Pipe comprising polypropylene composition

By introducing copolymers of specific comonomer units into polypropylene compositions and utilizing a multi-stage process with a single-point catalyst system, the balance between stiffness and impact performance of polypropylene copolymers in high-pressure pipelines was solved, achieving high impact performance under low-temperature conditions.

CN118900885AActive Publication Date: 2024-11-05北欧化工公司
View PDF 45 Cites 0 Cited by

Patent Information

Application Number
CN202380029204.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-04
Filing Date
2023-04-03
Publication Date
2024-11-05
Estimated Expiration
2043-04-03

AI Technical Summary

Technical Problem

Existing polypropylene copolymers are difficult to improve impact performance while maintaining good rigidity and pressure resistance in high-pressure pipeline applications, especially due to insufficient impact resistance under low-temperature conditions.

Method used

Polypropylene compositions are prepared by polymerization of copolymers containing propylene and comonomer units derived from 1-butene or 1-hexene, and copolymers containing ethylene and comonomer units derived from 1-butene and/or 1-hexene, in a multi-stage process using a single-point catalyst system. Parameters such as comonomer content and melt flow rate are optimized to improve impact performance.

Benefits of technology

Without compromising pressure resistance, the impact resistance of the pipeline is significantly improved, while maintaining appropriate stiffness to meet the requirements of high-pressure pipeline use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900885A_ABST
    Figure CN118900885A_ABST
Patent Text Reader

Abstract

The present invention relates to a pipe comprising a polypropylene composition comprising a copolymer of propylene with comonomer units derived from 1-butene or 1-hexene and a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene, a process for the manufacture of said pipe and the use of said polypropylene composition for the manufacture of pipes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a pipe comprising a polypropylene composition comprising a copolymer of propylene with comonomer units derived from 1-butene or 1-hexene and a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene, a method for producing the pipe and the use of the polypropylene composition for producing the pipe. Background Art

[0002] Polypropylene materials are commonly used in various piping applications, such as fluid transportation, where the fluid is pressurized and / or heated during transportation. In particular, polypropylene materials are suitable for plumbing and heating applications, such as in-house hot and cold water pressure pipes and fittings, floor and wall heating systems, and radiator connections.

[0003] In this regard, propylene copolymers are particularly suitable for pressure pipe applications in hot water and industrial pipes, since propylene copolymers have good impact properties, stiffness, creep resistance, slow cracking properties and long-term pressure resistance.

[0004] It is well known that increasing impact properties has an adverse effect on stiffness and vice versa. However, for high-pressure pipes, a good balance must be achieved between impact properties and stiffness to ensure sufficient pressure resistance to the internal pressure. In addition, propylene copolymer materials are required to have good processing properties to facilitate pipe extrusion and pipe injection molding. In order to increase the stiffness of propylene copolymer materials to the required level, the comonomer content in the polymer can be reduced, but doing so will have a negative impact on the toughness of the material. In particular, the impact resistance of propylene copolymer grades used for hot and cold water applications is often unsatisfactory, especially under low temperature conditions.

[0005] EP 3 567 061 A1 discloses a polypropylene composition comprising a single-site catalyzed propylene-1-hexene random copolymer suitable for pressure pipe applications. These pipes exhibit a good balance of properties in terms of stiffness and pressure resistance, but have a rather low impact strength.

[0006] Therefore, there is a need in the art to improve the impact properties of propylene copolymer materials without sacrificing stiffness and compression resistance.

[0007] The present invention is based on the following discovery to achieve excellent pipe performance: a polypropylene composition comprising a copolymer of propylene with comonomer units derived from 1-butene or 1-hexene, the copolymer being polymerized under a single site catalyst system, and a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene. Summary of the invention

[0008] The present invention relates to a pipe comprising a polypropylene composition, wherein the polypropylene composition comprises

[0009] (A) a copolymer of 70 to 95 wt.-%, based on the total weight of the polypropylene composition, of propylene and comonomer units derived from 1-butene or 1-hexene, said copolymer having:

[0010] 0.5 to 5.0 wt.-% total comonomer content;

[0011] a melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 230° C. of 0.10 to 2.0 g / 10 min; and

[0012] · a ratio of weight average molecular weight to number average molecular weight, Mw / Mn, as measured by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99 of 2.5 to 6.0; and

[0013] (B) 5 to 30 wt.-%, based on the total weight of the polypropylene composition, of a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene, said copolymer having:

[0014] 1.0 to 25.0 wt.-% total comonomer content;

[0015] 910.0 to 940.0 kg / m 3 The density measured in accordance with ISO 1183; and

[0016] a melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 190° C. of 0.05 to 3.0 g / 10 min;

[0017] The polypropylene composition has a melt flow rate MFR2 of 0.1 to 1.0 g / 10 min, measured at a load of 2.16 kg and a temperature of 230° C. according to ISO 1133.

[0018] Furthermore, the present invention relates to a method for manufacturing the above or following pipeline, comprising the following steps:

[0019] a) polymerizing propylene and 1-butene or 1-hexene in a multistage process in the presence of a single-site catalyst system to obtain a copolymer (A) of propylene and comonomer units derived from 1-butene or 1-hexene;

[0020] b) blending the propylene copolymer (A) with a copolymer (B) of ethylene and comonomer units derived from 1-butene and / or 1-hexene to obtain a polypropylene composition; and

[0021] c) manufacturing a pipe from the polypropylene composition.

[0022] Furthermore, the present invention relates to the use of a polypropylene composition for the manufacture of a pipe, wherein the polypropylene composition has a melt flow rate MFR2 of 0.1-1.0 g / 10 min measured at a load of 2.16 kg and a temperature of 230° C. according to ISO 1133 and comprises

[0023] (A) a copolymer of 70 to 95 wt.-%, based on the total weight of the polypropylene composition, of propylene and comonomer units derived from 1-butene or 1-hexene, said copolymer having:

[0024] 0.5 to 5.0 wt.-% total comonomer content;

[0025] a melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 230° C. of 0.10 to 2.0 g / 10 min; and

[0026] · a ratio of weight average molecular weight to number average molecular weight, Mw / Mn, as measured by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99 of 2.5 to 6.0; and

[0027] (B) 5 to 30 wt.-%, based on the total weight of the polypropylene composition, of a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene, said copolymer having:

[0028] 1.0 to 25.0 wt.-% total comonomer content;

[0029] 910.0 to 940.0 kg / m 3 The density measured in accordance with ISO 1183; and

[0030] • A melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 190° C. of 0.05 to 3.0 g / 10 min.

[0031] As can be seen from the Charpy notched impact test and the pipe impact test, the addition of 5 to 30 wt.-% of the above or below mentioned ethylene copolymer (B) to the polypropylene composition surprisingly improves the impact properties of the produced pipe without impairing the pressure resistance in the pressure test. The stiffness is still acceptable, as can be seen from the slightly lower but acceptable flexural modulus.

[0032] definition

[0033] The random propylene copolymer is a copolymer of propylene monomer units and comonomer units (in the present invention, 1-butene or 1-hexene comonomer units), wherein the comonomer units are randomly distributed on the polypropylene chain. Therefore, based on the total amount of the random propylene copolymer, the random propylene copolymer contains at least 90 wt%, more preferably at least 95 wt%, and still more preferably at least 96 wt% of a xylene-insoluble fraction (xylene cold insoluble (XCI) fraction). Therefore, the random propylene copolymer does not contain an elastic polymer phase dispersed therein.

[0034] Propylene homopolymers are polymers consisting mainly of propylene monomer units. Due to the presence of impurities, especially in commercial polymerization processes, propylene homopolymers may contain up to 0.1 mol-% of monomer units, preferably up to 0.05 mol-% of monomer units, most preferably up to 0.01 mol-% of monomer units.

[0035] "Ethylene homopolymer" refers to a polymer mainly composed of ethylene monomer units. Due to the requirements of large-scale polymerization, ethylene homopolymers may contain a small amount of comonomer units, usually less than 0.1 mol% of ethylene homopolymer, preferably less than 0.05 mol% and most preferably less than 0.01 mol%.

[0036] If a polymer is derived from ethylene monomer units and at least one α-olefin comonomer unit, the polymer is called an "ethylene copolymer". The α-olefin comonomer units are selected from 1-butene and / or 1-hexene. Polymers having ethylene monomer units and comonomer units derived from 1-butene and 1-hexene are called "ethylene terpolymers".

[0037] Ethylene polymers are usually classified according to density, such as low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE) and high density polyethylene (HDPE). In the literature, the density of ethylene polymers prepared in the presence of polymerization catalysts is 910 to 945 kg / m 3 Polyethylene is usually classified as linear low-density polyethylene (LLDPE) or medium-density polyethylene (MDPE).

[0038] A polymer comprising more than one fraction differing in at least one property, such as weight average molecular weight or comonomer content, is referred to as "multimodal". A multimodal polymer is referred to as "bimodal" if it comprises two different fractions, and accordingly, as "trimodal" if it comprises three different fractions. The form of the molecular weight distribution curve of such a multimodal polymer (i.e., the shape of a plot of the polymer weight fractions as a function of their molecular weight) will show more than two maxima, or at least be significantly broadened compared to the curves for the individual fractions, depending on the mode.

[0039] In contrast to "multimodal", unimodal polymers show only one maximum in a plot of polymer weight fraction as a function of its molecular weight and have a uniform distribution of comonomers.

[0040] In the following, unless otherwise stated, the contents are expressed as weight percent (wt.-%). DETAILED DESCRIPTION

[0041] In a first aspect, the present invention relates to a pipe comprising a polypropylene composition, wherein the polypropylene composition comprises

[0042] (A) a copolymer of 70 to 95 wt.-%, based on the total weight of the polypropylene composition, of propylene and comonomer units derived from 1-butene or 1-hexene, said copolymer having:

[0043] 0.5 to 5.0 wt.-% total comonomer content;

[0044] a melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 230° C. of 0.10 to 2.0 g / 10 min; and

[0045] · a ratio of weight average molecular weight to number average molecular weight, Mw / Mn, as measured by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99 of 2.5 to 6.0; and

[0046] (B) 5 to 30 wt.-%, based on the total weight of the polypropylene composition, of a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene, said copolymer having:

[0047] 1.0 to 25.0 wt.-% total comonomer content;

[0048] 910.0 to 940.0 kg / m 3 The density measured in accordance with ISO 1183; and

[0049] a melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 190° C. of 0.05 to 3.0 g / 10 min;

[0050] The polypropylene composition has a melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 230° C. of 0.1 to 1.0 g / 10 min.

[0051] The pipe has an improved balance among rigidity, impact performance and pressure resistance.

[0052] According to ISO 1167-1 and ISO 1167-2, the pipe pressure test stability of the pipe measured at a temperature of 95°C and a hoop stress of 4.6 MPa is preferably at least 5000 hours, more preferably at least 5750 hours.

[0053] The upper limit is usually not more than 15,000 hours, preferably not more than 12,500 hours.

[0054] Further, according to ISO 1167-1 and ISO 1167-2, the pipe pressure test stability of the pipe measured at a temperature of 20° C. and a hoop stress of 16 MPa is preferably at least 5 hours, more preferably at least 10 hours.

[0055] Further, the pipe preferably does not break in a pipe impact test at 0°C according to ISO 9854-2.

[0056] The pipe thus qualifies as a pressure pipe, preferably a pressure pipe for hot and cold water.

[0057] The content of the polypropylene composition in the pipe is preferably 90 to 100 wt.-%, more preferably 95 to 100 wt.-%, based on the total weight of the pipe. In a preferred embodiment, the pipe consists of the polypropylene composition.

[0058] The polypropylene composition comprises a propylene copolymer (A) and an ethylene copolymer (B).

[0059] Further, the polypropylene composition may comprise other polymer components different from the propylene copolymer (A) and the ethylene copolymer (B). The content of said other polymer components is typically 0 to 10 wt.-%, preferably 0 to 5 wt.-%.

[0060] Preferably the propylene copolymer (A) and the ethylene copolymer (B) are the only polymer components of the polypropylene composition.

[0061] Furthermore, the polypropylene composition may contain non-polymer components, such as additives. The additives include antioxidants, processing stabilizers, UV-stabilizers, pigments, fillers, antistatic additives, anti-blocking agents, nucleating agents and acid scavengers.

[0062] Suitable antioxidants and stabilizers are, for example, 2,6-di-tert-butyl-p-cresol, tetrakis-[methylene-3-(3',5-di-tert-butyl-4'-hydroxyphenyl)propionate]methane, octadecyl 3-3(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, dilauryl thiodipropionate, distearyl thiodipropionate, tris(nonylphenyl) phosphate, distearyl pentaerythritol diphosphite and tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphonate.

