Carbon black based on renewable carbon black feedstock
Through thermal oxidation pyrolysis or thermal cracking methods, combined with renewable carbon black raw materials and rubber-derived pyrolysis oil, the problem of dependence on fossil raw materials is solved, and carbon black materials with performance close to traditional carbon black are produced, achieving environmentally friendly and efficient carbon Black alternative.
Patent Information
- Application Number
- CN202380028857.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-29
- Filing Date
- 2023-04-18
- Publication Date
- 2024-11-05
AI Technical Summary
The existing carbon black production methods rely on fossil raw materials, resulting in environmental pollution and resource depletion. Renewable carbon black has performance challenges in application and is difficult to replace traditional carbon black.
Carbon black is produced by thermal oxidation pyrolysis or thermal cracking methods, and renewable carbon black raw materials and rubber-derived pyrolytic oil are used to control the content of carbon, hydrogen, sulfur, and nitrogen and the C/H atomic ratio, combined with specific process conditions. Carbon black materials with performance close to conventional carbon black are prepared, such as reactor design and termination steps.
It has achieved efficient and low cost production of carbon black from renewable materials, with mechanical properties and environmental protection advantages comparable to traditional carbon black, and is suitable for tires and mechanical rubber products, improving carbon dioxide balance.
Smart Images

Figure CN118900901A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing carbon black and the carbon black obtained by the method and the use of the carbon black. The present invention further relates to a composition comprising the carbon black and the use of the composition. Background Art
[0002] Carbon black is widely used in a variety of applications due to its unique properties, such as as a filler or pigment. However, carbon black is usually produced using fossil raw materials such as coal and crude oil. Fossil raw materials are limited and are being depleted at a fast rate. In addition, fossil raw materials mainly have a negative impact on the environment because their extraction and transportation have a great impact on the environment. For example, there have been oil spills in the past, which have led to water pollution and the death of aquatic animals (including those near the coast). In addition, it is well known that the combustion of fossil raw materials and the resulting carbon dioxide is one of the major factors causing global warming. The unstable prices of fossil raw materials and the dependence on politically unstable areas for transportation are further reasons for seeking alternatives to fossil raw materials.
[0003] It is desirable to avoid the disadvantages of using fossil raw materials. Renewable materials used as raw materials for the production of carbon black are more environmentally friendly. Renewable raw materials, such as plant-based renewable raw materials, are carbon dioxide neutral because the amount of carbon dioxide released into the atmosphere by the combustion of plant-based raw materials is equivalent to the amount of carbon dioxide absorbed by the plant during its life cycle. The use of renewable raw materials helps to conserve limited fossil resources and creates opportunities for the realization of a circular economy.
[0004] Depending on the application, it is desirable for carbon black materials produced from renewable feedstocks to exhibit certain properties comparable to known carbon blacks. However, this can be challenging when using renewable carbon black feedstocks.
[0005] Therefore, the object of the present invention is to provide a method for producing carbon black, creating opportunities for the realization of a circular economy and providing carbon black having comparable properties to known and already used carbon blacks. Another object of the present invention is to provide a rubber composition which improves the carbon dioxide balance while still providing comparable mechanical properties, suitable for the production of, for example, tires and mechanical rubber products. In addition, the rubber composition should also have good processability and be efficiently obtained from readily available materials at low cost. Summary of the invention
[0006] Surprisingly, the objects of the present invention are solved by the process disclosed in the independent claims and the carbon black obtained by the process. Particular or preferred variants of the invention are set out in the dependent claims.
[0007] The following items summarize certain aspects of the invention.
[0008] A first aspect of the present invention relates to a method for producing carbon black by thermal oxidative pyrolysis or thermal cracking of a carbon black feedstock, wherein the carbon black feedstock comprises (a) a renewable carbon black feedstock and (b) a rubber-derived pyrolysis oil.
[0009] A second aspect of the present invention relates to the method according to the first aspect, wherein the rubber-derived pyrolysis oil (b) comprises tire-derived pyrolysis oil (TPO).
[0010] A third aspect of the present invention relates to the method according to the first aspect or the second aspect, wherein the rubber-derived pyrolysis oil (b) consists of tire-derived pyrolysis oil (TPO).
[0011] A fourth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0012] Total carbon in the range of 80.0-90.0 mass %;
[0013] Total hydrogen in the range of 8.0-15.0 mass %; and
[0014] C / H atomic ratio in the range of 0.60-1.0;
[0015] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0016] A fifth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0017] Total carbon in the range of 85.0-90.0 mass %;
[0018] Total hydrogen in the range of 8.0-11.0 mass %; and
[0019] C / H atomic ratio in the range of 0.65-1.0;
[0020] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0021] A sixth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0022] Total carbon in the range of 86.0-90.0 mass %;
[0023] Total hydrogen in the range of 8.5-10.5 mass %; and
[0024] C / H atomic ratio in the range of 0.70-0.90;
[0025] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0026] A seventh aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0027] Total carbon in the range of 87.0-90.0 mass %;
[0028] Total hydrogen in the range of 9.0-10.0 mass %; and
[0029] C / H atomic ratio in the range of 0.70-0.85;
[0030] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0031] An eighth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0032] Up to 1.00 mass % total nitrogen; and / or
[0033] Up to 1.35 mass % total sulfur;
[0034] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0035] A ninth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0036] Up to 0.80 mass % total nitrogen; and / or
[0037] Up to 1.25 mass % total sulfur;
[0038] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0039] A tenth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0040] Up to 0.65 mass % total nitrogen; and / or
[0041] Up to 1.20 mass % total sulfur;
[0042] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0043] An eleventh aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0044] An ash content of less than 0.04 mass %, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil, and the ash content is determined according to ASTM D2415-20.
[0045] A twelfth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0046] An ash content of less than 0.03 mass %, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil, wherein the ash content is determined according to ASTM D2415-20.
[0047] A thirteenth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has:
[0048] Up to 250 mg / kg sieve residue based on the total weight of the rubber derived pyrolysis oil and determined according to ASTM D4870-18 (25 μm mesh size).
[0049] A fourteenth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil (b) has
[0050] Up to 230 mg / kg sieve residue based on the total weight of the rubber derived pyrolysis oil and determined according to ASTM D4870-18 (25 μm mesh size).
[0051] A fifteenth aspect of the present invention relates to a method according to any one of the second to fourteenth aspects, wherein the tire-derived pyrolysis oil (TPO) has
[0052] Total carbon in the range of 85.0-90.0 mass %;
[0053] Total hydrogen in the range of 8.0-11.0 mass %; and
[0054] C / H atomic ratio in the range of 0.65-1.0;
[0055] Wherein, mass % is based on the total mass of TPO excluding water and ash content, wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0056] A sixteenth aspect of the present invention relates to a method according to any one of the second to fifteenth aspects, wherein the TPO has:
[0057] Total carbon in the range of 86.0-90.0 mass %;
[0058] Total hydrogen in the range of 8.5-10.5 mass %; and
[0059] C / H atomic ratio in the range of 0.70-0.90;
[0060] Wherein, mass % is based on the total mass of TPO excluding water and ash content, wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0061] A seventeenth aspect of the present invention relates to a method according to any one of the second to sixteenth aspects, wherein the TPO has:
[0062] Total carbon in the range of 87.0-90.0 mass %;
[0063] Total hydrogen in the range of 9.0-10.0 mass %; and
[0064] C / H atomic ratio in the range of 0.70-0.85;
[0065] Wherein, mass % is based on the total mass of TPO excluding water and ash content, wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0066] The eighteenth aspect of the present invention relates to the method according to any one of the second to seventeenth aspects, wherein the TPO has:
[0067] 0.40-0.65 mass % total nitrogen; and / or
[0068] Up to 1.35 mass % total sulfur;
[0069] Wherein, mass % is based on the total mass of TPO excluding water and ash content, wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0070] A nineteenth aspect of the present invention relates to a method according to any one of the second to seventeenth aspects, wherein the TPO has
[0071] 0.45-0.65 mass % total nitrogen; and / or
[0072] Up to 1.25 mass % total sulfur;
[0073] Wherein, mass % is based on the total mass of TPO excluding water and ash content, wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0074] The twentieth aspect of the present invention relates to the method according to any one of the second to nineteenth aspects, wherein the TPO has:
[0075] 0.45-0.60 mass % total nitrogen; and / or
[0076] Up to 1.20 mass % total sulfur;
[0077] Wherein, mass % is based on the total mass of TPO excluding water and ash content, wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0078] A twenty-first aspect of the present invention relates to a method according to any one of the second to twentieth aspects, wherein the TPO has:
[0079] An ash content of less than 0.04 mass %, wherein the mass % is based on the total mass of the TPO, wherein the ash content is determined according to ASTM D2415-20.
