 95wt% of component (A) and 5 to 25wt% of component (B), or 80 to 95wt% of component (A) and 5 to 20wt% of component (B), or 55 to 90wt% of component (A) (A) and 10 to 45 wt% of component (B), or 60 to 90 wt% of component (A) and 10 to 40 wt% of component (B), or 65 to 90 wt% of component (A) and 10 to 35 wt% of component (B), or 70 to 90 wt% of component (A) and 10 to 30 wt% of component (B), or 75 to 90 wt% of component (A) and 10 to 25 wt% of component (B), or 80 to 90 wt% of component (A) and 10 to 20 wt% of component (B). In an embodiment, the multi-component composition includes component (B) containing 30 to 50 wt%, or 30 to less than 50 wt%, or 35 to 45 wt% of 1,4-cyclohexane dicarboxylate polyester. In an embodiment, this range of component B can provide a unique balance of tear resistance, modulus, and force retention properties.
[0166] In an embodiment, the multi-component composition comprises a polymer component (A) comprising TMCD and CHDM polyester or TMCD and EG polyester, and a component (B) comprising a polyester ether in an amount of one or more of: greater than 50 to 99 wt% of component (A) and 1 to less than 50 wt% of component (B), or 55 to 99 wt% of component (A) and 1 to 45 wt% of component (B), or 60 to 99 wt% of component (A) and 1 to 40 wt% of component (B). (B), or 65 to 99 wt% of component (A) and 1 to 35 wt% of component (B), or 70 to 99 wt% of component (A) and 1 to 30 wt% of component (B), or 75 to 99 wt% of component (A) and 1 to 25 wt% of component (B), or 80 to 99 wt% of component (A) and 1 to 20 wt% of component (B), or 55 to 95 wt% of component (A) and 5 to 45 wt% of component (B), or 60 to 95 wt% of component (A) and 5 to 45 wt% of component (B), % of component (A) and 5 to 40 wt% of component (B), or 65 to 95 wt% of component (A) and 5 to 35 wt% of component (B), or 70 to 95 wt% of component (A) and 5 to 30 wt% of component (B), or 75 to 95 wt% of component (A) and 5 to 25 wt% of component (B), or 80 to 95 wt% of component (A) and 5 to 20 wt% of component (B), or 55 to 90 wt% of component (A) and 10 to 45 wt% of component (B). t% of component (B), or 60 to 90wt% of component (A) and 10 to 40wt% of component (B), or 65 to 90wt% of component (A) and 10 to 35wt% of component (B), or 70 to 90wt% of component (A) and 10 to 30wt% of component (B), or 75 to 90wt% of component (A) and 10 to 25wt% of component (B), or 80 to 90wt% of component (A) and 10 to 20wt% of component (B).
[0167] In an embodiment, the multi-component composition comprises a polymer component (A) containing an isosorbide polyester and a component (B) containing a polyester ether in an amount of one or more of the following: greater than 50 to 99 wt% of component (A) and 1 to less than 50 wt% of component (B), or 55 to 99 wt% of component (A) and 1 to 45 wt% of component (B), or 60 to 99 wt% of component (A) and 1 to 40 wt% of component (B), or 65 to 99 wt% of component (A) and 1 to 40 wt% of component (B). % of component (A) and 1 to 35 wt% of component (B), or 70 to 99 wt% of component (A) and 1 to 30 wt% of component (B), or 75 to 99 wt% of component (A) and 1 to 25 wt% of component (B), or 80 to 99 wt% of component (A) and 1 to 20 wt% of component (B), or 55 to 95 wt% of component (A) and 5 to 45 wt% of component (B), or 60 to 95 wt% of component (A) and 5 to 40 wt% of component (B), or 65 to 95 wt% of component (A) and 5 to 35 wt% of component (B), or 70 to 95 wt% of component (A) and 5 to 30 wt% of component (B), or 75 to 95 wt% of component (A) and 5 to 25 wt% of component (B), or 80 to 95 wt% of component (A) and 5 to 20 wt% of component (B), or 55 to 90 wt% of component (A) and 10 to 45 wt% of component (B). (B), or 60 to 90 wt% of component (A) and 10 to 40 wt% of component (B), or 65 to 90 wt% of component (A) and 10 to 35 wt% of component (B), or 70 to 90 wt% of component (A) and 10 to 30 wt% of component (B), or 75 to 90 wt% of component (A) and 10 to 25 wt% of component (B), or 80 to 90 wt% of component (A) and 10 to 20 wt% of component (B).