[0063] Some hindered phenols are sold under the trade names Irganox 1076 and Irganox 1010. Commercially available mixtures of antioxidants and processing stabilizers are also useful, such as Irganox B225 sold by Ciba-Geigy.

[0064] Suitable acid scavengers are, for example, metal stearates, such as calcium stearate and zinc stearate. They are used in amounts generally known in the art, typically 500 ppm to 10000 ppm, preferably 500 to 5000 ppm.

[0065] The polypropylene composition preferably has an amount of 4 to 25 wt.-%, more preferably 6 to 20 wt.-%, still more preferably 8 to 15 wt.-% of a polymer fraction, the polymer fraction being the polymer fraction eluting at a temperature of 31 to 80 °C excluding the purge fraction and having a logM between 4.5 and 6.0 as measured by cross fractionation chromatography (CFC).

[0066] Further, the characteristic profile of the polypropylene composition in a temperature rising elution fractionation (TREF) elution profile (obtained from cross fractionation chromatography (CFC)) comprises two peaks, wherein the first peak Tp(1) is preferably eluted between 45 and 90°C, more preferably between 50 and 80°C, still more preferably between 55 and 70°C, and the second peak Tp(2) is preferably eluted between 85 and 100°C, more preferably between 87 and 99°C, still more preferably between 90 and 98°C.

[0067] The polypropylene composition preferably has a xylene cold soluble (XCS) content measured according to ISO 16152 of 1.0 to 3.5 wt.-%, more preferably of 1.2 to 3.2 wt.-%, still more preferably of 1.5 to 3.0 wt.-%.

[0068] Further, the polypropylene composition preferably has a first melting temperature Tm1 measured according to ISO 11357 / part 3 of 135 to 145°C, more preferably of 137 to 142°C.

[0069] Further, the polypropylene composition preferably has a second melting temperature Tm2 measured according to ISO 11357 / part 3 of 115 to 130°C, more preferably of 117 to 125°C.

[0070] Tm1 is usually higher than Tm2.

[0071] Furthermore, the polypropylene composition preferably has a crystallization temperature Tc measured according to ISO 11357 / part 3 of 100 to 110 °C, more preferably of 102 to 107 °C.

[0072] Furthermore, the polypropylene composition preferably has a first melting enthalpy Hm1 measured according to ISO 11357 / part 3 of 30 to 45 J / g, more preferably of 32 to 42 J / g.

[0073] Further, the polypropylene composition preferably has a second melting enthalpy Hm2 measured according to ISO 11357 / part 3 of 35 to 50 J / g, more preferably of 37 to 47 J / g.

[0074] Hm1 is usually lower than Hm2.

[0075] The polypropylene composition exhibits high impact strength at acceptable stiffness.

[0076] The polypropylene composition preferably has a flexural modulus of 700 to 1000 MPa, more preferably 800 to 950 MPa, still more preferably 850 to 925 MPa, measured according to ISO 178 on injection moulded specimens prepared according to EN ISO 1872-2.

[0077] Furthermore, the Charpy notched impact strength of the polypropylene composition at 23°C is preferably 7.5 to 15.0 kJ / m 2 , more preferably 8.5 to 14.0 kJ / m 2 , still more preferably 9.5 to 13.0 kJ / m 2 .

[0078] Furthermore, the Charpy notched impact strength of the polypropylene composition at 0°C is preferably 2.5 to 5.0 kJ / m 2 , more preferably 3.0 to 4.5 kJ / m 2 , still more preferably 3.0 to 4.0 kJ / m 2 .

[0079] Furthermore, the Charpy notched impact strength of the polypropylene composition at -20°C is preferably 1.5 to 4.0 kJ / m 2 , more preferably 1.7 to 3.5 kJ / m 2 , still more preferably 1.8 to 3.0 kJ / m 2 .

[0080] The Charpy notched impact strength at 23° C., 0° C. and −20° C. was determined according to ISO 179 1eA on injection molded test specimens prepared according to EN ISO 1872-2.

[0081] The polypropylene composition comprises 70 to 95 wt.-% of the propylene copolymer (A), preferably 75 to 93 wt.-%, more preferably 80 to 90 wt.-%, based on the total weight of the polypropylene composition.

[0082] The propylene copolymer (A) is a copolymer of propylene with comonomer units derived from 1-butene or 1-hexene. Preferably, the propylene copolymer (A) is a copolymer of propylene with comonomer units derived from 1-hexene.

[0083] "Copolymer of propylene with comonomer units derived from 1-butene" means that the propylene copolymer (A) comprises units derived from propylene and 1-butene only.

[0084] "Copolymer of propylene with comonomer units derived from 1-hexene" means that the propylene copolymer (A) comprises units derived from propylene and 1-hexene only.

[0085] The total monomer content of propylene copolymer (A), i.e. the content of monomer units derived from 1-butene or 1-hexene, based on the total weight of propylene copolymer (A) is from 0.5 to 5.0 wt.-%, more preferably from 1.0 to 4.0 wt.-%, still more preferably from 2.0 to 3.0 wt.-%.

[0086] The comonomer units are preferably randomly distributed in the polymer chain of the propylene copolymer (A). Thus, the propylene copolymer (A) is preferably a propylene random copolymer.

[0087] Further, the propylene copolymer (A) has a melt flow rate MFR2 measured according to ISO 1133 under a load of 2.16 kg and a temperature of 230° C. of 0.10 to 2.0 g / 10 min, preferably 0.15 to 1.5 g / 10 min, more preferably 0.20 to 1.0 g / 10 min.

[0088] Furthermore, the propylene copolymer (A) has a ratio Mw / Mn of weight average molecular weight to number average molecular weight as measured by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99 of 2.5 to 6.0, preferably 3.0 to 5.5, still more preferably 3.5 to 5.0.

[0089] The propylene copolymer (A) preferably has a xylene cold soluble (XCS) content measured according to ISO 16152 of 0.2 to 2.5 wt.-%, more preferably of 0.5 to 2.3 wt.-%.

[0090] The propylene copolymer (A) preferably has a melting temperature Tm measured according to ISO 11357 / part 3 of 135 to 145 °C.

[0091] Further, the propylene copolymer (A) preferably has a crystallization temperature Tc measured according to ISO 11357 / part 3 of 100 to 105 °C.

[0092] Furthermore, the propylene copolymer (A) preferably has a melting enthalpy Hm measured according to ISO 11357 / part 3 of 70 to 80 J / g.

[0093] The propylene copolymer (A) is obtainable by polymerization in the presence of a single site catalyst system.

[0094] The catalyst system preferably comprises

[0095] (i) A catalyst having the following structure:

[0096]

[0097] In the formula,

[0098] M is zirconium or hafnium;

[0099] Each X is independently a σ-donor ligand

[0100] L is the formula -(ER 10 2) y -bridge;

[0101] y is 1 or 2;

[0102] E is C or Si;

[0103] Each R 10 Independently C1-C 20 Hydrocarbon, tri(C1-C 20 Alkyl) silyl, C6-C 20 Aryl, C7-C 20 Arylalkyl or C7-C 20alkylaryl, or L is an alkylene group, such as methylene or ethylene;

[0104] R 1 are independently the same or different from each other and are CH2-R 11 Group, where R 11 is H or a linear or branched C1-C6 alkyl, C3-C8 cycloalkyl, C6-C 10 Aryl;

[0105] R 3 , R 4 and R 5 are independently the same or different from each other and are H or a linear or branched C1-C6 alkyl, C7-C 20 Aralkyl, C7-C 20 Alkyl or C6-C 20 Aryl, provided that if there are four or more R 3 , R 4 and R 5 group, then R 3 , R 4 and R 5 at least one of is not tert-butyl;

[0106] R 7 and R 8 are independently the same or different from each other and are H, CH2-R 12 Group, where R 12 is H or a linear or branched C1-C6 alkyl, SiR 13 3.GeR 13 3. OR 13 , SR 13 NR 13 2,

[0107] Among them, R 13 It is a straight or branched C1-C6 alkyl, C7-C 20 Alkaryl and C7-C 20 Arylalkyl or C6-C 20 Aryl, R 9 are each independently the same or different from each other and are H or a linear or branched C1-C6 alkyl group; and

[0108] R 2 and R 6 are H; and

[0109] (ii) A cocatalyst system comprising an aluminoxane cocatalyst.

[0110] It is emphasized that in certain cases, it may not be necessary to use this co-catalyst system.

[0111] The catalyst system can be used in non-supported form or in solid form.The catalyst system of the present invention can be used as a homogeneous catalyst system or as a heterogeneous catalyst system.

[0112] The catalyst system in solid form is preferably a catalyst system in the form of solid particles, which can be supported on an external support material (such as silica or alumina), or in a particularly preferred embodiment, no external support is required, but still in solid form. For example, the solid catalyst system can be obtained by the following method, wherein

[0113] (a) forming a liquid / liquid emulsion system comprising a solution of catalyst components (i) and (ii) dispersed in a solvent to form dispersed droplets; and

[0114] (b) by solidifying the dispersed droplets to form solid particles.

[0115] Specific compounds of the present invention include:

[0116] Racemic-trans-dimethylsilanediyl[2-methyl-4-(4-tert-butylphenyl)-5,6,7-trihydro-s-inden-1-yl][2-methyl-4-(4-tert-butylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium,

[0117] Racemic-trans-dimethylsilanediyl[2-isobutyl-4-(4-tert-butylphenyl)-5,6,7-trihydro-s-inden-1-yl][2-methyl-4-(4-tert-butylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium,

[0118] Racemic-trans-dimethylsilanediyl[2-neopentyl-4-(4-tert-butylphenyl)-5,6,7-trihydro-s-inden-1-yl][2-methyl-4-(4-tert-butylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium,

[0119] Racemic-trans-dimethylsilanediyl[2-benzyl-4-(4-tert-butylphenyl)-5,6,7-trihydro-s-inden-1-yl][2-methyl-4-(4-tert-butylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium,

[0120] Racemic-trans-dimethylsilanediyl[2-cyclohexylmethyl-4-(4-tert-butylphenyl)-5,6,7-tri-s-indan-1-yl][2-methyl-4-(4-tert-butylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium,

[0121] Racemic e-trans-dimethylsilanediyl[2-methyl-4-(3,5-dimethylphenyl)-5,6,7-trihydro-s-inden-1-yl][2-methyl-4-(3,5-dimethylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium,

[0122] Racemic-trans-dimethylsilanediyl[2-isobutyl-4-(3,5-dimethylphenyl)-5,6,7-trihydro-s-inden-1-yl][2-methyl-4-(3,5-dimethylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium,

[0123] Racemic-trans-dimethylsilanediyl[2-neopentyl-4-(3,5-dimethylphenyl)-5,6,7-trihydro-s-inden-1-yl][2-methyl-4-(3,5-dimethylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium,

[0124] Racemic-trans-dimethylsilanediyl[2-benzyl-4-(3,5-dimethylphenyl)-5,6,7-trihydro-s-inden-1-yl][2-methyl-4-(3,5-dimethylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium, and

[0125] Racemic-trans dimethylsilanediyl[2-cyclohexylmethyl-4-(3,5-dimethylphenyl)-5,6,7-trihydro-s-inden-1-yl][2-methyl-4-(3,5-dimethylphenyl)-5-methoxy-6-tert-butylindenyl zirconium dichloride or dimethyl zirconium.

[0126] The above catalysts have been described in documents such as WO2015 / 011135, which are incorporated herein by reference. A particularly preferred catalyst is catalyst No. 3 of WO2015 / 011135. The preparation method of metallocene has been described in WO2013 / 007650, which is incorporated herein by reference. A particularly preferred method for preparing the catalyst complex is E2 in WO2013 / 007650.

[0127] For the avoidance of doubt, the above narrow definition of a substituent may be combined with any other broad or narrow definition of a substituent.

[0128] In the above disclosure, when a narrow definition of a substituent is given, that narrow definition is deemed to be disclosed together with all broad and narrow definitions of other substituents in this application.

[0129] The ligands required for forming the complex and the catalyst / catalyst system can be synthesized by any method, and a skilled organic chemist can design various synthesis schemes to make the necessary ligand materials. For example, WO2007 / 116034 discloses the necessary chemical methods. Synthesis schemes can also be generally found in WO2002 / 02576, WO2011 / 135004, WO2012 / 084961, WO2012 / 001052, WO2011 / 076780 and WO2015 / 158790. The examples section also provides sufficient guidance for the technician.