[0080] The twenty-second aspect of the present invention relates to the method according to any one of the second to twenty-first aspects, wherein the TPO has:
[0081] An ash content of less than 0.03 mass %, wherein the mass % is based on the total mass of the TPO, wherein the ash content is determined according to ASTM D2415-20.
[0082] The twenty-third aspect of the present invention relates to the method according to any one of the second to twenty-second aspects, wherein the TPO has:
[0083] Up to 250 mg / kg sieve residue based on the total weight of TPO and determined according to ASTM D4870-18 (25 μm mesh size).
[0084] The twenty-fourth aspect of the present invention relates to the method according to any one of the second to twenty-third aspects, wherein the TPO has:
[0085] Up to 230 mg / kg sieve residue based on total TPO weight and determined according to ASTM D4870-18 (25 μm mesh size).
[0086] A twenty-fifth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the renewable carbon feedstock (a) comprises a plant-based feedstock.
[0087] The twenty-sixth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the renewable carbon black feedstock (a) comprises wood, grass, cellulose, hemicellulose, lignin, black liquor, tall oil, rubber seed oil, tobacco seed oil, castor oil, pongamia oil, crambe oil, neem oil, apricot kernel oil, rice bran oil, cashew nut shell liquid, cyperus esculentus oil, rice bran oil, rapeseed oil, linseed oil, palm oil, coconut oil, canola oil, soybean oil, sunflower seed oil, cottonseed oil, pine nut oil, olive oil, corn oil, grape seed oil, safflower oil, acai palm oil, jambú oil, sesame oil, chia seed oil, hemp seed oil, perilla oil, peanut oil, stillingia oil, etc. oil), cashew oil, Brazil nut oil, macadamia oil, walnut oil, almond oil, hazelnut oil, beechnut oil, candlenut oil, chestnut oil, or a mixture or combination of any of the foregoing.
[0088] The twenty-seventh aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the renewable carbon black feedstock (a) comprises soybean oil, rapeseed oil, or a mixture or combination of any of the foregoing.
[0089] A twenty-eighth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the renewable carbon black feedstock (a) comprises rapeseed oil.
[0090] The twenty-ninth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber-derived pyrolysis oil contains at least 10 wt. %, preferably at least 30 wt. %, more preferably at least 50 wt. %, even more preferably at least 70 wt. %, and most preferably at least 90 wt. % of tire-derived pyrolysis oil (TPO), based on the total weight of the rubber-derived pyrolysis oil.
[0091] The thirtieth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the carbon black feedstock has a ratio of renewable carbon black feedstock (a) to rubber-derived pyrolysis oil of 0.1:1 to 1:0.1, preferably 0.3:1 to 1:0.3.
[0092] The thirty-first aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the carbon black feedstock has a ratio of renewable carbon black feedstock (a) to rubber-derived pyrolysis oil of 0.5:1 to 1:0.5.
[0093] A thirty-second aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the carbon black feedstock comprises:
[0094] (a) 10-90 wt %, preferably 20-80 wt %, more preferably 40-60 wt %, most preferably 45-55 wt % of renewable carbon black feedstock, based on the total weight of the carbon black feedstock.
[0095] The thirty-third aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the carbon black feedstock comprises:
[0096] (b) 10-90 wt %, preferably 20-80 wt %, more preferably 40-60 wt %, most preferably 45-55 wt % of rubber derived pyrolysis oil, based on the total weight of the carbon black feedstock.
[0097] The thirty-fourth aspect of the present invention relates to a method according to any one of the preceding aspects, comprising: inputting an O2-containing gas stream and a fuel stream containing a combustible substance into a reactor; combusting the combustible substance in a combustion step to provide a combustion gas stream, wherein the O2-containing gas stream and the fuel stream containing the combustible substance are provided to the combustion step in an amount corresponding to a k factor in the range of 0.5-1.0, wherein the k factor is the ratio of the O2 theoretically required for the stoichiometric combustion of all the combustible substances in the combustion step to the total O2 provided for the combustion step; contacting a carbon black feedstock with the combustion gas stream in a reaction step to form carbon black; and terminating the carbon black forming reaction in a termination step;
[0098] The thirty-fifth aspect of the present invention relates to the method according to the thirty-fourth aspect, wherein the k factor is in the range of 0.6-1.0, preferably 0.7-1.0, more preferably 0.75-1.0, and even more preferably 0.8-1.0.
[0099] The thirty-sixth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the reaction is carried out in a furnace black reactor.
[0100] The thirty-seventh aspect of the present invention relates to carbon black obtained by the method according to any one of the preceding aspects.
[0101] The thirty-eighth aspect of the present invention relates to the carbon black according to the thirty-seventh aspect, wherein the carbon black has:
[0102] Equal to or greater than 70mL / 100g oil absorption number (OAN);
[0103] Herein, OAN is measured according to ASTM D2414-21.
[0104] The thirty-ninth aspect of the present invention relates to the carbon black according to the thirty-seventh or thirty-eighth aspect, wherein the carbon black has:
[0105] The difference (gap) between OAN and COAN in the range of 10-45 mL / 100 g;
[0106] OAN is measured according to ASTM D2414-21, and COAN is measured according to ASTM D3493-21.
[0107] The 40th aspect of the present invention relates to the carbon black according to any one of the 37th to 39th aspects, wherein the carbon black has:
[0108] Not more than or equal to 90m 2 / g of statistical adsorption layer thickness surface area (statistical thickness surface area, STSA);
[0109] Wherein STSA is measured according to ASTM D6556-19a.
[0110] The 41st aspect of the present invention is directed to the carbon black according to any one of the 37th to 40th aspects, wherein the carbon black has an OAN in the range of 70-145 mL / 100 g; wherein the OAN is measured according to ASTM D2414-21.
[0111] The 42nd aspect of the present invention relates to a carbon black according to any one of aspects 37 to 41, wherein the difference (gap) between the OAN and COAN of the carbon black is in the range of 10-40 mL / 100 g, preferably 12-35 mL / 100 g, and more preferably 12-30 mL / 100 g; wherein the OAN is measured according to ASTM D2414-21 and the COAN is measured according to ASTM D3493-21.
[0112] The 43rd aspect of the present invention relates to the carbon black according to any one of the 37th to 42nd aspects, wherein the carbon black has a STSA of 20-90 m 2 / g, preferably 23-90m 2 / g, more preferably 25-85m 2 / g; wherein STSA is measured according to ASTM D6556-19a.
[0113] The 44th aspect of the present invention relates to the carbon black according to any one of the 37th to 43rd aspects, wherein the carbon black has a BET specific surface area of 20-120 m 2 / g, preferably 23-110m 2 / g, more preferably 25-100m2 / g; wherein the BET specific surface area is measured according to ASTM D6556-19a.
[0114] The forty-fifth aspect of the present invention relates to a carbon black according to any one of aspects thirty-seven to forty-four, wherein the sulfur content of the carbon black is not more than 2.5%, preferably not more than 2.0%, and more preferably not more than 1.5%; wherein the sulfur content is determined according to ASTM D1619-20.
[0115] The forty-sixth aspect of the present invention relates to a carbon black according to any one of aspects thirty-seven to forty-fifth, wherein the pMC (percentage of modern carbon) of the carbon black is above 30%, preferably above 40%, more preferably above 50%, even more preferably above 75%, and most preferably above 90%, wherein the pMC is measured according to ASTM D6866-20 Method B (AMS).
[0116] The 47th aspect of the present invention relates to the carbon black according to any one of the 37th to 46th aspects, wherein the carbon black is furnace black.
[0117] The forty-eighth aspect of the present invention relates to the carbon black according to any one of the thirty-seventh to forty-seventh aspects, wherein the carbon black is oxidized and / or functionalized.
[0118] The forty-ninth aspect of the present invention relates to the use of the carbon black according to any one of the thirty-seventh to forty-eighth aspects as a reinforcing filler or additive, a UV stabilizer, a conductive carbon black or a pigment, preferably as a reinforcing filler or additive.
[0119] The fiftieth aspect of the present invention relates to the use of the carbon black according to any one of aspects 37 to 48 in rubber and rubber mixtures, plastics, inks (such as printing inks, inkjet inks or other inks), toners, paints, coatings, paper, adhesives, batteries or black matrix applications, preferably in rubber and rubber mixtures or plastics.