[0168] In certain embodiments, the polymer component (A) described herein is a minority component of a multi-component composition. In such embodiments, the major component may be the polymer component (B) described in any of the embodiments herein.
[0169] In certain embodiments, the multi-component composition forms or is included in one or more layers of the multi-layer structure film. In an embodiment, the multi-layer structure film is a three-layer structure having a core layer and two outer layers, with an outer layer on each side of the core layer. In an embodiment, the core layer comprises a multi-component composition, and the outer layer is made of other polymer compositions. In an embodiment, at least one outer layer comprises a multi-component composition, and the core layer is made of another polymer composition.
[0170] As described above, the total thickness of the film may range from about 100 μM to about 3000 μM, or about 300 μM to about 3000 μM. In other embodiments, the sheet thickness ranges from about 380 μM to about 1600 μM, or about 500 μM to 1000 μM.
[0171] Multicomponent composition films can be produced by compounding and extrusion, among other methods.
[0172] In the embodiment with the film structure of at least three layers, the core layer thickness can be in the range of about 1 μM to about 1000 μM. In certain embodiments, the core layer thickness ranges from about 1 μM to about 725 μM, or 1 μM to 600 μM. In certain embodiments, the outer layer thickness is each individually about 1 μM to about 2000 μM. In another embodiment, the outer layer thickness is about 25 μM to about 2000 μM.
[0173] Multilayer film can be prepared by coextrusion, extrusion lamination, hot lamination, adhesive lamination, etc. In coextrusion, multilayer polymer is produced by melting the polymer composition of each layer in different extruders, and the polymer composition is fed into a coextrusion module or die. Multilayer sheet or film is formed in this module or die. Extrusion lamination is a method in which at least two sheets or films (monolayer or coextrusion) are combined together by extruding a polymer melt between them, thereby producing a multilayer structure. Adhesive lamination adopts at least two sheets or films (monolayer or coextrusion) and uses a liquid adhesive to bond them together to produce multilayer sheet or film. Hot lamination is a batch method in which slices or films of various compositions or structures are stacked in a hot press. Multiple combinations and multilayers can be manufactured using these methods.
[0174] In the case where a multilayer film having a core layer and outer layers as described herein tends to separate or delaminate from each other during processing or use, at least one intermediate "tie layer" may be used between these layers. In one embodiment, the multilayer film has at least five film layers, including a core layer A and two outer layers B, one layer B on each side of the core layer A, and a tie layer between layer A and each layer B, i.e., "B-tie-A-tie-B". In certain embodiments, such tie layers may comprise one or more copolymers selected from polyethylene copolymers, polypropylene copolymers, anhydride-modified polyolefins, acid / acrylate-modified ethylene vinyl acetate copolymers, acid-modified ethylene acrylates, anhydride-modified ethylene acrylates, modified ethylene vinyl acetate, anhydride-modified ethylene vinyl acetate copolymers, anhydride-modified high density polyethylene, anhydride-modified linear low density polyethylene, anhydride-modified polypropylene, ethylene ethyl acrylate maleic anhydride copolymers and ethylene butyl acrylate maleic anhydride terpolymers, ethylene-α-olefin copolymers, olefin-unsaturated carboxylic acid or carboxylic acid derivative copolymers, ethylene-methacrylic acid copolymers, ethylene-vinyl acetate copolymers, ethylene-methacrylic acid copolymers, unsaturated dicarboxylic acid anhydride grafted copolymers, maleic anhydride grafted ethylene-vinyl acetate copolymers, maleic anhydride grafted polyethylene, styrene-butadiene copolymers, C3 or higher α-olefin copolymers with high α-olefin comonomer content, propylene-1-butene copolymers, and mixtures thereof.