[0130] As noted above, a cocatalyst system is not always required. However, when used, the cocatalyst system comprises an aluminoxane cocatalyst.

[0131] The aluminoxane cocatalyst may be one of formula (X):

[0132]

[0133] In the formula, n is usually 6 to 20, and R has the following meanings.

[0134] Aluminoxanes are formed by partial hydrolysis of organoaluminum compounds, such as those of the general formula AlR3, AlR2Y, and Al2R3Y3, wherein R can be, for example, C1-C 10 Alkyl, preferably C1-C5 alkyl, or C3-C 10 Cycloalkyl, C7-C 12 -aralkyl or alkaryl and / or phenyl or naphthyl, and wherein Y can be hydrogen, halogen, preferably chlorine or bromine, or C1-C 10 The alkoxy group is preferably a methoxy group or an ethoxy group. The oxygen-containing aluminoxane obtained is usually not a pure compound but a mixture of oligomers of the formula (X).

[0135] The preferred aluminoxane is methylaluminoxane (MAO).Since the aluminoxanes used as cocatalysts in the present invention are not pure compounds due to the way they are prepared, the molar concentrations of the aluminoxane solutions hereinafter are based on their aluminum content.

[0136] The molar ratio of Al in the aluminoxane to the metal ion of the metallocene may be 1:1 to 2000:1 mol / mol, preferably 10:1 to 1000:1, and more preferably 50:1 to 500:1 mol / mol.

[0137] The co-catalyst system may additionally comprise a boron-containing co-catalyst.

[0138] Related boron-based co-catalysts include those of formula (Z)

[0139] BY3(Z)

[0140] Wherein, Y is independently the same or different and is a hydrogen atom, an alkyl group of 1 to about 20 carbon atoms, an aryl group of 6 to about 15 carbon atoms, an alkaryl group, an aralkyl group, a haloalkyl group or a haloaryl group, each of which contains 1 to 10 carbon atoms in the alkyl group and 6 to 20 carbon atoms in the aryl group, or fluorine, chlorine, bromine or iodine. Preferred embodiments of Y are methyl, propyl, isopropyl, isobutyl or trifluoromethyl, unsaturated groups, such as aryl or haloaryl groups, such as phenyl, tolyl, benzyl, p-fluorophenyl, 3,5-difluorophenyl, pentachlorophenyl, pentafluorophenyl, 3,4,5-trifluorophenyl and 3,5-bis(trifluoromethyl)phenyl. Preferred choices are trifluoroborane, triphenylborane, tri(4-fluorophenyl)borane, tri(3,5-difluorophenyl)borane, tri(4-fluoromethylphenyl)borane, tri(2,4,6-trifluorophenyl)borane, tri(pentafluorophenyl)borane, tri(tolyl)borane, tri(3,5-dimethylphenyl)borane, tri(3,5-difluorophenyl)borane and / or tri(3,4,5-trifluorophenyl)borane.

[0141] Tris(pentafluorophenyl)borane is particularly preferred.

[0142] Borates, i.e. compounds containing borate 3+ ions, can be used. Such ionic promoters preferably contain non-coordinating anions, such as tetrakis(pentafluorophenyl)borate and tetraphenylborate. Suitable counterions are protonated amines or aniline derivatives, such as methylammonium, aniline, dimethylammonium, diethylamine, N-methylaniline, diphenylamine, N,N-dimethylaniline, trimethylammonium, triethylammonium, tri-n-butylammonium, methyldiphenylammonium, pyridine, p-bromo-N,N-dimethylaniline or p-nitro-N,N-dimethylaniline.

[0143] Preferred ionic compounds that can be used in the present invention include: triethylammonium tetra(phenyl)borate, tributylammonium tetra(phenyl)borate, trimethylammonium tetra(tolyl)borate, tributylammonium tetra(tolyl)borate, tributylammonium tetra(pentafluorophenyl)borate, tripropylammonium tetra(dimethylphenyl)borate, tributylammonium tetra(trifluoromethylphenyl)borate, tributylammonium tetra(4-fluorophenyl)borate, N,N-dimethylcyclohexylammonium tetra(pentafluorophenyl)borate, N,N-dimethylbenzylammonium tetra(pentafluorophenyl)borate, N,N-dimethylanilinium tetra(phenyl)borate , N,N-diethylanilinium tetrakis(phenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-di(propyl)ammonium tetrakis(pentafluorophenyl)borate, di(cyclohexyl)ammonium tetrakis(pentafluorophenyl)borate, triphenylphosphonium tetrakis(phenyl)borate, triethylphosphonium tetrakis(phenyl)borate, diphenylphosphonium tetrakis(phenyl)borate, tri(methylphenyl)phosphonium tetrakis(phenyl)borate, tri(dimethylphenyl)phosphonium tetrakis(phenyl)borate, triphenylcarbonium tetrakis(pentafluorophenyl)borate, or ferrocenium tetrakis(pentafluorophenyl)borate.

[0144] Preferred are triphenylcarbonium tetrakis(pentafluorophenyl)borate, N,N-dimethylcyclohexylammonium tetrakis(pentafluorophenyl)borate, or N,N-dimethylbenzylammonium tetrakis(pentafluorophenyl)borate.

[0145] Suitable amounts of promoter are well known to the skilled person.

[0146] The molar ratio of boron to the metal ion of the metallocene may be 0.5:1 to 10:1 mol / mol, preferably 1:1 to 10:1, particularly preferably 1:1 to 5:1 mol / mol.

[0147] The catalyst can be used in supported or unsupported form. The particulate support material used is preferably an organic or inorganic material, for example silicon dioxide, aluminum oxide or zirconium oxide or a mixed oxide, for example silicon dioxide-alumina, in particular silicon dioxide, aluminum oxide or silicon dioxide-alumina. Preference is given to using a silicon dioxide support. The skilled person is aware of the procedures required for supporting the metallocene catalyst.

[0148] The carrier is particularly preferably a porous material so that the complex can be loaded into the pores of the carrier, for example using methods similar to those described in WO94 / 14856 (Mobil), WO95 / 12622 (Borealis) and WO2006 / 097497. The particle size is not critical, but is preferably in the range of 5 to 200 μm, more preferably 20 to 80 μm. The use of these carriers is conventional in the art.

[0149] In an alternative embodiment, no support is used. Such catalyst systems can be prepared in solution, for example, in an aromatic solvent (e.g., toluene) by contacting the metallocene (solid or in solution) with a cocatalyst (e.g., methylaluminoxane previously dissolved in an aromatic solvent), or by sequentially adding the dissolved catalyst components to the polymerization medium.

[0150] In a particularly preferred embodiment, no external support is used, but the catalyst is still present in solid particulate form. Thus, no external support material such as an inert organic or inorganic support (such as the above-mentioned silica) is used.

[0151] In order to provide the catalyst in the present invention in a solid form without using an external carrier, it is preferred to use a liquid / liquid emulsion system. The method comprises forming a dispersed catalyst component (i) and (ii) in a solvent and forming solid particles by solidifying the dispersed droplets.

[0152] In particular, the method comprises preparing a solution of one or more catalyst components; dispersing the solution in a solvent to form an emulsion, wherein the one or more catalyst components are present in droplets of a dispersed phase; immobilizing the catalyst components in the dispersed droplets in the absence of an external particulate porous support to form solid particles comprising the catalyst, and optionally recovering the particles.

[0153] The method is capable of producing active catalyst particles with improved morphology, such as having a predetermined spherical shape, surface characteristics and particle size, and without using any additional external porous support material, such as an inorganic oxide (e.g., silica). The term "preparing a solution of more than one catalyst component" means that the catalyst-forming compounds can be mixed with one solution dispersed in an immiscible solvent, or at least two separate catalyst solutions can be prepared for each part of the catalyst-forming compound and then dispersed in the solvent in sequence.

[0154] In a preferred method of forming the catalyst, at least two separate solutions may be prepared for each or a portion of the catalyst and then dispersed sequentially into immiscible solvents.

[0155] More preferably, the complex solution comprising the transition metal compound and the co-catalyst is mixed with a solvent to form an emulsion, wherein the inert solvent forms a continuous liquid phase and the solution comprising the catalyst component forms a dispersed phase (discontinuous phase) in the form of dispersed droplets. The droplets are then solidified to form solid catalyst particles, which are separated from the liquid and optionally washed and / or dried. The solvent forming the continuous phase may be immiscible with the catalyst solution at least under the conditions (e.g., temperature) in the dispersion step.

[0156] The term "immiscible with the catalyst solution" means that the solvent (continuous phase) is completely immiscible or partially immiscible, ie, not completely miscible, with the dispersed phase solution.

[0157] Preferably, the solvent is inert with respect to the compounds of the catalyst system to be prepared. WO 03 / 051934 fully discloses the necessary process.

[0158] The inert solvent must be chemically inert at least under the conditions (e.g. temperature) of the dispersing step. Preferably, the solvent of the continuous phase does not contain any significant amount of the catalyst-forming compound dissolved therein. Thus, solid particles of the catalyst are formed in droplets of the compound from the dispersed phase (i.e. provided to the emulsion in the form of a solution dispersed in the continuous phase).

[0159] "Immobilisation" and "solidification" are used interchangeably herein for the same purpose, namely for forming free-flowing solid catalyst particles in the absence of an external porous particle support such as silica. Thus, solidification occurs within the droplets. The step may be achieved in various ways as disclosed in WO03 / 051934. Preferably, solidification is caused by an external stimulus to the emulsion system, such as a change in temperature. Thus, during the step, the catalyst components remain "fixed" in the solid particles formed. More than one catalyst component may also participate in the solidification / immobilization reaction.

[0160] Therefore, solid particles having a uniform composition and a predetermined particle size range can be obtained.

[0161] Furthermore, the particle size of the catalyst particles of the present invention can be controlled by the size of the droplets in the solution, thereby obtaining spherical particles with uniform particle size distribution.

[0162] The method is also industrially advantageous because it enables the preparation of solid particles to be carried out in a one-pot procedure. The catalyst can also be prepared using a continuous or semi-continuous process.

[0163] The polypropylene composition comprises 5 to 30 wt.-% of ethylene copolymer (B), preferably 7 to 25 wt.-%, more preferably 10 to 20 wt.-%, based on the total weight of the polypropylene composition.

[0164] The ethylene copolymer (B) is a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene. Preferably, the ethylene copolymer (B) is a terpolymer of ethylene with comonomer units derived from 1-butene and 1-hexene.

[0165] The term "copolymer of ethylene and comonomer units derived from 1-butene" means that the ethylene copolymer (B) comprises units derived from ethylene and 1-butene only.

[0166] The term "copolymer of ethylene and comonomer units derived from 1-hexene" means that the ethylene copolymer (B) comprises units derived from ethylene and 1-hexene only.

[0167] The term "ethylene terpolymer of ethylene with comonomer units derived from 1-butene and 1-hexene" means that the ethylene copolymer (B) comprises units derived from ethylene, 1-butene and 1-hexene only.

[0168] The total comonomer content of the ethylene copolymer (B), ie the content of comonomer units derived from 1-butene and / or 1-hexene, is from 1.0 to 25.0 wt.-%, preferably from 1.5 to 22.5 wt.-%, still more preferably from 2.0 to 20.0 wt.-%.

[0169] The 1-butene content of the ethylene copolymer (B) is preferably from 0.1 to 5.0 wt.-%, more preferably from 0.2 to 3.5 wt.-%, still more preferably from 0.3 to 2.0 wt.-%, based on the total weight of the ethylene copolymer (B).

[0170] The 1-hexene content of the ethylene copolymer (B) is preferably 5.0 to 25.0 wt.-%, more preferably 6.0 to 22.5 wt.-%, still more preferably 7.5 to 20.0 wt.-%, based on the total weight of the ethylene copolymer (B).

[0171] The comonomer distribution of the ethylene copolymer (B) may be monomodal. This means that the comonomer units derived from 1-butene and / or 1-hexene are uniformly distributed in the ethylene copolymer (B).

[0172] The ethylene copolymer (B) may be multimodal with respect to the comonomer distribution.

[0173] This means that the ethylene copolymer (B) comprises different components.

[0174] When being a copolymer of ethylene and a comonomer unit derived from 1-butene or 1-hexene, in one embodiment, the ethylene copolymer (B) may comprise an ethylene homopolymer component and a copolymer of ethylene and 1-butene or 1-hexene component.

[0175] When being a copolymer of ethylene and comonomer units derived from 1-butene or 1-hexene, in another embodiment, the ethylene copolymer (B) may comprise two copolymers of ethylene and 1-butene or 1-hexene components having two different comonomer contents.