[0120] The fifty-first aspect of the present invention is directed to a rubber composition including at least one rubber material and at least one carbon black according to any one of the thirty-seventh to forty-eighth aspects.
[0121] The fifty-second aspect of the present invention relates to a rubber composition according to the fifty-first aspect, wherein at least one rubber material includes natural rubber, styrene-butadiene rubber, such as emulsion-styrene-butadiene rubber and solution-styrene-butadiene rubber, polybutadiene, polyisoprene, ethylene-propylene-diene rubber, ethylene-propylene rubber, butyl rubber, halogenated butyl rubber, chlorinated polyethylene, chlorosulfonated polyethylene, nitrile rubber, hydrogenated nitrile rubber, polychloroprene, acrylate rubber, ethylene-vinylacetate rubber, ethylene-acrylic acid rubber, epichlorohydrin rubber, silicone rubber, fluorosilicone rubber, fluorocarbon rubber or a mixture or combination of any of the above rubbers.
[0122] The fifty-third aspect of the present invention relates to the use of the rubber composition according to the fifty-first or fifty-second aspect for producing a tire, preferably a pneumatic tire, a tire tread, a belt, a belt reinforcement, a carcass, a carcass reinforcement, a sidewall, an inner liner, an apex, a shoulder, a hump strip, a chafer, a beadfiller, a cable sheath, a pipe, a drive belt, a conveyor belt, a roller covering, a shoe sole, a hose, a seal, a profile, a damping element, a coating or a colored or printed product.
[0123] The fifty-fourth aspect of the present invention is directed to a tire made from the rubber composition according to the fifty-first or fifty-second aspect.
[0124] The fifty-fifth aspect of the present invention relates to a tire according to the fifty-fourth aspect, wherein the tire includes a tire tread, a belt layer, a belt layer reinforcement, a carcass, a carcass reinforcement, a sidewall, an inner liner, a apex strip, a shoulder, a peak strip, a bead cover, and a bead outer guard, wherein at least one of the above components is made of a rubber composition according to the fifty-first or fifty-second aspect.
[0125] The fifty-sixth aspect of the present invention relates to a tire according to the fifty-fourth or fifty-fifth aspect, wherein the tire has a circumferential tread of a cap / base configuration, the circumferential tread of the cap / base configuration comprising a circumferential outer tread cap rubber layer comprising the running surface of the tire, and a tread base rubber layer at least partially covering the tread cap rubber layer, wherein at least one of the tread cap rubber layer and the tread base rubber layer is made of the rubber composition according to the fifty-first or fifty-second aspect.
[0126] The fifty-seventh aspect of the present invention relates to an article made from the rubber composition according to the fifty-first or fifty-second aspect, which is a cable sheath, a pipe, a transmission belt, a conveyor belt, a roller covering, a shoe sole, a hose, a seal, a profile, a damping element, a coating or a colored or printed product.
[0127] The fifty-eighth aspect of the present invention relates to a plastic composition comprising at least one plastic material and at least one carbon black according to any one of the thirty-seventh to forty-eighth aspects.
[0128] The fifty-ninth aspect of the present invention relates to a plastic composition according to the fifty-eighth aspect, wherein at least one plastic material comprises a thermoplastic polymer, a thermosetting polymer, a thermoplastic elastomer, preferably low-density and high-density polyethylene and polypropylene, polyvinyl chloride, melamine-formaldehyde resin, phenolic resin, epoxy resin, polyamide, polyester, polyoxymethylene, polymethyl methacrylate, polycarbonate, polystyrene, polyurethane, polyphenylene oxide, polysiloxane, polyacryloamide, polyaryletherketone, polysulfone, polyetherimide, acrylonitrile-styrene-acrylate or acrylonitrile-butadiene-styrene polymer, and mixtures or copolymers of any of the above substances. DETAILED DESCRIPTION
[0129] The present invention relates to a method for producing carbon black by thermal oxidation pyrolysis or thermal cracking of carbon black raw materials. The carbon black raw materials of the present invention include (a) renewable carbon black raw materials and (b) rubber-derived pyrolysis oil.
[0130] As used herein, the term "carbon black" refers to a material consisting essentially of carbon, e.g., a material containing more than 80%, or more than 90%, or more than 95% carbon based on the total weight of the material. The production of carbon black is well known in the art, e.g., in J.-B. Donnet et al., "Carbon Black: Science and Technology", 2 nd edition and H.Ferch "Pigmentruβe",1 st This is summarized in , Curt R. Vincentz Verlag, Hannover (1995), and is further described below.
[0131] As used herein, the term "rubber-derived pyrolysis oil" refers to the liquid fraction obtained during the pyrolysis of rubber products. Rubber-derived pyrolysis oil generally contains a mixture of saturated and unsaturated hydrocarbons and may contain polar compounds including sulfur, nitrogen and oxygen.
[0132] The pyrolysis of rubber products generally includes heating the rubber products to a temperature of, for example, at least 300° C. under anaerobic conditions to volatilize and decompose the rubber products, producing oil, gas and char. As used herein, the term "rubber product" refers to a product composed of rubber, for example, a product composed of at least 50% by weight of rubber based on the total weight of the rubber product. Examples of rubber products include, but are not limited to, tires, conveyor belts, washers (e.g., door washers), transmission belts, floor mats, soles, belts, cable sheaths, hoses, and the like. Preferably, the rubber product includes a tire. The term "rubber" includes natural rubber and synthetic rubber or mixtures thereof. Natural rubber can be obtained from Helvea brasiliensis, guayule and dandelion. The synthetic rubber may include styrene butadiene rubber, such as emulsion and solution polymerized styrene butadiene rubber, polybutadiene, polyisoprene, EPDM, EPDM, butyl rubber, halogenated butyl rubber, chlorinated polyethylene, chlorosulfonated polyethylene, nitrile rubber, hydrogenated nitrile rubber, chloroprene rubber, acrylate rubber, ethylene vinyl acetate rubber, ethylene acrylic rubber, epichlorohydrin rubber, silicone rubber, fluorosilicone rubber, fluorocarbon rubber, or a mixture or combination of any of the above rubbers.
[0133] According to the present invention, rubber-derived pyrolysis oil may include tire-derived pyrolysis oil (TPO). As used herein, the term "tire-derived pyrolysis oil" ("TPO") refers to a liquid fraction obtained by pyrolyzing a tire under anaerobic conditions. TPO typically contains a mixture of saturated and unsaturated hydrocarbons and may contain polar compounds including sulfur, nitrogen and oxygen. Typically, waste tires (also known as "end-of-life" tires (ELT)) are used for pyrolysis to obtain TPO. As used herein, "waste tires" or "scrap tires" refer to tires that are unsuitable for use on vehicles due to, for example, wear or irreparable damage (e.g., punctures), such as truck tires, passenger car tires, off-road tires, aircraft tires, agricultural tires, and earth-moving machinery tires.
[0134] Pyrolysis processes for rubber products (e.g., tires) are well known in the art and include heating the tire in the absence of oxygen. Suitable methods for obtaining rubber-derived pyrolysis oils, particularly TPO, include, but are not limited to, those described in US2002 / 0072641A1, US2002 / 0072640A1, US2005 / 0101812A1, and EP2427533A1.
[0135] The rubber-derived pyrolysis oil may comprise at least 5 wt %, such as at least 10 wt %, or at least 10 wt %, or at least 15 wt %, or at least 20 wt %, or at least 25 wt %, or at least 30 wt %, or at least 35 wt %, or at least 40 wt %, or at least 45 wt %, or at least 50 wt %, or at least 55 wt %, or at least 60 wt %, or at least 65 wt %, or at least 70 wt %, or at least 75 wt %, or at least 80 wt %, or at least 85 wt %, or at least 90 wt %, or at least 95 wt %, or at least 99 wt % of tire-derived pyrolysis oil (TPO), based on the total weight of the rubber-derived pyrolysis oil. According to the present invention, the rubber-derived pyrolysis oil may comprise at least 10 wt %, preferably at least 30 wt %, more preferably at least 50 wt %, even more preferably at least 70 wt %, and most preferably at least 90 wt % of TPO, based on the total weight of the rubber-derived pyrolysis oil. The rubber-derived pyrolysis oil of the present invention may consist of TPO.