[0175] In embodiments, the film (e.g., a monolayer or multilayer film, depending on the embodiment) has a tear force of at least 10 N, or at least 20 N, or at least 30 N, or at least 40 N, or at least 50 N, or at least 60 N, or in the range of 10 N to 100 N, or 20 N to 100 N, or 40 N to 100 N, or 50 N to 90 N, or 60 N to 80 N, according to ASTM D 1938; and / or 70% or less, or 50% or less, or 10 to 70%, or 10 to 50%, or 20 to 50%, or 20 to 40% force retention, as measured in the embodiments herein; and / or greater than 1000 MPa, or at least 1200 MPa, or at least 1500 MPa, or a flexural modulus in the range of greater than 1000 to 2200 MPa, or greater than 1200 to 2000 MPa, or greater than 1500 to 2000 MPa, or 1600 to 2000 MPa, or 1600 to 1800 MPa, measured according to ASTM D790. In an embodiment, the multilayer sheet has the above-mentioned tear force and force retention properties. In an embodiment, the film has each of the above-mentioned tear force, force retention and flexural modulus properties. In embodiments, the total thickness of the film is in the range of 100 to 1050 microns, or 500 to 1050 microns, or 500 to 1000 microns, or 600 to 900 microns, or 600 to 800 microns, or 635 microns (25 mils) to 889 microns (35 mils), or 635 microns (25 mils) to 762 microns (30 mils). In embodiments of multilayer films, the thickness of the inner layer (or core layer) may be 10% to 50%, or 15% to 45%, or 20% to 40%, or 20% to 35%, or 25% to 35% of the total thickness of the multilayer film.
[0176] Due to its structure with customizable modulus and excellent tear resistance, the film can be used to prepare removable orthodontic tooth positioning aligners, as long as the film has a sufficiently high modulus and excellent tear resistance. See, for example, US Patents 9,655,691; 9,655,693; 10,052,176, which are hereby incorporated by reference into this specification.
[0177] Thus, in another embodiment, the present invention provides a removable orthodontic tooth positioning appliance having a tooth receiving cavity shaped to directly receive at least some of the patient's teeth, the appliance comprising a polymer structure formed from a film comprising a multi-component composition comprising at least two polymer components (A) and (B), wherein polymer component (A) is present in an amount of greater than 50 to 99 wt % and polymer component (B) is present in an amount of 1 to less than 50 wt %; and wherein polymer component (A) comprises a polyester comprising:
[0178] (a) a dicarboxylic acid component comprising:
[0179] i) 70 to 100 mol % of terephthalic acid residues; and
[0180] ii) 0 to 30 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0181] (b) a diol component comprising:
[0182] i) 10 to 50 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues;
[0183] ii) 0 to 90 mol% of 1,4-cyclohexanedimethanol residues; and
[0184] iii) 0 to 90 mol % of ethylene glycol residues; and having an inherent viscosity of about 0.4 to about 0.9 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.; and
[0185] The polymer component (B) comprises a polyester different from the polyester in the polymer component (A), and wherein the total thickness of the film is from 100 to 3000 microns, or from 300 to 3000 microns.
[0186] In another embodiment, the polymer component (A) comprises a polyester comprising:
[0187] (a) a dicarboxylic acid component comprising:
[0188] i) 90 to 100 mol % of terephthalic acid residues;
[0189] ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0190] (b) a diol component comprising:
[0191] i) 10 to 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues;
[0192] ii) 60 to 90 mol% of 1,4-cyclohexanedimethanol residues; and
[0193] Having an inherent viscosity of about 0.5 to about 0.9 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
[0194] In another embodiment, the polymer component (A) comprises a polyester comprising:
[0195] (a) a dicarboxylic acid component comprising:
[0196] i) 90 to 100 mol % of terephthalic acid residues;
[0197] ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0198] (a) a diol component comprising:
[0199] i) 10 to 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues;
[0200] ii) 60 to 90 mol% of ethylene glycol residues; and having an inherent viscosity of about 0.4 to about 0.9 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C. In another embodiment, the inherent viscosity of polymer component (A) is about 0.5 to 0.7 dL / g.
[0201] In an embodiment, a film comprising a multi-component composition for forming an appliance may include any of the film embodiments described herein and any combination of polymer components (A) and (B) for a two (or more) component composition, or any combination of polymer components (A), (B), and (C) for a three (or more) component composition.
[0202] In another embodiment, the present invention provides a removable orthodontic tooth positioning appliance having a tooth receiving cavity formed to directly receive at least a portion of a patient's teeth, the appliance comprising a multilayer polymer structure formed by a film comprising two outer layers and at least one core layer, wherein at least one layer comprises the multi-component composition described herein.
[0203] In an embodiment, a dental appliance may be made from any of the single or multi-layer films described herein.
[0204] The present invention may be further illustrated by the following examples of specific embodiments thereof, but it should be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the present invention unless otherwise expressly stated.
[0205] Example
[0206] The following examples are provided to illustrate certain embodiments of the invention.