[0176] When being a terpolymer of ethylene and comonomer units derived from 1-butene and 1-hexene, in one embodiment, the ethylene copolymer (B) may comprise an ethylene homopolymer component, a copolymer component of ethylene and 1-butene, and a copolymer component of ethylene and 1-hexene.

[0177] When being a terpolymer of ethylene with comonomer units derived from 1-butene and 1-hexene, in another embodiment, the ethylene copolymer (B) may comprise a terpolymer of an ethylene homopolymer component and ethylene, 1-butene and 1-hexene components.

[0178] When being a terpolymer of ethylene and comonomer units derived from 1-butene and 1-hexene, in yet another embodiment, the ethylene copolymer (B) may comprise a copolymer of ethylene with a 1-butene component and a copolymer of ethylene with a 1-hexene component.

[0179] In a preferred embodiment, the ethylene copolymer (B) is a terpolymer of ethylene and comonomer units selected from 1-butene and 1-hexene, and has a 1-butene content of 0.1-5.0 wt.-%, preferably 0.2 to 3.5 wt.-%, and more preferably 0.3 to 2.0 wt.-%, based on the total weight of the ethylene copolymer (B). The 1-hexene content is 5.0 to 24.9 wt.-%, more preferably 6.0 to 22.3 wt.-%, and more preferably 7.5 to 19.7 wt.-%.

[0180] The density of the ethylene copolymer (B) measured according to ISO 1183 is 910.0 to 940.0 kg / m 3 , preferably 912.0 to 938.0 kg / m 3 , and more preferably 0.15 to 935 kg / m 3 .

[0181] The ethylene copolymer (B) is preferably a linear low density polyethylene (LLDPE).

[0182] The ethylene copolymer (B) has a melt flow rate MFR2 measured according to ISO 1133 under a load of 2.16 kg and a temperature of 190° C. of 0.05 to 3.0 g / 10 min, preferably 0.10 to 2.5 g / 10 min, more preferably 0.50 to 2.0 g / 10 min.

[0183] The ethylene copolymer (B) preferably has an intrinsic viscosity iV, measured to DIN ISO 1628 / 1, October 1999 (in decalin at 135° C.), of 1.5 to 2.5 dl / g, more preferably 1.7 to 2.2 dl / g.

[0184] Further, the ethylene copolymer (B) preferably has a ratio of weight average molecular weight to number average molecular weight Mw / Mn measured by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99 of 2.0 to 5.0, preferably 2.5 to 4.5, more preferably 3.0 to 4.0.

[0185] The ethylene copolymer (B) is preferably obtained by polymerization in the presence of a single site catalyst system. The single site catalyst system preferably comprises a catalytically active metallocene compound or complex in combination with a cocatalyst. The metallocene compound or complex is also referred to herein as an organometallic compound (C).

[0186] The organometallic compound (C) comprises a transition metal (M) from Groups 3 to 10 of the Periodic Table of Elements (IUPAC 2007) or from the actinides or lanthanides.

[0187] The term "organometallic compound (C)" in the present invention includes any metallocene compound of a transition metal, which carries at least one organic (coordinating) ligand and exhibits catalytic activity alone or together with a cocatalyst. Transition metal compounds are well known in the art and preferably include metal compounds of Groups 3 to 10, such as Groups 3 to 7 or Groups 3 to 6, such as Groups 4 to 6 of the Periodic Table (IUPAC 2007), as well as lanthanides or actinides.

[0188] In one embodiment, the organometallic compound (C) has the following formula (I):

[0189] (L)mRnMXq(I)

[0190] In the formula,

[0191] "M" is a transition metal (M) of Groups 3 to 10 of the Periodic Table of Elements (IUPAC 2007),

[0192] Each "X" is independently a monoanionic ligand, such as an o-ligand,

[0193] Each "L" is independently an organic ligand coordinated to the transition metal "M",

[0194] "R" is a bridging group connecting the organic ligand (L),

[0195] "m" is 1, 2 or 3, preferably 2,

[0196] "n" is 0, 1 or 2, preferably 1,

[0197] "q" is 1, 2 or 3, preferably 2, and

[0198] m+q equals the valence of the transition metal (M).

[0199] “M” is preferably selected from zirconium (Zr), hafnium (Hf) or titanium (Ti), and more preferably selected from zirconium (Zr) and hafnium (Hf).

[0200] "X" is preferably halogen, most preferably Cl.

[0201] Most preferably, the organometallic compound (C) is a metallocene complex comprising a transition metal compound as defined above, which comprises a cyclopentadienyl, indenyl or fluorenyl ligand as a substituent "L". Further, the ligand "L" may have a substituent, such as an alkyl, aryl, aralkyl, alkaryl, silyl, siloxy, alkoxy or other heteroatom groups, etc. Suitable metallocene catalysts are known in the art and are disclosed in WO-A-95 / 12622, WO-A-96 / 32423, WO-A-97 / 28170, WO-A-98 / 32776, WO-A-99 / 61489, WO-A-03 / 010208, WO-A-03 / 051934, WO-A-03 / 051514, WO-A-2004 / 085499, EP-A-1752462 and EP-A-1739103.

[0202] Most preferably, the metallocene catalyst (meaning the catalytically active metallocene complex as defined above) is used together with a cocatalyst (also referred to as an activator). Suitable activators are metal alkyl compounds known in the art, especially alkylaluminum compounds. Particularly suitable activators for use with metallocene catalysts are alkylaluminum oxide compounds, such as methylaluminoxane (MAO), tetraisobutylaluminoxane (TIBAO) or hexaisobutylaluminoxane (HIBAO).

[0203] method

[0204] In another aspect, the present invention relates to a method for manufacturing the above or following pipeline, comprising the following steps

[0205] a) polymerizing propylene and 1-butene or 1-hexene in a multistage process in the presence of a single-site catalyst system to obtain a copolymer (A) of propylene and comonomer units derived from 1-butene or 1-hexene;

[0206] b) blending the propylene copolymer (A) with a copolymer (B) of ethylene and comonomer units derived from 1-butene and / or 1-hexene to obtain a polypropylene composition; and

[0207] c) manufacturing a pipe from the polypropylene composition.

[0208] The propylene copolymer (A) is preferably polymerized under the above-mentioned single-site catalyst system.

[0209] The propylene copolymer (A) is preferably polymerized in a multistage process, which is a sequential polymerization process having at least two polymerization reactors connected in series.

[0210] The multi-stage process preferably comprises the following steps:

[0211] (i) introducing a stream of propylene and 1-butene or 1-hexene (preferably 1-hexene) into a first reactor such that the ratio of the feed rate of 1-butene or 1-hexene (preferably 1-hexene) to the feed rate of propylene is 2.0 to 4.0 mol / kmol; further introducing a stream of a catalyst system into the first reactor,

[0212] (ii) extracting a product stream comprising the first intermediate (PP1) from the first reactor

[0213] (iii) transferring the first intermediate (PP1) to a second reactor and further polymerizing the first intermediate in the presence of hydrogen by further adding propylene, 1-butene or 1-hexene (preferably 1-hexene) in the second reactor, such that

[0214] The ratio of hydrogen concentration to propylene concentration is in the range of 0.1 to 0.8 mol / kmol; and further

[0215] The concentration of 1-butene or 1-hexene (preferably 1-hexene) relative to the concentration of propylene is in the range of 3.0 to 6.0 mol / kmol

[0216] (iv) producing a powder of the propylene copolymer (A).

[0217] About overall process, propylene composition is prepared in a continuous polymerization process, and this process comprises at least two polymerization zones that operate under different conditions to prepare propylene composition.Polymerization zone can be operated under slurry, solution or gas phase conditions or their combination.Suitable process is disclosed in WO-A-98 / 58976, EP-A-887380 and WO-A-98 / 58977.

[0218] The catalyst may be transferred to the polymerization zone by any means known in the art. Thus, the catalyst may be suspended in a diluent and maintained as a homogeneous slurry. It is particularly preferred to use an oil having a viscosity of 20 to 1500 mPa·s as disclosed in WO-A-2006 / 063771 as a diluent. The catalyst may also be mixed with a viscous mixture of grease and oil and the resulting paste introduced into the polymerization zone. Furthermore, the catalyst may be allowed to settle and part of the catalyst slurry thus obtained may be introduced into the polymerization zone in a manner such as disclosed in EP-A-428054.

[0219] Gas phase polymerization can be carried out in a fluidized bed reactor, a fast fluidized bed reactor or a settled bed reactor or any combination of these reactors. When a combination of reactors is used, the polymer is transferred from one polymerization reactor to another. In addition, part or all of the polymer from a polymerization stage can be returned to the previous polymerization stage.

[0220] In a preferred embodiment, the prepolymerization is carried out continuously in liquid propylene as a bulk slurry polymerization, i.e. the liquid phase mainly comprises propylene with small amounts of other reactants and optional inert components dissolved therein. The prepolymerization is preferably carried out in a continuous stirred tank reactor or a loop reactor.

[0221] The prepolymerization reaction is usually carried out at a temperature of 0 to 40°C, preferably 10 to 30°C, more preferably 15 to 25°C.

[0222] The pressure in the prepolymerisation reactor is not critical but must be high enough to keep the reaction mixture in the liquid phase. Thus, the pressure may be from 20 to 100 bar, for example from 30 to 70 bar.

[0223] The reaction conditions are well known in the art, for example those disclosed in GB 1580635.

[0224] In the prepolymerization step, comonomers may also be added to the prepolymerization stage.

[0225] On average, the amount of prepolymer on the catalyst is preferably from 10 to 1000 g per gram of solid catalyst component, more preferably from 50 to 500 g per gram of solid catalyst component.

[0226] As known to those skilled in the art, the catalyst particles recovered from the continuous stirring prepolymerization reactor do not all contain the same amount of prepolymer. On the contrary, each particle has its own characteristic amount, which depends on the residence time of the particle in the prepolymerization reactor. Because some particles stay in the reactor for a relatively long time, and some stay for a relatively short time, the amount of prepolymer on different particles is also different, and some individual particles may contain the amount of prepolymer exceeding the above range. However, the average amount of prepolymer on the catalyst is preferably within the above range. The amount of prepolymer is known in the art, for example disclosed in GB 1580635.

[0227] Other components may also be added to the prepolymerization stage. Thus, as is known in the art, hydrogen may be added to the prepolymerization stage to control the molecular weight of the prepolymer. In addition, as disclosed in WO-A-00 / 66640, antistatic additives may be used to prevent particles from adhering to each other or to the reactor walls.

[0228] The polymerization in the first polymerization zone may be carried out in a slurry. The polymer particles formed in the polymerization are then suspended in a fluid hydrocarbon together with the catalyst fragmented and dispersed in the particles. The slurry is stirred to transfer the reactants from the fluid to the particles.

[0229] Slurry polymerization is preferably a so-called bulk polymerization. "Bulk polymerization" refers to a process in which polymerization is carried out in liquid monomers in the substantial absence of an inert diluent. However, as is known to those skilled in the art, monomers used for commercial production are never pure but always contain aliphatic hydrocarbons as impurities. For example, propylene monomer may contain up to 5% of propane impurities. Since propylene is consumed in the reaction and also recycled from the reaction effluent back to the polymerization reaction, inert components tend to accumulate and the reaction medium may therefore contain up to 40 wt-% of other compounds besides the monomers. However, it should be understood that such a polymerization process is still within the meaning of "bulk polymerization" as defined above.

[0230] The temperature in the slurry polymerization is generally 50 to 110° C., preferably 60 to 100° C., particularly preferably 65 to 95° C. The pressure is 1 to 150 bar, preferably 10 to 100 bar. In some cases, it is preferred to polymerize at a temperature higher than the critical temperature of the fluid mixture constituting the reaction phase and a pressure higher than the critical pressure of the fluid mixture. Such reaction conditions are generally referred to as "supercritical conditions". "Supercritical fluid" is used to represent a fluid or fluid mixture whose temperature and pressure exceed the critical temperature and pressure.

[0231] The slurry polymerization can be carried out in any known reactor for slurry polymerization. Such reactors include continuous stirred tank reactors and loop reactors. It is particularly preferred to carry out the polymerization in a loop reactor. In such a reactor, the slurry is circulated at high speed along a closed pipeline by using a circulation pump. Loop reactors are well known in the art, and examples are given, for example, in US-A-4582816, US-A-3405109, US-A-3324093, EP-A-479186 and US-A-5391654.