[0136] Suitable examples of rubber derived pyrolysis oils, particularly TPOs, include, but are not limited to, ThermoTireOil RR commercially available from Pyrum Innovations AG (Germany).
[0137] According to the present invention, the flash point of the rubber-derived pyrolysis oil may be at least 3°C, preferably at least 5°C, more preferably 50°C, and most preferably at least 65°C. As used herein, the term "flash point" refers to the lowest temperature at which a volatile substance vaporizes in air to form a flammable mixture. The flash point may be determined according to ASTM D93D. The rubber-derived pyrolysis oil may be treated by distillation (e.g., atmospheric fractionation, thin film distillation, etc.) to obtain a fraction having a higher flash point, e.g., at least 65°C.
[0138] According to the present invention, the total carbon of the rubber-derived pyrolysis oil (b) may be at least 80.0% by mass, such as at least 81.0% by mass, or at least 82.0% by mass, or at least 83.0% by mass, or at least 84.0% by mass, or at least 85.0% by mass, or at least 85.5% by mass, or at least 86.0% by mass, or at least 86.5% by mass, or at least 87.0% by mass, or at least 87.5% by mass, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The total carbon of the rubber-derived pyrolysis oil (b) may be 90.0% by mass or less, such as 89.5% by mass or less, or 89.0% by mass or less, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The moisture content may be determined according to ASTM D4928-12R18, and the ash content may be determined according to ASTM D2415-20 (at 550°C). Those skilled in the art will appreciate that any range between any explicitly disclosed lower and upper limits is disclosed herein. Thus, the total carbon of the rubber derived pyrolysis oil (b) may be in the range of 80.0-90.0 mass %, preferably 85.0-90.0 mass %, more preferably 86.0-90.0 mass %, and most preferably 87.0-90.0 mass %, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content. The total carbon is determined according to ASTM D5291C-21.
[0139] According to the present invention, the total hydrogen of the rubber-derived pyrolysis oil (b) may be at least 8.0% by mass, such as at least 8.5% by mass, or at least 9.0% by mass, or at least 9.5% by mass, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The moisture content may be determined according to ASTM D4928-12R18, and the ash content may be determined according to ASTM D2415-20 (at 550° C.). The total hydrogen of the rubber-derived pyrolysis oil (b) may be 15.0% by mass or less, such as 14.0% by mass or less, or 13.0% by mass or less, or 12.0% by mass or less, or 11.0% by mass or less, or 10.5% by mass or less, or 10.0% by mass or less, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the total hydrogen of the rubber-derived pyrolysis oil (b) may be in the range of 8.0-15.0 mass %, preferably 8.0-11.0 mass %, more preferably 8.5-10.5 mass %, most preferably 9.0-10.0 mass %, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The total hydrogen is determined according to ASTM D5291C-21.
[0140] According to the present invention, the C / H atomic ratio of the rubber-derived pyrolysis oil (b) may be at least 0.60, such as at least 0.65, or at least 0.70, or at least 0.75. The C / H atomic ratio of the rubber-derived pyrolysis oil (b) may be less than 1.0, such as less than 0.95, or less than 0.90, or less than 0.85, or less than 0.80. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the C / H atomic ratio of the rubber-derived pyrolysis oil (b) may be in the range of 0.60-1.0, preferably 0.65-1.0, preferably 0.70-0.90, and more preferably 0.70-0.85. The C / H atomic ratio is calculated based on the total carbon and total hydrogen determined according to ASTM D5291C-21 as described above.
[0141] The rubber derived pyrolysis oil (b) may have:
[0142] Total carbon in the range of 80.0-90.0 mass %, preferably 85.0-90.0 mass %, more preferably 86.0-90.0 mass %, most preferably 87.0-90.0 mass %;
[0143] Total hydrogen in the range of 8.0-15.0 mass %, preferably 8.0-11.0 mass %, more preferably 8.5-10.5 mass %, most preferably 9.0-10.0 mass %; and
[0144] a C / H atomic ratio in the range of 0.60-1, preferably 0.65-1.0, more preferably 0.70-0.90, most preferably 0.70-0.85;
[0145] Wherein, mass % is based on the total mass of rubber derived pyrolysis oil excluding water and ash content. Total carbon and total hydrogen are determined according to ASTM D5291C-21. C / H atomic ratio is calculated based on total carbon and total hydrogen. Water content can be determined according to ASTMD4928-12R18, and ash content can be determined according to ASTM D2415-20 (at 550°C).
[0146] According to the present invention, the total nitrogen of the rubber-derived pyrolysis oil (b) may be at least 0.01 mass%, such as at least 0.02 mass%, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The moisture content may be determined according to ASTM D4928-12R18, and the ash content may be determined according to ASTM D2415-20 (at 550° C.). The total nitrogen of the rubber-derived pyrolysis oil (b) may be at most 1.00 mass%, such as at most 0.90 mass%, or at most 0.80 mass%, or at most 0.70 mass%, or at most 0.65 mass%, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Thus, the total nitrogen of the rubber derived pyrolysis oil (b) may be in the range of 0.01-1.00 mass %, such as 0.01-0.80 mass %, or 0.01-0.65 mass %, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content. The total nitrogen is determined according to ASTM D5291C-21.
[0147] According to the present invention, the total sulfur of the rubber-derived pyrolysis oil (b) may be at most 1.35 mass%, such as at most 1.30 mass%, or at most 1.25 mass%, or at most 1.20 mass%, or at most 1.15 mass%, or at most 1.10 mass%, wherein the mass% is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The moisture content may be determined according to ASTM D4928-12R18, and the ash content may be determined according to ASTM D2415-20 (at 550°C). The total sulfur is determined according to ASTM D5291C-21.
[0148] The rubber derived pyrolysis oil (b) may have:
[0149] Up to 1.00 mass %, preferably up to 0.80 mass %, more preferably up to 0.65 mass % of total nitrogen; and
[0150] Up to 1.35 mass %, preferably up to 1.25 mass %, more preferably up to 1.20 mass % total sulfur;
[0151] Wherein, mass % is based on the total mass of rubber derived pyrolysis oil excluding water and ash content. Total nitrogen and total sulfur are determined according to ASTM D5291C-21. Moisture content can be determined according to ASTM D4928-12R18, and ash content can be determined according to ASTM D2415-20 (at 550°C).
[0152] According to the present invention, the rubber derived pyrolysis oil (b) may have:
[0153] Total carbon in the range of 80.0-90.0 mass %, preferably 85.0-90.0 mass %, more preferably 86.0-90.0 mass %, most preferably 87.0-90.0 mass %;
[0154] Total hydrogen in the range of 8.0-15.0, preferably 8.0-11.0 mass %, more preferably 8.5-10.5 mass %, most preferably 9.0-10.0 mass %;
[0155] a C / H atomic ratio in the range of 0.60-1.0, preferably 0.65-1.0, more preferably 0.70-0.90, most preferably 0.70-0.85;
[0156] Up to 1.00 mass %, preferably up to 0.80 mass %, more preferably up to 0.65 mass % of total nitrogen; and
[0157] Up to 1.35 mass %, preferably up to 1.25 mass %, more preferably up to 1.20 mass % total sulfur;
[0158] Wherein, mass % is based on the total mass of rubber derived pyrolysis oil excluding water and ash content. Total carbon, total hydrogen, total nitrogen and total sulfur are determined according to ASTM D5291C-21. C / H atomic ratio is calculated based on total carbon and total hydrogen. Water content can be determined according to ASTM D4928-12R18, and ash content can be determined according to ASTM D2415-20 (at 550°C).
[0159] According to the present invention, the ash content of the rubber-derived pyrolysis oil (b) may be less than 0.04 mass %, such as less than 0.03 mass %, or less than 0.02 mass %, or less than 0.01 mass %, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil. The ash content is measured according to ASTM D2415-20 (at 550°C).
[0160] The sieve residue of the rubber derived pyrolysis oil (b) may be 250 mg / kg or less, such as 230 mg / kg or less, based on the total weight of the rubber derived pyrolysis oil. The sieve residue is determined according to ASTM D4870-18 (25 μm mesh size).