[0207] Test methods
[0208] The tensile properties of the examples were determined using a test method derived from ASTM D882. Small V-shaped tensile bars were cut from the films. Unless otherwise stated, samples were aged for at least 40 hours and tested at 23°C / 50% relative humidity. The crosshead speed used was 1.27 mm / min.
[0209] The flexural properties of the embodiments were determined using a test method derived from ASTM D790, Procedure A. Unless otherwise stated, the films were aged for 24 hours and tested at 23°C / 50% relative humidity. The crosshead speed was 1.27 mm / min.
[0210] The tear force of the examples was determined using a test method derived from ASTM D 1938. Unless otherwise stated, the films were aged for 24 hours and tested at 23°C / 50% relative humidity. The load was applied at 250 mm / min.
[0211] The stress relaxation properties of the examples were analyzed using dynamic mechanical analysis (DMA) in tensile mode on film samples with a thickness of 0.7-0.8 mm and a width of 3.1-3.3 mm. The samples were held at 0.5% strain for 24 hours, during which the stress was monitored. The test was conducted at 37°C and a relative humidity of 90-100% (which may include testing while immersed in water).
[0212] The hardness of the examples was determined using a test method derived from ASTM D 2240. Unless otherwise stated, samples were conditioned for at least 40 hours and tested at 23°C / 50% relative humidity.
[0213] Examples
[0214] The materials used in the examples include:
[0215] R1 – Tritan copolyester MP100 (Eastman Chemical Company)
[0216] R2 – Neostar 19972 elastomer (Eastman Chemical Company)
[0217] R3 – Ecdel 9966 elastomer (Eastman Chemical Company)
[0218] M1 – Kane Ace MV-01 core-shell impact modifier (Kaneka)
[0219] Example 1
[0220] Example 1 was conducted by blending R1 with two different polyesters in different amounts. Examples 1-1 to 1-4 are blends of R1 with 15, 30, 40 and 50 wt% R2, respectively. Examples 1-5 and 1-6 are blends of R1 with 15 and 30 wt% R3, respectively.
[0221] Example 2
[0222] Example 2 was conducted using unblended R1 and blending R1 with a core-shell polymer impact modifier in varying amounts. Example 2-1 is unblended (or neat) R1. Examples 2-2 to 2-4 are blends of R1 with M1 at 3, 4, and 5 wt% loadings, respectively.
[0223] All blends were compounded on a 26 mm twin screw extruder and strand pelletized prior to film extrusion. Compounder barrel and die temperatures were in the range of 260-270°C. Film samples were extruded on a 1.5″ single screw extruder with a target film thickness of 0.7-0.8 mm. Film extrusion barrel temperature was 260-270°C. All materials were dried prior to compounding and extrusion. The properties provided were tested using the methods outlined in the “Test Conditions” above. The results for Example 1 are listed in Table 1 below and the results for Example 2 are listed in Table 2 below.
[0224] Table 1 - Properties of Example 1
[0225]
[0226]
[0227] Review of Table 1 shows that blending R2 and R3 into R1 provides the ability to balance certain properties, such as modulus, tear resistance, and force relaxation, depending on the specific application needs. Examples 1-2 through 1-4 result in a significant increase in tear resistance while maintaining a balance of modulus and force retention.
[0228] Table 2 - Properties of Example 2
[0229]
[0230]
[0231] Review of Table 2 shows that the addition of M1 has less impact on changing certain properties such as modulus compared to the blends in Table 1.
[0232] The invention has been described in detail with particular reference to specific embodiments thereof, but it will be understood that variations and modifications can be effected within the spirit and scope of the invention.
Claims
1. A film comprising a multi-component composition comprising at least two polymer components (A) and (B), wherein the polymer component (A) is present in an amount of 50 to 99 wt%, or greater than 50 to 99 wt%, and the polymer component (B) is present in an amount of 1 to 50 wt%, or 1 to less than 50 wt%; and wherein The polymer component (A) comprises a polyester comprising: (a) a dicarboxylic acid component comprising: i) 70 to 100 mol % of terephthalic acid residues; and ii) 0 to 30 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: i) 10 to 50 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues; ii) 0 to 90 mol% of 1,4-cyclohexanedimethanol residues; and iii) 0 to 90 mol% of ethylene glycol residues; and having an inherent viscosity of about 0.4 to about 0.9 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.; and The polymer component (B) comprises a polyester different from the polyester in the polymer component (A); wherein the total thickness of the film is from 100 to 3000 microns.