[0232] The slurry can be extracted from the reactor continuously or intermittently. A preferred mode for intermittent extraction is to use a settling leg, wherein the solids concentration of the slurry is increased before a batch of concentrated slurry is extracted from the reactor. The use of a settling leg is disclosed in US-A-3374211, US-A-3242150 and EP-A-1310295. Continuous extraction is disclosed in EP-A-891990, EP-A-1415999, EP-A-1591460 and EP-A-1860125. Continuous extraction can be combined with a suitable concentration method as disclosed in EP-A-1860125 and EP-A-1591460.

[0233] Other components may also be introduced into the slurry polymerization stage as is known in the art.

[0234] Process additives may also be introduced into the reactor to promote stable operation of the process.

[0235] When a slurry polymerisation stage is followed by a gas phase polymerisation stage, it is preferred to introduce the slurry directly into the gas phase polymerisation zone without a flash step between the two stages. Such direct feeds are described in EP-A-887379, EP-A-887380, EP-A-887381 and EP-A-991684.

[0236] The propylene copolymer (A) obtained from the multistage process can be extruded and pelletized and then blended with the ethylene copolymer (B) in the form of pellets.

[0237] The propylene copolymer (A) obtained from the multistage process can also be blended with the ethylene copolymer (B) in powder form.

[0238] The ethylene copolymer (B) is preferably polymerized under the above-mentioned single-site catalyst system.

[0239] Ethylene copolymer (B) can be prepared by any suitable polymerization process known in the art, the method comprising at least one polymerization stage, wherein the polymerization is usually carried out in solution, slurry, bulk or gas phase. Preferably, ethylene copolymer (B) is prepared in a multistage polymerization process comprising at least two polymerization zones.

[0240] The first ethylene polymer component is preferably prepared in the first polymerization zone, and the second ethylene polymer component is preferably prepared in the second polymerization zone.The first polymerization zone and the second polymerization zone can be connected in any order, and promptly the first polymerization zone can be before the second polymerization zone, or the second polymerization zone can be before the first polymerization zone, or, polymerization zone can be connected in parallel.But, preferably operate polymerization zone in cascade mode.Polymerization zone can be operated under slurry, solution or gas phase condition or their combination.

[0241] Suitable processes comprising cascaded slurry and gas phase polymerisation stages are disclosed in WO-A-92 / 12182 and WO-A-96 / 18662.

[0242] It is generally preferred to remove the reactants of the previous polymerization stage from the polymer before introducing it into a subsequent polymerization stage. This is preferably done when transferring the polymer from one polymerization stage to another.

[0243] The catalyst may be transferred to the polymerization zone by any means known in the art. For example, the catalyst may be suspended in a diluent and maintained as a homogeneous slurry, the catalyst may be mixed with a viscous mixture of grease and oil and the resulting paste fed to the polymerization zone, or the catalyst may be allowed to settle and a portion of the catalyst slurry thus obtained may be introduced into the polymerization zone.

[0244] The polymerization in the first polymerization zone is preferably carried out in a slurry. The polymer particles formed in the polymerization are then suspended in a fluid hydrocarbon together with the catalyst fragmented and dispersed in the particles. The slurry is stirred to transfer the reactants from the fluid to the particles.

[0245] The polymerization is usually carried out in an inert diluent, usually a hydrocarbon diluent, such as methane, ethane, propane, n-butane, isobutane, pentane, hexane, heptane, octane, etc., or a mixture thereof. Preferably, the diluent is a low boiling hydrocarbon having 1 to 4 carbon atoms or a mixture of these hydrocarbons, and the preferred diluent is propane.

[0246] The ethylene content in the fluid phase of the slurry may be 2 to about 50 mol%, preferably about 2 to about 20 mol%, and particularly preferably about 3 to about 12 mol%.

[0247] The temperature in the slurry polymerization is generally from 50 to 115° C., preferably from 60 to 110° C., particularly preferably from 70 to 100° C. The pressure is from 1 to 150 bar, preferably from 10 to 100 bar.

[0248] The slurry polymerization can be carried out in any known reactor for slurry polymerization.

[0249] Such reactors include continuous stirred tank reactors and loop reactors. It is particularly preferred to carry out polymerization in a loop reactor. In such a reactor, the slurry is circulated at high speed along a closed pipeline by using a circulation pump. Loop reactors are well known in the art, and examples are given, for example, in US-A-4582816, US-A-3405109, US-A-3324093, EP-A-479186 and US-A-5391654.

[0250] Sometimes, it is advantageous to carry out slurry polymerization above the critical temperature and pressure of the fluid mixture. Such operation is described in US-A-5391654. In such operation, the temperature is generally 85 to 110°C, preferably 90 to 105°C, and the pressure is 30 to 150 bar, preferably 50 to 100 bar.

[0251] The slurry can be extracted from the reactor continuously or intermittently. A preferred mode of intermittent extraction is to use a settling rod, wherein the slurry can be concentrated before a batch of concentrated slurry is extracted from the reactor. It is advantageous to combine continuous extraction with a suitable concentration method as disclosed in EP-A-1310295 and EP-A-1591460.

[0252] As known in the art, hydrogen can be added to the reactor to control the molecular weight of the polymer. In addition, for example, 1-butylene and / or 1-hexene can be added to the reactor to control the density of the polymer product. The actual amount of these hydrogen and 1-butylene and / or 1-hexene feeds depends on the melt index (or molecular weight) and the density (or comonomer content) of the catalyst used and the resulting polymer expectation.

[0253] The polymerization in the second polymerization zone is preferably carried out in gas phase, preferably in a fluidized bed reactor, a fast fluidized bed reactor or a settled bed reactor or any combination of these reactors. The polymerization in the second polymerization zone is more preferably carried out in a fluidized bed gas phase reactor, wherein ethylene is polymerized together with 1-butene and / or 1-hexene in the presence of a polymerization catalyst and preferably in the presence of the reaction mixture from the first polymerization zone in an upwardly moving gas stream. The reactor typically comprises a fluidized bed comprising polymer particles containing an active catalyst growing above a fluidization grid.

[0254] The polymer bed is fluidized by means of a fluidizing gas comprising olefin monomer, eventually comonomer, eventually chain growth controller or chain transfer agent (e.g. hydrogen) and eventually inert gas. The fluidizing gas is introduced into the inlet chamber at the bottom of the reactor. More than one of the above components may be added continuously to the fluidizing gas to compensate for losses caused by reaction or product extraction, etc.

[0255] The fluidizing gas is passed through the fluidized bed. The superficial velocity of the fluidizing gas must be higher than the minimum fluidizing velocity of the particles contained in the fluidized bed, otherwise no fluidization will occur. On the other hand, the velocity of the gas should be lower than the starting velocity for pneumatic transport, otherwise the entire bed will be carried along by the fluidizing gas.

[0256] When the fluidizing gas contacts the bed containing the active catalyst, the reactive components of the gas (e.g., monomers and chain transfer agents) react in the presence of the catalyst to form polymer products. At the same time, the gas is heated by the heat of reaction.

[0257] Unreacted fluidizing gas is removed from the top of the reactor and cooled in a heat exchanger to remove the heat of reaction. The gas is cooled to a temperature below the bed temperature to prevent the bed from heating up due to the reaction. The gas can be cooled to a temperature at which a portion of the gas condenses. When liquid droplets enter the reaction zone, they are vaporized.

[0258] The heat of evaporation helps to remove the heat of reaction. This operation is called condensing mode and variants thereof are disclosed in WO-A-2007 / 025640, USA-4543399, EP-A-699213 and WO-A-94 / 25495. As disclosed in EP-A-696293, condensing agents can also be added to the circulating gas stream. Condensing agents are non-polymerizable components, such as n-pentane, isopentane, n-butane or isobutane, which are at least partially condensed in a cooler.

[0259] The gas is then compressed and recycled to the inlet chamber of the reactor. Fresh reactants are introduced into the fluidizing gas stream before entering the reactor to compensate for losses caused by the reaction and product extraction. As is well known, the composition of the fluidizing gas should be analyzed and gas components introduced to keep the composition constant. The actual composition is determined by the desired properties of the product and the catalyst used in the polymerization.

[0260] The catalyst can be introduced into the reactor in various ways, continuously or intermittently. When the gas phase reactor is part of a cascade reactor, the catalyst is usually dispersed in polymer particles from the previous polymerization stage. As disclosed in EP-A-1415999 and WO-A-00 / 26258, polymer particles can be introduced into the gas phase reactor. As disclosed in EP-A-887379, EP-A-887380, EP-A-887381 and EP-A-991684, in particular if the previous reactor is a slurry reactor, it is advantageous to introduce the slurry directly into the fluidized bed of the gas phase reactor.

[0261] The polymer product can be extracted from the gas phase reactor continuously or intermittently. Combinations of these methods can also be used. Continuous extraction is disclosed in WO-A-00 / 29452. Intermittent extraction is disclosed in US-A-4621952, EP-A-188125, EP-A-250169 and EP-A-579426.

[0262] If desired, antistatic agents such as water, ketones, aldehydes and alcohols may also be introduced into the gas phase reactor. The reactor may also include a mechanical agitator to further promote mixing within the fluidized bed.

[0263] The fluidized bed polymerization reactor is usually operated at a temperature of 50 to 100° C., preferably 65 to 90° C. The pressure is suitably 10 to 40 bar, preferably 15 to 30 bar.

[0264] The polymerization of the first ethylene polymer component and the second ethylene polymer component in the first and second polymerization zones can be carried out before the prepolymerization step. The purpose of the prepolymerization is to polymerize a small amount of polymer onto the catalyst at low temperatures and / or low monomer concentrations. Through the prepolymerization, the performance of the catalyst in the slurry can be improved and / or the performance of the final polymer can be changed.

[0265] The prepolymerization step can be carried out in slurry or gas phase. The prepolymerization is preferably carried out in slurry, preferably in a loop reactor. The prepolymerization is then preferably carried out in an inert diluent, preferably a low boiling hydrocarbon having 1 to 4 carbon atoms or a mixture of these hydrocarbons.

[0266] The temperature in the prepolymerization step is usually from 0 to 90°C, preferably from 20 to 80°C, more preferably from 25 to 70°C.

[0267] The pressure is not critical and is usually 1 to 150 bar, preferably 10 to 100 bar.

[0268] The catalyst components are preferably all introduced into the prepolymerization step.

[0269] Preferably, the reaction product of the prepolymerization step is then introduced into the first polymerization zone.

[0270] The ethylene copolymer (B) obtained from the multistage process can be extruded and pelletized and then blended with the propylene copolymer (A) in the form of pellets.

[0271] The ethylene copolymer (B) obtained from the multistage process can also be blended with the propylene copolymer (A) in powder form.

[0272] Extrusion can be carried out in a manner generally known in the art, preferably in a twin screw extruder. An example of a suitable twin screw extruder is a co-rotating twin screw extruder. These are manufactured by Coperion or Japan Steel Works. Another example is a counter-rotating twin screw extruder. Such extruders are manufactured by Kobe Steel and Japan Steel Works.

[0273] Extruders typically include a melting section for molten polymer and a mixing section for homogenizing the polymer melt. Melting and homogenization are achieved by introducing energy into the polymer. The more energy introduced into the polymer, the better the homogenization effect achieved. However, too high energy introduction can lead to polymer degradation and deterioration of mechanical properties. Suitable specific energy input (SEI) levels are from about 200 to about 450 kWh / ton polymer, preferably from 240 to 350 kWh / ton.

[0274] Typically, the average residence time of the polymer in the extruder is from about 30 seconds to about 10 minutes. This value depends to some extent on the type of extruder. However, for most extruder types, a value of 1 minute to 5 minutes provides a good compromise between polymer homogeneity and mechanical properties.

[0275] Suitable extrusion methods are disclosed in EP-A-1600276 and WO-A-98 / 15591.

[0276] Prior to extrusion, the desired additives are mixed with the polymer.

[0277] use

[0278] In another aspect, the present invention relates to the use of a polypropylene composition for the manufacture of a pipe, the polypropylene composition having a melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 230° C. of 0.1 to 1.0 g / 10 min and comprising

[0279] (A) a copolymer of 70 to 95 wt.-%, based on the total weight of the polypropylene composition, of propylene and comonomer units derived from 1-butene or 1-hexene, said copolymer having:

[0280] 0.5 to 5.0 wt.-% total comonomer content;

[0281] a melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 230° C. of 0.10 to 2.0 g / 10 min; and

[0282] · a ratio of weight average molecular weight to number average molecular weight, Mw / Mn, as measured by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99 of 2.5 to 6.0; and

[0283] (B) 5 to 30 wt.-%, based on the total weight of the polypropylene composition, of a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene, said copolymer having:

[0284] 1.0 to 25.0 wt.-% total comonomer content;

[0285] 910.0 to 940.0 kg / m 3 The density measured in accordance with ISO 1183; and

[0286] • A melt flow rate MFR2 measured according to ISO 1133 at a load of 2.16 kg and a temperature of 190° C. of 0.05 to 3.0 g / 10 min.