[0161] According to the present invention, the total carbon of the TPO can be at least 85.0% by mass, such as at least 85.5% by mass, or at least 86.0% by mass, or at least 86.5% by mass, or at least 87.0% by mass, or at least 87.5% by mass, wherein the mass % is based on the total weight of the TPO excluding water and ash content. The moisture content can be determined according to ASTM D4928-12R18, and the ash content can be determined according to ASTM D2415-20 (at 550° C.). The total carbon of the TPO can be 90.0% by mass or less, such as 89.5% by mass or less, or 89.0% by mass or less, wherein the mass % is based on the total mass of the TPO excluding water and ash content. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the total carbon of TPO can be in the range of 85.0-90.0 mass %, preferably 86.0-90.0 mass %, more preferably 87.0-90.0 mass %, wherein the mass % is based on the total mass of TPO excluding water and ash content. The total carbon is determined according to ASTM D5291C-21.
[0162] According to the present invention, the total hydrogen of TPO can be at least 8.0% by mass, such as at least 8.5% by mass, or at least 9.0% by mass, or at least 9.5% by mass, wherein the mass % is based on the total mass of TPO excluding water and ash content. The moisture content can be determined according to ASTM D4928-12R18, and the ash content can be determined according to ASTM D2415-20 (at 550°C). The total hydrogen of TPO can be 11.0% by mass or less, such as 10.5% by mass or less, or 10.0% by mass or less, wherein the mass % is based on the total mass of TPO excluding water and ash content. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the total hydrogen of TPO can be in the range of 8.0-11.0% by mass, preferably 8.5-10.5% by mass, and more preferably 9.0-10.0% by mass, wherein the mass % is based on the total mass of TPO excluding water and ash content. The total hydrogen is determined according to ASTM D5291C-21.
[0163] According to the present invention, the C / H atomic ratio of TPO can be at least 0.65, such as at least 0.70, or at least 0.75. The C / H atomic ratio of TPO can be less than 1.0, such as less than 0.95, or less than 0.90, or less than 0.85, or less than 0.80. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the C / H atomic ratio of TPO can be in the range of 0.65-1.0, preferably 0.70-0.90, and more preferably 0.70-0.85. The C / H atomic ratio is calculated based on the total carbon and total hydrogen determined according to ASTM D5291C-21 as described above.
[0164] TPO can have:
[0165] Total carbon in the range of 85.0-90.0 mass %, preferably 86.0-90.0 mass %, more preferably 87.0-90.0 mass %;
[0166] Total hydrogen in the range of 8.0-11.0 mass %, preferably 8.5-10.5 mass %, more preferably 9.0-10.0 mass %; and
[0167] a C / H atomic ratio in the range of 0.65-1.0, preferably 0.70-0.90, more preferably 0.70-0.85;
[0168] Wherein, mass % is based on the total mass of TPO excluding water and ash content. The water content can be measured according to ASTM D4928-12R18, and the ash content can be measured according to ASTM D2415-20 (at 550°C). The total carbon and total hydrogen are measured according to ASTM D5291C-21. The C / H atomic ratio is calculated based on the total carbon and total hydrogen.
[0169] According to the present invention, the total nitrogen of TPO can be at least 0.40% by mass, such as at least 0.45% by mass, or at least 0.50% by mass, wherein the mass % is based on the total mass of TPO excluding water and ash content. The moisture content can be determined according to ASTM D4928-12R18, and the ash content can be determined according to ASTM D2415-20 (at 550° C.). The total nitrogen of TPO can be 0.65% by mass or less, such as 0.60% by mass or less, or 0.55% by mass or less, wherein the mass % is based on the total mass of TPO excluding water and ash content. Those skilled in the art will understand that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the total nitrogen of TPO can be in the range of 0.40-0.65% by mass, preferably 0.45-0.65% by mass, and more preferably 0.45-0.60% by mass, wherein the mass % is based on the total mass of TPO excluding water and ash content. Total nitrogen is determined according to ASTM D5291C-21.
[0170] According to the present invention, the total sulfur of TPO can be at most 1.35 mass%, such as at most 1.30 mass%, or at most 1.25 mass%, or at most 1.20 mass%, or at most 1.15 mass%, or at most 1.10 mass%, wherein the mass% is based on the total mass of TPO excluding water and ash content. The moisture content can be measured according to ASTM D4928-12R18, and the ash content can be measured according to ASTM D2415-20 (at 550°C). The total sulfur is measured according to ASTM D5291C-21.
[0171] TPO can have:
[0172] 0.40-0.65 mass %, preferably 0.45-0.65 mass %, more preferably 0.45-0.60 mass % of total nitrogen; and
[0173] Up to 1.35 mass %, preferably up to 1.25 mass %, more preferably up to 1.20 mass % total sulfur;
[0174] Wherein, mass % is based on the total mass of TPO excluding water and ash content. The water content can be measured according to ASTM D4928-12R18, and the ash content can be measured according to ASTM D2415-20 (at 550°C). Total nitrogen and total sulfur are measured according to ASTM D5291C-21.
[0175] According to the present invention, TPO may have:
[0176] Total carbon in the range of 85.0-90.0 mass %, preferably 86.0-90.0 mass %, more preferably 87.0-90.0 mass %;
[0177] Total hydrogen in the range of 8.0-11.0 mass %, preferably 8.5-10.5 mass %, more preferably 9.0-10.0 mass %;
[0178] a C / H atomic ratio in the range of 0.65-1.0, preferably 0.70-0.90, more preferably 0.70-0.85;
[0179] 0.40-0.65 mass %, preferably 0.45-0.65 mass %, more preferably 0.45-0.60 mass % of total nitrogen; and
[0180] Up to 1.35 mass %, preferably up to 1.25 mass %, more preferably 0.90-1.20 mass % total sulfur;
[0181] Wherein, mass % is based on the total mass of TPO excluding water and ash content. The water content can be measured according to ASTM D4928-12R18, and the ash content can be measured according to ASTM D2415-20 (at 550°C). The total carbon, total hydrogen, total nitrogen and total sulfur are measured according to ASTM D5291C-21. The C / H atomic ratio is calculated based on the total carbon and total hydrogen.
[0182] According to the present invention, the ash content of TPO can be less than 0.04 mass%, such as less than 0.03 mass%, or less than 0.02 mass%, or less than 0.01 mass%, wherein the mass% is based on the total mass of TPO. The ash content is measured according to ASTM D2415-20 (at 550°C).
[0183] The sieve residue of TPO may be 250 mg / kg or less, for example 230 mg / kg or less, based on the total weight of TPO. The sieve residue is measured according to ASTM D4870-18 (25 μm mesh size).
[0184] According to the present invention, the renewable carbon black raw material (a) may include a plant-based raw material. The plant-based raw material may be a waste plant-based raw material. The term "waste" refers to a material that is discarded or disposed of because it is unsuitable or no longer used for its intended purpose (e.g., after use).
[0185] The renewable carbon black feedstock may include a solid component and / or a liquid component. Preferably, the renewable carbon black feedstock may include a liquid component.
[0186] The renewable carbon black feedstock may preferably include plant-based oils, more preferably waste plant-based oils.
[0187] The renewable carbon black feedstock (a) may include wood, grass, cellulose, hemicellulose, lignin, black liquor, tall oil, rubber seed oil, tobacco seed oil, castor oil, pongamia oil, crambe oil, neem oil, apricot kernel oil, rice bran oil, cashew nut shell liquid, cyperus culentus oil, rice bran oil, rapeseed oil, linseed oil, palm oil, coconut oil, canola oil, soybean oil, sunflower seed oil, cottonseed oil, pine nut oil, olive oil, corn oil, grape seed oil, safflower oil, acai palm oil, stinky bean oil, sesame oil, chia seed oil, hemp seed oil, perilla oil, peanut oil, stillingia oil, etc. oil), cashew oil, Brazil nut oil, macadamia oil, walnut oil, almond oil, hazelnut oil, beechnut oil, candlenut oil, chestnut oil, or a mixture or combination of any of the foregoing.
[0188] Preferably, the renewable carbon black feedstock (a) comprises soybean oil, rapeseed oil or a mixture or combination of any of the foregoing. According to the present invention, the renewable carbon black feedstock (a) may comprise rapeseed oil.
[0189] As used herein, the term "wood" refers to the porous and fibrous structural tissue found in the stems and roots of trees and other woody plants. Suitable examples of wood include, but are not limited to, pine, spruce, larch, juniper, ash, hornbeam, birch, alder, beech, oak, pine, chestnut, mulberry, or mixtures thereof. Suitable examples of grass include, but are not limited to, cereal grasses, such as corn, wheat, rice, barley, or millet; bamboo and natural grassland grasses and species cultivated in lawns and pastures. Suitable examples of lignin may include, but are not limited to, lignin removed by Kraft process and lignin sulfonates.