2. The film according to claim 1, wherein The polymer component (B) comprises a polyester comprising: (a) a dicarboxylic acid component comprising 1,4-cyclohexanedicarboxylate residues, and (b) a diol component comprising 1,4-cyclohexanedimethanol residues.
3. The film according to claim 1 or 2, wherein the polymer component (B) comprises a polyester comprising: (a) a dicarboxylic acid component comprising: i) 90 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues; ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: i) 90 to 100 mol % of 1,4-cyclohexanedimethanol residues, and ii) 0 to 10 mol% of modifying diol residues; and Having an inherent viscosity of about 0.5 to about 1.2 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
4. The film of claim 1, wherein the polymer component (B) comprises a copolyester comprising: A polyester portion and a polyether portion, wherein: The polyester portion comprises residues of an aliphatic diol and an aliphatic dicarboxylic acid or an aliphatic dicarboxylic acid ester, and The polyether portion comprises a polyalkylene glycol; and wherein the copolyester ether has an inherent viscosity of about 0.6 to about 1.5 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
5. The film according to claim 4, wherein The polymer component (B) includes a copolyester including a dicarboxylic acid component including residues of 1,4-cyclohexanedicarboxylate and a diol component including residues of 1,4-cyclohexanedimethanol and poly(tetramethylene ether) glycol.
6. The film according to claim 5, wherein The polymer component (B) comprises a copolyester comprising: (a) a dicarboxylic acid component comprising: i) 90 to 100 mol % of 1,4-cyclohexanedicarboxylic acid residues; ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: i) 95 to 80 mol % of 1,4-cyclohexanedimethanol residues, and ii) 5 to 20 mol% of poly(tetramethylene ether) glycol residues; and Having an inherent viscosity of about 0.9 to about 1.4 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
7. The film according to claim 6, wherein The copolyester of polymer component (B) has an inherent viscosity of about 1.02 to about 1.
26.
8. The film according to any one of claims 1 to 7, wherein The polymer component (A) is a polyester comprising: (a) a dicarboxylic acid component comprising: i) 90 to 100 mol % of terephthalic acid residues; ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: i) 10 to 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues; ii) 60 to 90 mol% of 1,4-cyclohexanedimethanol residues; and Having an inherent viscosity of about 0.5 to about 0.9 dL / g, or about 0.6 and 0.8 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
9. The film according to any one of claims 1 to 7, wherein The polymer component (A) is a polyester comprising: (a) a dicarboxylic acid component comprising: i) 90 to 100 mol % of terephthalic acid residues; ii) 0 to 10 mol % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: i) 10 to 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues; ii) 60 to 90 mol% of ethylene glycol residues; and Having an inherent viscosity of about 0.4 to about 0.9 dL / g, or about 0.5 and 0.7 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.
10. The film according to any one of claims 1 to 9, wherein The total thickness of the membrane is from about 100 μM to about 3000 μM, or from about 300 μM to about 3000 μM, or from about 380 μM to about 1600 μM, or from about 500 μM to about 1000 μM.
11. The film according to any one of claims 1 to 10, wherein The film has an average tear force of at least 10 N on a film having a thickness of 0.7 to 0.8 mm, measured according to ASTM D1938, and a force retention of 70% or less on a film having a thickness of 0.7 to 0.8 mm, measured as described in the specification.
12. The film according to any one of claims 1 to 11, wherein The film has a tear force in the range of 20N to 100N on a film having a thickness of 0.7 to 0.8 mm, measured according to ASTM D1938, and a force retention in the range of 10% to 80% or 10% to 40% on a film having a thickness of 0.7 to 0.8 mm, measured as described in the specification.
13. The film according to any one of claims 1 to 12, wherein The film has a flexural modulus below 2100 MPa, measured according to ASTM D 790.
14. The film according to any one of claims 1 to 13, wherein The films have a flexural modulus in the range of greater than 500 MPa to 2100 MPa, measured according to ASTM D 790.
15. The membrane according to any one of claims 1 to 14, wherein The polymer component (A) is present in an amount of 50 to 70 wt%, and the polymer component (B) is present in an amount of 30 to 50 wt%.
16. The film according to claim 15, wherein The polymer component (A) is present in an amount of greater than 50 to 70 wt%, and the polymer component (B) is present in an amount of 30 to less than 50 wt%.
17. A removable orthodontic tooth positioning appliance having a tooth receiving cavity shaped to directly receive at least a portion of a patient's teeth, the appliance comprising a film according to any one of claims 1 to 16.