[0287] All aspects of the polypropylene composition and pipe described above or below also apply to the use according to the present invention.

[0288] Hereinafter, the present invention is further illustrated by examples.

[0289] Example

[0290] 1. Determination method:

[0291] Unless otherwise defined, the following definitions of terms and determination methods apply to the above general description of the invention as well as to the following examples.

[0292] Quantification of copolymer microstructure by NMR spectroscopy

[0293] Comonomer determination:

[0294] 1-Hexene content in propylene-1-hexene copolymer

[0295] The NMR spectrometer was used on a Bruker Avance III 500 at 500.13 and 125.76 MHz. 1 H and 13 C to operate and record the quantitative 13 C{ 1 H} NMR spectra. All spectra were obtained using 13A C-optimized 7 mm magic angle spinning (MAS) probe was recorded at 180 °C, with nitrogen used for all pneumatics. Approximately 200 mg of material was loaded into a 7 mm outer diameter zirconium oxide MAS rotor and spun at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification. (Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2006; 207:382., Parkinson, M., Klimke, K., S piess,HW,Wilhelm,M.,Macromol.Chem.Phys.2007;208:2128.,Castignolles,P.,Graf,R.,Parkinson,M.,Wilhelm,M.,Gaborieau,M.,Polymer 50(2009)2373). Standard single pulse excitation (Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, H. W., Wilhelm, M., Macromol. Chem. Phys. 2006; 207: 382., Pollard, M., Klimke, K., Graf, R., Spiess, H. W., Wilhelm, M., Sperber, O., Piel, C., Kaminsky, W., Macromolecules 2004; 37: 813.) and RS-HEPT decoupling protocol were performed using NOE within a short recycle delay of 3 seconds. (Filip, X., Tripon, C., Filip, C., J. Mag. Resn. 2005, 176, 239., Griffin, JM, Tripon, C., Samoson, A., Filip, C., and Brown, SP, Mag. Res. in Chem. 2007 45, S1, S198.) A total of 16384 (16k) transients were collected for each spectrum.

[0296] Quantitative 13 C{ 1 H} NMR spectra were processed, integrated, and the relevant quantitative properties were determined from the integration. All chemical shifts were internally referenced to the methyl isotactic pentad (mmmm) at 21.85 ppm.

[0297] A characteristic signal corresponding to the incorporation of 1-hexene was observed and the comonomer content was quantified in the following manner.

[0298] The amount of 1-hexene incorporated in the PHP isolation sequence was quantified using the integral of the αB4 site over the number of reporter sites per comonomer at 44.2 ppm:

[0299] H=I αB4 / 2

[0300] The amount of 1-hexene incorporated in the PHHP bicontinuous sequence was quantified using the integral of the ααB4 site over the number of reporter sites per comonomer at 41.7 ppm:

[0301] HH=2*I ααB4

[0302] When two consecutive incorporations are observed, the amount of 1-hexene incorporated in the PHP separation sequence needs to be compensated due to the overlap of the signals αB4 and αB4B4 at 44.4 ppm:

[0303] H=(I αB4 –2*I ααB4 ) / 2

[0304] The total 1-hexene content was calculated based on the sum of separated and continuously incorporated 1-hexene:

[0305] H 总计 =H+HH

[0306] When no sites indicative of continuous incorporation were observed, the total content of 1-hexene comonomer was calculated based solely on this amount:

[0307] H 总计 =H

[0308] Characteristic signals indicative of regional 2,1-erythro defects were observed (Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000, 100, 1253).

[0309] The Pαβ (21e8) and Pαγ (21e6) methyl sites located at 17.7 and 17.2 ppm indicate the presence of 2,1-erythro regiodefects, which are confirmed by other characteristic signals.

[0310] The total amount of secondary (2,1-erythro) propylene incorporation was quantified based on the αα21e9 methylene site at 42.4 ppm:

[0311] P 21 =I αα21e9

[0312] The total amount of primary (1,2) incorporation of propylene is quantified based on the primary Sαα methylene site at 46.7 ppm and compensated for the relative amounts of unaccounted 2,1-erythro, αB4 and ααB4B4 methylene units of propylene (note the H and HH counts for the hexene monomers per sequence, not the number of sequences):

[0313] P 12 =I Sαα +2*P 21 +H+HH / 2

[0314] The total amount of propene is quantified as the sum of primary (1,2) and secondary (2,1-erythro) incorporated propene:

[0315] P 总计 =P 12 +P 21 =I Sαα +3*I αα21e9 +(I αB4 –2*I ααB4 ) / 2+I ααB4

[0316] Simplified to:

[0317] P 总计 =I Sαα +3*I αα21e9 +0.5*I αB4

[0318] The total mole fraction of 1-hexene in the polymer was calculated as follows:

[0319] f H =H 总计 / (H 总计 +P 总计 )

[0320] The complete integrated equation for the mole fraction of 1-hexene in the polymer is:

[0321] f H =(((I αB4 –2*I ααB4 ) / 2)+(2*I ααB4 )) / ((I Sαα +3*I αα21e9 +0.5*I αB4 )+

[0322] ((I αB4 –2*I ααB4 ) / 2)+(2*I ααB4 ))

[0323] Simplified to:

[0324] fH =(I αB4 / 2+I ααB4 ) / (I Sαα +3*I αα21e9 +I αB4 +I ααB4 )

[0325] The total comonomer incorporation of 1-hexene in mole percent is calculated in the conventional manner from the mole fractions:

[0326] H[mol-%]=100*f H

[0327] The total comonomer incorporation of 1-hexene in weight percent is calculated from the mole fractions in the standard manner:

[0328] H[wt.-%]=100*(f H *84.16) / ((f H *84.16)+((1-f H )*42.08))

[0329] Comonomer content of 1-butene and 1-hexene in linear low density polyethylene (LLDPE)

[0330] The NMR spectrometer was used on a Bruker Avance III 500 at 500.13 and 125.76 MHz. 1 H and 13 C to operate and record the quantitative 13 C{ 1 H} NMR spectra. All spectra were obtained using 13C was recorded at 150°C using a C-optimized 7 mm magic angle spinning (MAS) probe head, with nitrogen used for all pneumatics. Approximately 200 mg of material was loaded into a 7 mm outer diameter zirconium oxide MAS rotor and spun at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification. (Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2006; 207:382., Parkinson, M., Klimke, K., S piess,HW,Wilhelm,M.,Macromol.Chem.Phys.2007;208:2128.,Castignolles,P.,Graf,R.,Parkinson,M.,Wilhelm,M.,Gaborieau,M.,Polymer 50(2009)2373). Standard single pulse excitation (Pollard, M., Klimke, K., Graf, R., Spiess, H. W., Wilhelm, M., Sperber, O., Piel, C., Kaminsky, W., Macromolecules 2004; 37:813., Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, H. W., Wilhelm, M., Macromol. Chem. Phys. 2006; 207:382.) and RS-HEPT decoupling scheme (Filip, X., Tripon, C., Filip, C., J. Mag. Resn. 2005, 176, 239, Griffin, J. M., Tripon, C., Samoson, A., Filip, C., and Brown, S. P., Mag. Res. in Chem. Phys. 2006; 207:382.) were performed with a short recycle delay of 3 s. Chem. 2007 45, S1, S198). A total of 1024 (1k) transients were collected for each spectrum. This setting was chosen because of its high sensitivity to low comonomer contents.

[0331] Processing, integration and quantification using custom automated spectral analysis routines 13 C{ 1 H} NMR spectra and quantitative properties were determined. All chemical shifts were internally referenced to the bulk methylene signal (δ+) at 30.00 ppm (J. Randall, Macromol. Sci., Rev. Macromol. Chem. Phys. 1989, C29, 201).

[0332] The amount of ethylene is quantified based on the integration of the methylene (δ+) sites at 30.00 ppm over the number of reported sites per monomer:

[0333] E=I δ+ / 2

[0334] Correction of isolated comonomer units based on the number of isolated comonomer units:

[0335] E 总计 =E+(3*B+2*H) / 2

[0336] Where B and H are defined for the respective comonomers. Corrections are made in a similar manner when there are continuous and discontinuous copolymer incorporations.

[0337] Characteristic signals corresponding to the incorporation of 1-butene (J. Randall, Macromol. Sci., Rev. Macromol. Chem. Phys. 1989, C29, 201.) were observed as well as the total amount calculated relative to all other monomers in the polymer.

[0338] The amount of isolated 1-butene incorporated into the EEBEE sequence was quantified using the integration of the *B2 site at 38.3 ppm over the number of reporter sites per monomer:

[0339] B=I *B2

[0340] The amount of 1-butene continuously incorporated into the EEBBEE sequence was quantified using the integral of the ααB2B2 sites at 39.4 ppm over the number of reporter sites per monomer:

[0341] BB=2*I ααB2B2

[0342] The amount of 1-butene non-continuously incorporated into the EEBEBEE sequence was quantified using the integral of the ββB2B2 sites at 24.7 ppm over the number of reporter sites per monomer:

[0343] BEB=2*I ββB2B2

[0344] Since the *B2 and *βB2B2 sites of isolated (EEBEE) and discontinuously incorporated (EEBEBEE) 1-butene overlap, respectively, the total amount of isolated 1-butene incorporation was corrected based on the amount of discontinuous 1-butene:

[0345] B=I *B2 -2*I ββB2B2

[0346] The total amount of 1-butene was calculated based on the sum of isolated, continuous and discontinuously incorporated 1-butene:

[0347] B 总计 =B+BB+BEB

[0348] The total mole fraction of 1-butene in the polymer was calculated as follows:

[0349] f B =(B 总计 ) / (E 总计 +B 总计 +H 总计 )

[0350] Characteristic signals corresponding to the incorporation of 1-hexene (J. Randall, Macromol. Sci., Rev. Macromol. Chem. Phys. 1989, C29, 201) were observed as well as the total amount calculated relative to all other monomers in the polymer.

[0351] The amount of isolated 1-hexene incorporated into the EEHEE sequence was quantified using the integration of the *B4 site at 39.9 ppm over the number of reporter sites per monomer:

[0352] H=I *B4

[0353] The amount of 1-hexene incorporated continuously into the EEHHEE sequence was quantified using the integral of the ααB4B4 sites over the number of reporter sites per monomer at 40.5 ppm:

[0354] HH=2*I ααB4B4

[0355] The amount of 1-hexene non-continuously incorporated into the EEHEHEE sequence was quantified using the integral of the ββB4B4 sites over the number of reporter sites per monomer at 24.7 ppm:

[0356] HEH=2*I ββB4B4

[0357] Due to the overlap of the ββB2B2 sites of the discontinuously incorporated (EEBEBEE) 1-butene and the ββB4B4 sites of the discontinuously incorporated (EEHEHEE) 1-hexene, the total amount of the discontinuously incorporated (EEBEBEE) 1-butene was assumed to be proportional to the amount of isolated 1-butene (B) incorporated, and the total amount of the discontinuously incorporated (EEHEHEE) 1-hexene was assumed to be proportional to the amount of isolated 1-hexene (H).

[0358] The total mole fraction of 1-hexene in the polymer was calculated as follows:

[0359] fH=(H总计 ) / (E 总计 +B 总计 +H 总计 )

[0360] The mole percentage of comonomer incorporated is calculated from the mole fraction:

[0361] B[mol-%]=100*f B

[0362] H[mol-%]=100*f H

[0363] The weight percent of comonomer incorporated is calculated from the mole fraction:

[0364] B[wt.-%]=100*(f B *56.11) / ((f B *56.11)+(f H *84.16)+((1-(f B +f H ))*28.05))

[0365] H[wt.-%]=100*(f H *84.16) / ((f B *56.11)+(f H *84.16)+((1-(f B +f H ))*28.05))

[0366] Melt flow rate (MFR)

[0367] The melt flow rate (MFR) or melt index (MI) is measured according to ISO 1133. Where a different load can be used, the load is usually indicated by a subscript, e.g. MFR2 for a 2.16 kg load. According to ISO 1133, the temperature is chosen for the particular polymer, e.g. 230°C for polypropylene and 190°C for polyethylene. Thus, for polypropylene, MFR2 is measured at a temperature of 230°C and a load of 2.16 kg, while for polyethylene, MFR2 is measured at a temperature of 190°C and a load of 2.16 kg.

[0368] density

[0369] Density was measured according to ISO 1183-187. Sample preparation was done by compression molding according to ISO 1872-2:2007.