[0190] The ratio of the renewable carbon black raw material (a) to the rubber-derived pyrolysis oil (b) in the carbon black raw material may be 0.1:1 to 1:0.1, preferably 0.3:1 to 1:0.3. According to the present invention, the ratio of the renewable carbon black raw material (a) to the rubber-derived pyrolysis oil (b) in the carbon black raw material may be 0.5:1 to 1:0.5.
[0191] According to the present invention, based on the gross weight of the carbon black raw material, the carbon black raw material may include at least 10 weight %, such as at least 15 weight %, or at least 20 weight %, or at least 25 weight %, or at least 30 weight %, or at least 35 weight %, or at least 40 weight %, or at least 45 weight % of renewable carbon black raw material (a). Based on the gross weight of the carbon black raw material, the carbon black raw material of the present invention may include less than 90 weight %, such as less than 85 weight %, or less than 80 weight %, or less than 75 weight %, or less than 70 weight %, or less than 65 weight %, or less than 60 weight %, or less than 55 weight % of renewable carbon black raw material (a). It will be appreciated by those skilled in the art that any range between any clearly disclosed lower and upper limits is disclosed herein. Therefore, based on the gross weight of the carbon black raw material, the carbon black raw material may include 10-90 weight %, preferably 20-80 weight %, more preferably 40-60 weight %, and most preferably 45-55 weight % of renewable carbon black raw material (a).
[0192] According to the present invention, the carbon black feedstock may contain at least 10 wt%, such as at least 15 wt%, or at least 20 wt%, or at least 25 wt%, or at least 30 wt%, or at least 35 wt%, or at least 40 wt%, or at least 45 wt% of rubber-derived pyrolysis oil (b), based on the total weight of the carbon black feedstock. The carbon black feedstock of the present invention may contain 90 wt% or less, such as 85 wt% or less, or 80 wt% or less, or 75 wt% or less, or 70 wt% or less, or 65 wt% or less, or 60 wt% or less, or 55 wt% or less of rubber-derived pyrolysis oil (b), based on the total weight of the carbon black feedstock. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the carbon black feedstock may contain 10-90 wt%, preferably 20-80 wt%, more preferably 40-60 wt%, and most preferably 45-55 wt% of rubber-derived pyrolysis oil (b), based on the total weight of the carbon black feedstock.
[0193] The carbon black feedstock may include 20-80 wt %, preferably 25-75 wt %, more preferably 40-60 wt % of renewable carbon black feedstock (a), and 20-80 wt %, preferably 25-75 wt %, more preferably 40-60 wt % of rubber derived pyrolysis oil (b), based on the total weight of the carbon black feedstock. Preferably, the carbon black feedstock may include 45-55 wt % of renewable carbon black feedstock (a) and 45-55 wt % of rubber derived pyrolysis oil (b), based on the total weight of the carbon black feedstock.
[0194] The method of the present invention may include: inputting an O2-containing gas stream and a fuel stream containing a combustible substance into a reactor; burning the combustible substance in a combustion step to provide a combustion gas stream, wherein the O2-containing gas stream and the fuel stream containing the combustible substance are provided to the combustion step in an amount corresponding to a k factor in the range of 0.5-1.0, wherein the k factor is the ratio of the O2 theoretically required for the stoichiometric combustion of all the combustible substances in the combustion step to the total O2 provided for the combustion step; contacting the carbon black feedstock with the combustion gas stream in a reaction step to form carbon black; and terminating the carbon black forming reaction in a termination step;
[0195] The k factor is the ratio of the theoretically required O2 for stoichiometric combustion of all combustible materials in the combustion step to the total O2 provided for the combustion step. Thus, a k factor of 1 indicates stoichiometric combustion. In the case of excess oxygen, the k factor is less than 1.
[0196] According to the present invention, the fuel stream can be any combustible material. The fuel stream preferably includes liquid and / or gaseous hydrocarbons, hydrogen, carbon monoxide or mixtures thereof. The fuel stream may contain at least 50% by weight, such as at least 70% by weight, such as at least 90% by weight, such as at least 95% by weight of hydrocarbons. Suitable examples of fuel streams include, but are not limited to, natural gas, coal gas, petroleum gas, petroleum liquid fuels such as heavy oil, or coal-derived liquid fuels (coil derived liquid fuel, such as creosote, fuel oil, wash oil, anthracene oil and crude coal tar). Preferably, the fuel stream includes natural gas. Alternatively, the fuel stream may include plasma gas. The fuel stream is burned in the combustion step to provide a combustion gas stream.
[0197] As the O2-containing gas stream, any oxygen-containing gas stream can be used. Suitable examples of the O2-containing gas stream include, but are not limited to, air, oxygen-reduced air, and oxygen-enriched air.
[0198] The combustion may be carried out at a temperature in the range of 1,000-2,700°C, preferably 1,200-2,400°C, more preferably 1,300-2,300°C.
[0199] According to the present invention, the k factor may further range from 0.6 to 1.0, preferably from 0.7 to 1.0, more preferably from 0.75 to 1.0, and even more preferably from 0.8 to 1.0. Those skilled in the art will appreciate that the k factor may be easily calculated based on the content and type of combustible material, the O content in the feed stream and their respective flow rates.
[0200] In the method of the present invention, the combustion gas generated in the combustion step can be contacted with the carbon black raw material of the present invention in the reaction step. In the reaction step, the carbon black raw material undergoes pyrolysis or cracking to form carbon black and tail gas.
[0201] The formation of carbon black may be carried out in a temperature range of 1,000-2,000°C, preferably 1,100-1,900°C, more preferably 1,300-1,900°C, most preferably 1,300-1,800°C.
[0202] According to the present invention, the formation of carbon black can be terminated in a termination step. The termination of the formation of carbon black can be achieved by any means known to those skilled in the art, such as by direct or indirect heat exchange cooling, such as by using a quench boiler and / or by quenching. Quenching is usually achieved by injecting a suitable quenching liquid (e.g. water). Preferably, the formation of carbon black is terminated by water quenching.
[0203] According to the present invention, the method can be carried out in a furnace black reactor, including generating a combustion gas flow in a combustion zone, and passing the combustion gas from the combustion zone through a reaction zone into a termination zone, injecting a carbon black feedstock into the combustion gas in the reaction zone to form carbon black, and terminating the carbon black formation in the termination zone by quenching and / or lowering the temperature using a quenching boiler. The furnace black reactor of the present invention can be provided with a combustion zone, a reaction zone and a termination zone along the reactor axis. A suitable furnace black reactor is, for example, described in EP2479223A1 or EP1233042A2.
[0204] The present invention also relates to carbon black obtained by the above-mentioned method of the present invention.
[0205] According to the present invention, the carbon black of the present invention may have an oil absorption number (OAN) equal to or greater than 70 mL / 100 g, such as equal to or greater than 80 mL / 100 g. The carbon black of the present invention may have an oil absorption number (OAN) of less than 150 mL / 100 g, such as less than 145 mL / 100 g, or less than 140 mL / 100 g, or less than 135 mL / 100 g, or less than 130 mL / 100 g. The carbon black according to the present invention may have an OAN within a range between any of the lower and upper values recited. The carbon black may have an oil absorption number in the range of 70-145 mL / 100 g, preferably 80-130 mL / 100 g. OAN is determined according to ASTM D2414-21.
[0206] According to the present invention, the difference (gap) between the OAN and COAN of carbon black (OAN-COAN) can be at least 10mL / 100g, such as at least 12mL / 100g, or at least 15mL / 100g, or at least 20mL / 100g. The difference (gap) between the OAN and COAN of carbon black (OAN-COAN) can be 50mL / 100g or less, such as 45mL / 100g or less, or 40mL / 100g or less, or 35mL / 100g or less, or 30mL / 100g or less. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the difference (gap) between the OAN and COAN of carbon black (OAN-COAN) can be in the range of 10-45mL / 100g, preferably 12-35mL / 100g, and more preferably 12-30mL / 100g. OAN is measured according to ASTM D2414-21, and COAN is measured according to ASTM D3493-21. The difference within the range can make the carbon black have good dispersibility in the composition, especially in the rubber and / or plastic composition.
[0207] According to the present invention, the statistical adsorption layer thickness surface area (STSA) of carbon black may be not greater than or equal to 90 m 2 / g, for example, not greater than or equal to 85m 2 / g. The STSA of carbon black may be at least 20m 2 / g, for example at least 23m 2 / g, or at least 25m 2 / g. Those skilled in the art will appreciate that any range between any explicitly disclosed lower and upper limits is disclosed herein. Thus, the STSA of carbon black may be in the range of 20-90 m 2 / g, preferably 23-90m 2 / g, more preferably 25-85m 2 / g range. STSA is measured according to ASTM D6556-19a. Low STSA can provide low rolling resistance and low heat build-up.
[0208] The BET specific surface area of the carbon black of the present invention may be at least 20 m 2 / g, for example at least 23m 2 / g, or at least 25m 2 / g. The BET specific surface area of carbon black can be 120m 2 / g or less, for example 110m 2 / g or less or 100m 2 / g or less. Those skilled in the art will appreciate that any range between any explicitly disclosed lower and upper limits is disclosed herein. Thus, the BET specific surface area of carbon black may be in the range of 20-120 m2 / g, preferably 23-110m 2 / g, more preferably 25-100m 2 The BET specific surface area is measured according to ASTM D6556-19a.
[0209] According to the present invention, the sulfur content of carbon black may be no more than 2.5%, preferably no more than 2.0%, more preferably no more than 1.5%. The sulfur content is determined according to ASTM D1619-20.
[0210] The pMC (percentage of modern carbon) of the carbon black of the present invention can be 30% or more, such as 32% or more, or 35% or more, or 37% or more, or 40% or more, or 42% or more, or 45% or more, or 47% or more, or 50% or more, or 52% or more, or 55% or more, or 57% or more, or 60% or more, or 62% or more, or 65% or more, or 67% or more, or 70% or more, or 72% or more, or 75% or more, or 77% or more, or 80% or more, or 82% or more, or 85% or more, or 87% or more, or 90% or more, or 92% or more, or 95% or more, or 97% or more, or 99% or more. The pMC is determined according to ASTM D6866-20 Method B (AMS). Calculate the pMC of each sample. 14 C / 13 C ratio and compared with the measured value of oxalic acid II standard (NIST-4990C). The measured value (pMC) is corrected by d13C measured by isotope ratio mass spectrometer (IRMS). The pMC (percentage of modern carbon) of the carbon black of the present invention can be 30% or more, preferably 40% or more, more preferably 50% or more, even more preferably 75% or more, and most preferably 90% or more.
[0211] According to the present invention, the carbon black may be furnace black.
[0212] According to the present invention, carbon black can be oxidized. In this article, the term "oxidation" refers to that carbon black is oxidized and therefore contains oxygen-containing functional groups. Therefore, unlike non-oxidized carbon black, oxidized carbon black generally has a significant oxygen content and has oxygen-containing functional groups, such as, but not limited to, quinone groups, carboxyl groups, phenolic groups, lactol groups, lactone groups, anhydride groups, and ketone groups. For example, based on the gross weight of the oxidized carbon black material, the oxygen content of the oxidized carbon black can be more than 0.5 wt %, such as more than 1 wt % or more than 2 wt %. Typically, the oxygen content is no more than 20 wt % based on the gross weight of the oxidized carbon black material. For example, based on the gross weight of the oxidized carbon black material, the oxidized carbon black can contain 0.5-20 wt %, or 1-15 wt %, or 2-10 wt %, or 2-5 wt % of oxygen.
[0213] Oxidized carbon black can be produced by various methods known in the art, such as those disclosed in US Pat. No. 6,120,594 and US Pat. No. 6,471,933. Suitable methods include oxidizing the carbon black material with an oxidant such as a peroxide, such as hydrogen peroxide; a persulfate, such as sodium persulfate and potassium persulfate; a hypohalite, such as sodium hypochlorite; ozone or oxygen; a transition metal-containing oxidant, such as permanganate, osmium tetroxide, chromium oxide, cerium ammonium nitrate; or an oxidizing acid, such as nitric acid or perchloric acid; and mixtures or combinations thereof.
[0214] According to the present invention, carbon black can also be further functionalized. Carbon black can be functionalized by treatment with a functionalizing agent. As described in WO2021 / 001156A1, functionalized carbon black can be obtained, for example, by treating oxidized carbon black with a sulfur-containing primary or secondary amine or a salt thereof. Thus, the treatment chemically changes the oxidized carbon black by the sulfur-containing amine, which imparts functional groups (e.g., sulfur-containing moieties and / or amine groups) from the treating agent to the oxidized carbon black.
[0215] The invention also relates to the use of the carbon black according to the invention as reinforcing filler or additive, UV stabilizer, conductive carbon black or pigment, preferably as reinforcing filler or additive.
[0216] The invention further relates to the use of the carbon black according to the invention in rubber and rubber mixtures, plastics, inks (e.g. printing inks, inkjet inks or other inks), toners, paints, coatings, paper, adhesives, batteries or black matrix applications, preferably in rubber and rubber mixtures or plastics.
[0217] In addition, the present invention relates to a rubber composition. The rubber composition of the present invention comprises at least one rubber material and at least one carbon black according to the present invention. Unless otherwise specified, the terms "rubber", "rubber material" and "elastomer" can be used interchangeably in this specification. According to the present invention, the rubber that can be used includes rubber containing olefin unsaturation, i.e., diene-based rubber materials, and non-diene-based rubber materials. The term "diene-based rubber material" is intended to include natural rubber and synthetic rubber or mixtures thereof.
[0218] Natural rubber can be used in unprocessed form or in a processed form commonly used in various rubber processing technologies. For example, natural rubber can be obtained from rubber trees (Helvea brasiliensis), guayule and dandelions.
[0219] Synthetic rubber can include styrene butadiene rubber, for example emulsion polystyrene butadiene rubber and solution polystyrene butadiene rubber, polybutadiene, polyisoprene, EPDM, EPDM, butyl rubber, halogenated butyl rubber, chlorinated polyethylene, chlorosulfonated polyethylene, acrylonitrile-butadiene rubber, hydrogenated acrylonitrile-butadiene rubber, chloroprene rubber, acrylate rubber, ethylene-vinyl acetate rubber, ethylene-acrylic acid rubber, epichlorohydrin rubber, silicone rubber, fluorosilicone rubber, fluorocarbon rubber or the mixture of the combination of above-mentioned arbitrary rubber.According to the present invention, synthetic rubber can also be obtained from renewable materials.For example, polybutadiene can be produced by the alcohol (alcohol) obtained by plant biomass fermentation.
[0220] Suitable rubber can also include functionalized rubber and rubber coupled with silicon or tin. For example, the rubber can be functionalized with functional groups such as amine, alkoxy, silyl, mercaptan, thioester, thioether, thiol, sulfanyl, sulfhydryl, sulfide or their combination. One or more functional groups can be primary, secondary or tertiary functional groups, can be located at one or both ends of the chain (such as α, ω-functionalization), can also be suspended from the polymer backbone and / or provided in the polymer backbone chain. The rubber according to the present invention can also be partially cross-linked. Therefore, before being used for the composition of the present invention, the partial polymer chains of the rubber material can be cross-linked by a coupling agent or not by a coupling agent.
[0221] Composition according to the present invention can be especially curable composition (curable composition), for example vulcanizable rubber composition (vulcanizable rubber composition).Term " vulcanizable rubber composition " refers to the composition of various other components commonly used in rubber component and optional rubber mixing field, and it can be cured by vulcanization when forming vulcanized rubber (vulcanizate).Unless otherwise indicated, the terms "curable (curable)" and "vulcanizable (vulcanizable)" are used interchangeably in this specification, referring to the chemical reaction that polymer chains are interconnected by crosslinking agent or vulcanizing agent.Curing reaction can be induced by any method known in the art, such as light, moisture (moisture), heat and / or adding crosslinking agent.
[0222] The rubber material may include more than 5 phr of natural rubber, for example, more than 10 phr, or more than 15 phr, or more than 20 phr, or more than 30 phr, or more than 40 phr, or more than 50 phr, or more than 60 phr, or more than 70 phr, or more than 80 phr of natural rubber. As used herein, the term "phr" refers to the weight parts of the corresponding material recorded in every 100 parts by weight of rubber or elastomer. The rubber material may include less than 100 phr of natural rubber, for example, less than 95 phr, or less than 90 phr, or less than 85 phr, or less than 80 phr, or less than 75 phr, or less than 70 phr, or less than 65 phr, or less than 60 phr of natural rubber. The rubber material may include natural rubber in a range between any lower and upper limits recorded. For example, the rubber material may contain natural rubber in the range of 5-95 phr, such as in the range of 10-90 phr, or in the range of 20-80 phr, or in the range of 30-70 phr, or in the range of 40-60 phr.According to the present invention, the rubber material may consist of natural rubber.