[0370] Analytical Temperature Rising Elution Fractionation (TRFF) obtained from Cross Fractionation Chromatography (CFC)

[0371] The chemical composition distribution as well as the determination of the molecular weight distribution and the corresponding molecular weight averages (Mn, Mw and Mv) at a certain elution temperature (polymer crystallinity in solution) are determined by fully automated cross fractionation chromatography (CFC) as described in Ortin A., Monrabal B., Sancho-Tello J., Macromol. Symp., 2007, 257, 13-28.

[0372] Cross fractionation chromatography (TREF×SEC) was performed using a CFC instrument (PolymerChar, Valencia, Spain). A four-band IR5 infrared detector (PolymerChar, Valencia, Spain) was used to monitor the concentration. At 150°C, about 40 mg of the polymer sample was dissolved in 25 ml of TCB in a stainless steel container for 150 minutes. Once the sample was completely dissolved, a 0.5 mL aliquot was loaded into the TREF column and stabilized at 110°C for a period of time. The polymer was crystallized and precipitated to a temperature of 30°C at a constant cooling rate of 0.1°C / min. The following temperature steps were used for the discontinuous elution method (30, 40, 50, 60, 70, 75, 80, 84, 88, 92, 95, 98, 100, 102, 104, 106, 108, 110, 115, 120, 130 and 140).

[0373] In the second dimension, GPC analysis manufactured by Agilent (Churchistriton, UK) was used with 3PLOlexis columns and 1x Olexis guard columns as stationary phase. 1,2,4-Trichlorobenzene (TCB, stabilized with 250 mg / L 2,6-di-tert-butyl-4-methylphenol) was used as eluent at 150 °C and a constant flow rate of 1 mL / min. The column set was calibrated using universal calibration (according to ISO 16014-2:2003) and at least 15 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11 500 kg / mol. The following Mark Houwink constants were used to convert PS molecular weights to PP molecular weight equivalents.

[0374] KPS = 19x10 -3 mL / g,α PS =0.655

[0375] KPP = 19x10 -3 mL / g,α PS =0.725

[0376] A third order polynomial fit was used to fit the calibration data. Data processing was performed using software provided by PolymerChar and the CFC instrument.

[0377] The polymer fraction with a logM between 4.5 and 6.0 eluting at temperatures between 31 and 80°C was determined.

[0378] The polymer fraction eluting between 31 and 80°C and having a molecular weight between logM 4.5 and 6 was calculated from the CFC data in the following manner:

[0379]

[0380] In a discontinuous elution process (see above), the polymer component eluting at 30°C is considered as the sweep fraction and is not included in the above calculation, which starts at 31°C.

[0381] GPC: Average molecular weight, molecular weight distribution and polydispersity index (M n 、M w 、M w / M n )

[0382] The average molecular weight (M) was determined by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99. w , M n ), molecular weight distribution (MWD) and its width, described by the polydispersity index, PDI = M w / M n (where M n is the number average molecular weight, M w is the weight average molecular weight).

[0383] A PolymerChar GPC instrument equipped with an infrared (IR) detector was used with 3xOlexis and 1x Olexis guard columns manufactured by Polymer Laboratories using 1,2,4-trichlorobenzene (TCB, stabilized with 250 mg / L 2,6-di-tert-butyl-4-methylphenol) as solvent at 160°C and a constant flow rate of 1 mL / min. 200 μL of sample solution was injected for each analysis. The column set was calibrated using a universal calibration (according to ISO 16014-2:2003) and at least 15 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11 500 kg / mol. Mark Houwink constants for PS, PE, and PP are as described in ASTM D 6474-99. All samples were prepared by dissolving 5.0 to 9.0 mg of polymer in 8 mL (160°C) stabilized TCB (same as mobile phase) with a dissolution time of 2.5 hours for PP and up to 3 hours for PE. Gentle shaking was continued in the autosampler of the GPC instrument at 160 °C.

[0384] DSC analysis, melting temperature (Tm) and crystallization temperature (Tc):

[0385] The measurements were performed on 5 to 7 mg samples using a TA Instruments Q2000 Differential Scanning Calorimetry (DSC). The DSC was run according to ISO 11357 / Part 3 / Method C2 in a heating / cooling / heating cycle with a scan rate of 10°C / min and a temperature range of -30 to +225°C.

[0386] The crystallization temperature (Tc) and the heat of crystallization (Hc) are determined by the cooling step, while the melting temperature (Tm) and the melting enthalpy (Hm) are determined by the second heating step.

[0387] Xylene solubles (XCS)

[0388] The xylene soluble (XCS) fraction, as defined and described in the present invention, is determined according to ISO 16152: 2.0 g of the polymer is dissolved in 250 mL of p-xylene under stirring at 135°C. After 30 minutes, the solution is cooled at ambient temperature for 15 minutes and then allowed to stand at 25 + / - 0.5°C for 30 minutes. The solution is filtered into two 100 mL flasks using filter paper. The solution of the first 100 mL container is evaporated in a stream of nitrogen and the residue is dried under vacuum at 90°C until a constant weight is reached. The xylene soluble fraction (percentage) can be determined as follows:

[0389] XS[%]=(100·m·V0) / (m0·V); m0=initial polymer amount [g]; m=residue weight [g]; V0=initial volume [ml]; V=analyzed sample volume [ml].

[0390] Determination of Al and Zr (ICP method)

[0391] The elemental analysis of the catalyst was performed by removing a solid sample of mass M and cooling it on dry ice. The sample was diluted to a known volume V by dissolving in nitric acid (HNO3, 65%, 5% V) and fresh deionized (DI) water (5% V). The solution was then added to hydrofluoric acid (HF, 40%, 3% V), diluted to a final volume V with deionized water, and left to stabilize for two hours.

[0392] The analysis was carried out at room temperature using an iCAP 6300 inductively coupled plasma optical emission spectrometer (ICP-OES) from Thermo Elemental, USA, which was calibrated using a blank solution (5% HNO3, 3% HF in deionized water) and six standard Al at 0.5 ppm, 1 ppm, 10 ppm, 50 ppm, 100 ppm and 300 ppm, and Hf and Zr at 0.5 ppm, 1 ppm, 5 ppm, 20 ppm, 50 ppm and 100 ppm in a 5% HNO3, 3% HF solution in deionized water.

[0393] Immediately prior to analysis, a "resloped" calibration was performed using a blank sample and 100ppm Al, 50ppm Hf, Zr standards, and a quality control sample (20ppmAl, 5ppm Hf, Zr in 5% HNO3, 3% HF in deionized water) was run to confirm the resloped. QC samples were also run after every 5 samples and at the end of a scheduled analysis set.

[0394] The hafnium content was monitored using the 282.022nm and 339.980nm lines, and the zirconium content was monitored using the 339.198nm line. The aluminum content was monitored by the 167.079nm line when the Al concentration in the ICP sample was between 0-10ppm (calibrated to 100ppm only), and by the 396.152nm line when the Al concentration exceeded 10ppm.

[0395] The values ​​reported are the average of three consecutive aliquots taken from the same sample and are related to the original catalyst by entering the original mass and dilution volume of the sample into the software.

[0396] In case of analysis of the elemental composition of the prepolymerized catalyst, the polymer fraction is digested by ashing so that the elements can be freely dissolved by acid. The total amount calculated corresponds to the weight percentage of the prepolymerized catalyst.

[0397] Catalyst activity

[0398] The catalyst activity was calculated based on the following formula:

[0399]

[0400] Yield

[0401] The total yield is calculated as follows

[0402]

[0403] For catalyst activity and productivity, the amount of catalyst used refers to the grams of prepolymerized catalyst or the grams of metallocene in the amount of prepolymerized catalyst used.

[0404] Degree of prepolymerization (DP): weight of polymer before prepolymerization step / weight of solid catalyst

[0405] The composition of the catalyst (before the off-line prepolymerization step) has been determined by ICP as described above. The metallocene content of the prepolymerized catalyst was calculated based on the ICP data as follows:

[0406] Formula 1

[0407]

[0408] Formula 2

[0409]

[0410] Formula 3

[0411]

[0412] Formula 4

[0413]

[0414] Particle size

[0415] Particle size distribution was measured with a Coulter LS200 particle size analyzer according to ISO 13320-1. The instrument is capable of measuring particle size distribution in the range of 0.4 to 2000 μm. The method is a laser diffraction method in which a laser beam is directed to a sample traveling in a flow-through cuvette. n-Heptane was used as the sample fluid.

[0416] The polymer sample is first pretreated by sieving out particles larger than 2 mm. The sieved sample is mixed with isopropanol and placed in an ultrasonic device in order to separate the particles from each other. The pretreated sample is then placed in the sample device for analysis. The results are calculated using a computer program provided with the instrument.

[0417] The PSD index (also called SPAN) is defined by the following equation (3):

[0418]

[0419] Where, d 50 (Dv 50 ) represents the median particle size, d 90 (Dv 90 ) means that 90% of the particles have a diameter smaller than d 90 The minimum particle size; d 10 (Dv 10) represents that 10% of the particles have a diameter smaller than d 10 The minimum particle size.

[0420] The following particle sizes and particle size distributions were used in the experiments:

[0421] D v90 = the volume of the particle size when the cumulative particle size is 90%,

[0422] D v10 = the volume of the particle size when the cumulative particle size is 10%,

[0423] D v50 = the volume of the particle size when the cumulative particle size is 50% (median volume particle size),

[0424] SPAN=(D v90 –D v10 ) / D v50 .

[0425] Flexural modulus

[0426] The flexural modulus was determined according to ISO 178. The dimensions of the test specimen were 80×10×4.0 mm 3 (length x width x thickness), produced by injection molding according to ISO 1873-2. The span length between the brackets was 64 mm, and the test speed was 2 mm / min.

[0427] Notched Impact Strength (NIS)

[0428] Charpy notched impact strength (NIS) according to ISO 179 1eA at +23°C, using 80×10×4 mm prepared according to EN ISO 1873-2 3 The measurements were performed on injection molded bar test specimens.

[0429] Pipeline pressure test

[0430] The pressure test performance of pipes made from the composition of the invention and the comparative composition was tested according to ISO 1167-1 and ISO 1167-2. Pipes with a diameter of 32 mm and a wall thickness of 3 mm were produced according to ISO 1167-2 on a conventional pipe extrusion line and then subjected to circumferential (hoop) stresses of 4.6 MPa and 4.9 MPa at a temperature of 95°C in a water-in-water apparatus according to ISO 1167-1. The time to failure was recorded in hours, plus the time "still in service" indicating that the time to failure had not yet been reached at the time of filing this patent application.

[0431] Pipe impact test

[0432] The Charpy impact strength of the pipe was measured according to ISO 9854-2. The samples were cut from the pipe (preparation details are shown below) and the sample size was 50×6×3 mm. 3 The tests were conducted at 0°C and 10 samples were tested each time. The failure type (broken / not broken) and the number of samples for each failure type are reported.

[0433] 2. Polymers used in the examples

[0434] a) Propylene copolymer

[0435] The polymerization of propylene copolymers was carried out on a pilot scale using a loop-gas phase reactor apparatus.

[0436] The polymerization catalyst for polymerizing the propylene copolymer is prepared as described in WO 2015 / 011135 A1 (metallocene complex MC1 with methylaluminoxane (MAO) and borate to form catalyst 3 described in WO 2015 / 011135 A1), provided that the surfactant is 2,3,3,3-tetrafluoro-2-(1,1,2,2,3,3-heptafluoropropoxy)-1-propanol. The metallocene complex (MC1 in WO 2015 / 011135 A1) is prepared as described in WO 2013 / 007650 A1 (metallocene E2 in WO 2013 / 007650 A1).

[0437] Hexene was used as comonomer in all cases and was introduced into both reactors (loop reactor and gas phase reactor) in order to control the desired hexene content of the final product.

[0438] The polymerization conditions are shown in Table 1.

[0439] Table 1: Polymerization conditions of propylene copolymers

[0440]

[0441]

[0442] b) Ethylene copolymers

[0443] The ethylene copolymer used in Example IE1 of the present invention is the linear low-density polyethylene of Example IE1 of EP 3 257 895 A1, having a 1-butene content of 0.3 mol-% (0.6 wt.-%), a 1-hexene content of 2.6 mol-% (8.1 wt.-%), and a density of 918 kg / m 3 , the melt flow rate MFR2 (190°C, 2.16kg) is 1.5g / 10min.

[0444] 3. Polypropylene composition and pipe

[0445] To prepare the polypropylene compositions of Comparative Examples CE, the above propylene copolymer was mixed with additives (1000 ppm of Irganox B215 (a 1:2 mixture of pentaerythritol-tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)-propionate (CAS No. 6683-19-8) and tris(2,4-di-tert-butylphenyl)phosphite (CAS No. 31570-04-4)) produced by BASF and 500 ppm of calcium stearate produced by Baerlocher) in a co-rotating twin-screw extruder at 220°C.

[0446] To prepare the polypropylene composition of inventive example IE, the above propylene copolymer and 15 wt% of an ethylene copolymer were mixed with additives (1000 ppm of Irganox B215 (a 1:2 mixture of pentaerythritol-tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)-propionate (CAS No. 6683-19-8) and tris(2,4-di-tert-butylphenyl)phosphite (CAS No. 31570-04-4) produced by BASF and 500 ppm of calcium stearate produced by Baerlocher) in a co-rotating twin-screw extruder at 220°C.

[0447] Pipes with a diameter of 32 mm and a wall thickness of 3 mm are produced on a Battenfeld Pro pipe extrusion line. Typical conditions are as follows:

[0448] Melting temperature: 224℃

[0449] Output: 30kg / h

[0450] Screw speed: 38rpm

[0451] Cooling water temperature: 20℃

[0452] Vacuum spray tank: 0.23bar

[0453] Water flow rate at the calibrator inlet: 4 l / h.

[0454] The polypropylene compositions and pipe properties of CE and IE are listed in Table 2.

[0455] Table 2: Compositions and properties of CE and IE pipes

[0456]

[0457] NB=No Break

[0458] *Testing stopped without any failures.

[0459] Figure 1 The TREF fractionation patterns and corresponding viscosity average molecular weights of IE1 and CE1 obtained by CFC analysis are shown.

[0460] Figure 2 The CFC profile of IE1 is shown. Claimed polymer fractions eluting between 31 and 80°C and logM between 4.5 and 6 are marked with squares.

[0461] Figure 3 The CFC profile of CE1 is shown. Claimed polymer fractions eluting between 31 and 80°C and logM between 4.5 and 6 are marked with squares.

[0462] In Example IE, the pipe manufactured according to the present invention exhibits a good balance of properties in terms of good surface quality, acceptable pressure resistance and improved impact resistance. In contrast, the pipe of Comparative Example CE breaks in the pipe impact test at 0°C.

Claims

1. A pipe comprising a polypropylene composition, in, The polypropylene composition comprises (A) a copolymer of 70 to 95 wt.-%, based on the total weight of the polypropylene composition, of propylene and comonomer units derived from 1-butene or 1-hexene, said copolymer having: 0.5 to 5.0 wt.-% total comonomer content; · Melt flow rate MFR measured according to ISO 1133 at a load of 2.16 kg and a temperature of 230° C. of 0.10 to 2.0 g / 10 min 2 ;as well as · a ratio of weight average molecular weight to number average molecular weight, Mw / Mn, as measured by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99 of 2.5 to 6.0; and (B) 5 to 30 wt.-%, based on the total weight of the polypropylene composition, of a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene, said copolymer having: 1.0 to 25.0 wt.-% total comonomer content; 910.0 to 940.0 kg / m 3 Density measured according to ISO 1183; as well as · Melt flow rate MFR measured according to ISO 1133 at a load of 2.16 kg and a temperature of 190° C. of 0.05 to 3.0 g / 10 min 2 ; The polypropylene composition has a melt flow rate (MFR) measured at a load of 2.16 kg and a temperature of 230° C. according to ISO 1133. 2 0.1 to 1.0 g / 10 min.

2. The pipeline according to claim 1, in, The polypropylene composition has a polymer fraction eluting at a temperature of 31 to 80°C excluding the purge fraction and having a logM between 4.5 and 6.0, the amount of the polymer fraction measured by cross fractionation chromatography (CFC) is 4 to 25 wt.-%, and / or the polypropylene composition has a characteristic profile in a temperature rising elution fractionation (TREF) elution profile obtained from cross fractionation chromatography (CFC) analysis comprising two peaks, wherein a first peak Tp(1) elutes between 45 to 90°C and a second peak Tp(2) elutes between 85 to 100°C.

3. A pipeline according to claim 1 or 2, in, The polypropylene composition has a flexural modulus of 700 to 1000 MPa, measured according to ISO 178 on injection molded specimens prepared according to EN ISO 1872-2.

4. A pipeline according to any one of claims 1 to 3, in, The polypropylene composition has a Charpy notched impact strength of 7.5 to 15.0 kJ / m at 23°C. 2 and / or a Charpy notched impact strength of 2.5 to 5.0 kJ / m at 0°C 2 and / or Charpy notched impact strength at -20°C of 1.5 to 4.0 kJ / m 2 , Charpy notched impact strength is determined according to ISO 179 1eA on injection molded specimens prepared according to EN ISO 1872-2.

5. The pipeline according to any one of claims 1 to 4, in, The polypropylene composition has one or more, preferably all, of the following properties: a xylene cold soluble content (XCS) of 1.0 to 3.5 wt.-%, measured according to ISO 16152; Melting temperature Tm measured according to ISO 11357 / Part 3 is 135 to 145°C; A crystallization temperature Tc of 100 to 110°C measured according to ISO 11357 / Part 3; and / or The melting enthalpy Hm measured according to ISO 11357 / Part 3 is 30 to 45 J / g.

6. A pipeline according to any one of claims 1 to 5, in, The propylene copolymer (A) has one or more, preferably all, of the following properties: a xylene cold soluble content (XCS) of 0.2 to 2.5 wt.-%, measured according to ISO 16152; Melting temperature Tm measured according to ISO 11357 / Part 3 is 135 to 145°C; A crystallization temperature Tc of 100 to 105°C measured according to ISO 11357 / Part 3; and / or The melting enthalpy Hm measured according to ISO 11357 / Part 3 is 70 to 80 J / g.

7. A pipeline according to any one of claims 1 to 6, in, The propylene copolymer (A) is obtained by polymerization in the presence of a single-site catalyst system, wherein the catalyst system comprises: (i) A catalyst having the following structure: In the formula, M is zirconium or hafnium; Each X is independently a σ-donating ligand L is the formula -(ER 10 2 ) y - bridge foundation; y is 1 or 2; E is C or Si; Each R 10 Independently for C 1 -C 20 Hydrocarbon, tri(C 1 -C 20 alkyl) silyl, C 6 -C 20 Aryl, C 7 -C 20 Arylalkyl or C 7 -C 20 Alkaryl, or L is an alkylene group, such as methylene or ethylene; R 1 are independently the same or different from each other and are CH 2 -R 11 Group, where R 11 is H or a straight or branched C 1 -C 6 Alkyl, C 3 -C 8 Cycloalkyl, C 6 -C 10 Aryl; R 3 , R 4 and R 5 are independently the same or different from each other and are H or a linear or branched C 1 -C 6 Alkyl, C 7 -C 20 Aralkyl, C 7 -C 20 Alkyl or C 6 -C 20 Aryl, provided that if there are four or more R 3 , R 4 and R 5 group, then R 3 , R 4 and R 5 at least one of is not tert-butyl; R 7 and R 8 are independently the same or different from each other and are H, CH 2 -R 12 Group, where R 12 is H or a straight or branched C 1 -C 6 Alkyl, SiR 13 3 ,GeR 13 3 , OR 13 , SR 13 NR 13 2 , Among them, R 13 Is a straight or branched chain C 1 -C 6 Alkyl, C 7 -C 20 Alkyl and C 7 -C 20 Arylalkyl or C 6 -C 20 Aryl, R 9 are independently the same or different from each other and are H or a linear or branched C 1 -C 6 Alkyl; and R 2 and R 6 are H; and (ii) A cocatalyst system comprising an aluminoxane cocatalyst.

8. A pipeline according to any one of claims 1 to 7, in, The ethylene copolymer (B) is a terpolymer of ethylene and a comonomer unit selected from 1-butene and 1-hexene, wherein the terpolymer has a 1-butene content of 0.1 to 5.0 wt.-%, and a 1-hexene content of 5.0 to 24.9 wt.-%.

9. A pipeline according to any one of claims 1 to 8, in, The ethylene copolymer (B) has an intrinsic viscosity iV, measured according to DIN ISO 1628 / 1, October 1999 (in decalin at 135° C.), of 1.5 to 2.5 dl / g.

10. The pipeline according to any one of claims 1 to 9, in, The ethylene copolymer (B) is obtained by polymerization in the presence of a single-site catalyst system.

11. The pipe according to any one of claims 1 to 10, wherein the pipe is a pressure pipe, preferably a pressure pipe for hot and cold water.

12. A method for manufacturing a pipe as claimed in any one of claims 1 to 11, comprising the following steps a) polymerizing propylene and 1-butene or 1-hexene in a multistage process in the presence of a single-site catalyst system to obtain a copolymer (A) of propylene and comonomer units derived from 1-butene or 1-hexene; b) blending the propylene copolymer (A) with a copolymer (B) of ethylene and comonomer units derived from 1-butene and / or 1-hexene to obtain a polypropylene composition; and c) manufacturing a pipe from the polypropylene composition.

13. The method according to claim 12, in, The multistage process is a sequential polymerization process having at least two polymerization reactors connected in series.

14. The method according to claim 12 or 13, in, The catalyst system comprises: (i) A catalyst having the following structure: In the formula, M is zirconium or hafnium; Each X is independently a σ-donor ligand L is the formula -(ER 10 2 ) y - bridge foundation; y is 1 or 2; E is C or Si; Each R 10 Independently for C 1 -C 20 Hydrocarbon, tri(C 1 -C 20 alkyl) silyl, C 6 -C 20 Aryl, C 7 -C 20 Arylalkyl or C 7 -C 20 Alkaryl, or L is an alkylene group, such as methylene or ethylene; R 1 are independently the same or different from each other and are CH 2 -R 11 Group, where R 11 is H or a straight or branched C 1 -C 6 Alkyl, C 3 -C 8 Cycloalkyl, C 6 -C 10 Aryl; R 3 , R 4 and R 5 are independently the same or different from each other and are H or a linear or branched C 1 -C 6 Alkyl, C 7 -C 20 Aralkyl, C 7 -C 20 Alkyl or C 6 -C 20 Aryl, provided that if there are four or more R 3 , R 4 and R 5 group, then R 3 , R 4 and R 5 at least one of is not tert-butyl; R 7 and R 8 are independently the same or different from each other and are H, CH 2 -R 12 Group, where R 12 is H or a straight or branched C 1 -C 6 Alkyl, SiR 13 3 ,GeR 13 3 , OR 13 , SR 13 NR 13 2 , Among them, R 13 Is a straight or branched chain C 1 -C 6 Alkyl, C 7 -C 20 Alkyl and C 7 -C 20 Arylalkyl or C 6 -C 20 Aryl, R 9 are independently the same or different from each other and are H or a linear or branched C 1 -C 6 Alkyl; and R 2 and R 6 are H; and (ii) A cocatalyst system comprising an aluminoxane cocatalyst.

15. Use of the polypropylene composition for producing a pipe, in, The melt flow rate MFR of the polypropylene composition measured according to ISO 1133 at a load of 2.16 kg and a temperature of 230° C. 2 0.1-1.0g / 10min, and contains (A) a copolymer of 70 to 95 wt.-%, based on the total weight of the polypropylene composition, of propylene and comonomer units derived from 1-butene or 1-hexene, said copolymer having: 0.5 to 5.0 wt.-% total comonomer content; · Melt flow rate MFR measured according to ISO 1133 at a load of 2.16 kg and a temperature of 230° C. of 0.10 to 2.0 g / 10 min 2 ;as well as · a ratio of weight average molecular weight to number average molecular weight, Mw / Mn, as measured by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99 of 2.5 to 6.0; and (B) 5 to 30 wt.-%, based on the total weight of the polypropylene composition, of a copolymer of ethylene with comonomer units derived from 1-butene and / or 1-hexene, said copolymer having: 1.0 to 25.0 wt.-% total comonomer content; 910.0 to 940.0 kg / m 3 Density measured according to ISO 1183; as well as · Melt flow rate MFR measured according to ISO 1133 at a load of 2.16 kg and a temperature of 190° C. of 0.05 to 3.0 g / 10 min 2 .

Citation Information

Patent Citations

  • Catalyst

    EP1739103A1

  • Bi- or multimodal polyethylene terpolymer with enhanced rheological properties

    EP3257895A1

  • Polypropylene pipe composition

    EP3567061A1

  • Process for preparing -olefin polymers or copolymers

    GB1580635A

  • Method and apparatus for the recovery of solid olefin polymer from a continuous path reaction zone

    US3242150A