[0223] The rubber material may contain more than 5 phr of synthetic rubber, such as more than 10 phr, or more than 15 phr, or more than 20 phr, or more than 30 phr, or more than 40 phr, or more than 50 phr, or more than 60 phr, or more than 70 phr, or more than 80 phr of synthetic rubber. The rubber material may contain less than 100 phr of synthetic rubber, such as less than 95 phr, or less than 90 phr, or less than 85 phr, or less than 80 phr, or less than 75 phr, or less than 70 phr, or less than 65 phr, or less than 60 phr of synthetic rubber. The rubber material may include synthetic rubber in a range between any lower and upper limits described. For example, the rubber material may include synthetic rubber in the range of 5-95 phr, such as in the range of 10-90 phr, or in the range of 20-80 phr, or in the range of 30-70 phr, or in the range of 40-60 phr. According to the present invention, the rubber material may be composed of synthetic rubber.
[0224] The rubber material may include 5-100 phr of natural rubber and 5-100 phr of synthetic rubber, for example, 10-90 phr of natural rubber and 10-90 phr of synthetic rubber, or 20-80 phr of natural rubber and 20-80 phr of synthetic rubber, or 30-70 phr of natural rubber and 30-70 phr of synthetic rubber, or 40-60 phr of natural rubber and 40-60 phr of synthetic rubber, or 40-100 phr of natural rubber and 5-60 phr of synthetic rubber, or 50-95 phr of natural rubber and 5-50 phr of synthetic rubber, or 60-90 phr of natural rubber and 10-50 phr of synthetic rubber, or 5-40 phr of natural rubber and 60-100 phr of synthetic rubber, or 10-20 phr of natural rubber and 80-90 phr of synthetic rubber.
[0225] The rubber composition according to the present invention can include the carbon black of the present invention in an amount of more than 3 phr, such as more than 5 phr, or more than 10 phr, more than 15 phr, more than 20 phr, more than 25 phr, more than 30 phr, more than 40 phr, or more than 50 phr. As used herein, the term "phr" refers to the weight percentage of the corresponding material recorded in every 100 parts by weight of rubber or elastomer. The rubber composition can include the carbon black of the present invention in an amount of less than 200 phr, such as less than 190 phr, or less than 180 phr, or less than 150 phr, or less than 130 phr, or less than 110 phr, or less than 100 phr. The rubber composition according to the present invention can include the carbon black of the present invention in an amount between any lower limit and upper limit recorded. For example, the rubber composition according to the present invention can include the carbon black of the present invention in an amount of 3-200 phr, such as 5-190 phr, or 10-150 phr, or 20-130 phr, or 30-100 phr.
[0226] Rubber composition according to the present invention can also include at least one vulcanizing agent.Possible vulcanizing agent includes any vulcanizing agent known in the art such as sulphur and sulphur donor.Suitable sulphur donors for the practice of the present invention include dithioalkanes, dicaprolactam sulfide, polymeric polysulfides, sulphur olefin adducts, thiurams and sulfonamides, for example, containing at least two sulphur atoms in the sulphur bridge.Preferably use elemental sulphur.The amount range of vulcanizing agent in the rubber composition according to the present invention is generally 0.5-10phr, for example 1-5phr.
[0227] The rubber composition according to the present invention may further comprise one or more other additives commonly used in the formulation field. For example, such additives include curing aids (such as primary vulcanization accelerators and secondary vulcanization accelerators, activators and pre-vulcanization inhibitors), processing additives (such as oil, wax, resin, plasticizer, softener or rheology modifier), pigment, peptizing agent (peptizing agent), coupling agent, surfactant, bactericide and antidegradant (such as heat stabilizer or light stabilizer, antioxidant and antiozonant). Those skilled in the art will select such optional additives and their relative dosages according to the required performance and / or purposes of the rubber composition. For example, guanidines, dicarbamates, dithiocarbamates, thiurams, thioureas, 2-mercaptobenzothiazole, benzothiazole sulfonamides, aldehydeamines, amines, disulfides, thiazoles, xanthates and sulfenamides can be used as primary vulcanization accelerators and secondary vulcanization accelerators. As a specific example, for example, N-tert-butyl-2-benzothiazyl sulfenamide can be purchased from Rhein Chemie Additives under the trade name Rhenogran TBBS-80. Suitable vulcanization activators that can be used for rubber composition of the present invention include combinations such as zinc oxide, etc., and fatty acids such as stearic acid, lauric acid, palmitic acid, oleic acid or naphthenic acid. If used, such activators are generally used in amounts of 1 to 10 phr, such as 2 to 5 phr.
[0228] Other additives may include metal oxides, metal hydroxides and filler materials, for example metal oxides, metal hydroxides and filler materials, such as silica, preferably precipitated silica and fumed silica, organic silica, carbon nanotubes, carbon fibers, graphite and metal fibers and organosilanes, such as bis(trialkoxysilylalkyl) oligo- or polysulfides.
[0229] Rubber composition of the present invention can be obtained and processed by common rubber processing technology.For example, can be by carbon black of the present invention and any optional component (if used) and rubber material combination and mix them, for example carbon black and any optional component (if used) are dispersed in rubber material, thereby obtain rubber composition according to the present invention.Dispersion can be realized by any method known in the art, for example mixing, stirring, grinding, kneading, ultrasound, dissolver, vibrating mixer, rotor-stator dispersion assembly or high pressure homogenizer or their combination.For example, can use the laboratory mixer with meshing rotor geometry (intermeshing rotor geometry) shape. For example, according to the procedure described in A. Wehmeier, "Filler Dispersion Analysis by Topography Measurements", Technical Report TR 820, Degussa GmbH and A. Wehmeier, "Entwicklung eines Verfahrens zur Charakterisierung der Fuellstoff dispersion in Gummimischungen mittels einer Oberflaechen topographie", thesis, 1998 at the Muenster University of Applied Sciences and DE 199 17 975 C2, dispersion can be carried out, for example, until the carbon black is uniformly dispersed in the rubber material, so that the dispersion index determined by the surface topography including Medalia correction is below 8%, preferably below 5%. The dispersion index obtained according to this method generally has a good correlation (for example a coefficient of determination greater than 0.95) with the dispersion index determined by optical methods (for example the dispersion index determined according to test method B of ASTM D2663-14).
[0230] For example, a multi-step process can be used to prepare a rubber composition according to the present invention: first, carbon black and optional non-curative additives (non-curative additives) (if used) can be added to the rubber material simultaneously or successively. Then, the rubber material, carbon black and additives (if used) can be mixed, usually at a temperature in the range of 40° C. to 160° C., with a total mixing time of less than 10 minutes, for example, in the range of 2-8 minutes. Subsequently, at a temperature below 115° C., the obtained mixture can be mixed with one or more curing additives for less than 5 minutes, usually less than 3 minutes, preferably about 2.5 minutes.
[0231] The method may include other steps, such as extrusion or cooling the product to room temperature and storing it for further processing. The method may also include a curing step, for example, the rubber composition may be placed under heat curing conditions, such as curing at a temperature of 120-200° C. for 5 minutes to 3 hours. For example, curing may be performed in a curing press at a temperature of 140-180° C. and a pressure between 100-150 bar for 5-60 minutes.
[0232] As will be appreciated, the rubber composition according to the present invention can be used in various technical applications of polymer-based materials that need to contain carbon black fillers, such as for imparting antistatic or conductive properties, color, mechanical reinforcement and / or low hysteresis properties. Particularly when producing tires, the mechanical properties of concern include tear resistance, resilience and hysteresis. The cured composition provided by the rubber composition according to the present invention has good and useful mechanical properties, and is particularly suitable for tire production. According to the present invention, useful mechanical properties are such as high tensile strength, high resilience and low hysteresis. The cured composition provided by the rubber composition according to the present invention has mechanical properties comparable to the rubber composition comprising conventional carbon black.
[0233] The present invention relates to the use of a rubber composition according to the invention for producing a tire, preferably a pneumatic tire, a tire tread, a belt, a belt reinforcement, a carcass, a carcass reinforcement, a sidewall, an inner liner, an apex, a shoulder, a hump strip, a chafer, a bead filler, a cable sheath, a tube, a drive belt, a conveyor belt, a roller covering, a shoe sole, a hose, a seal, a profile, a damping element, a coating or a colored or printed article.
[0234] Therefore, the present invention also relates to a tire made of the above-mentioned rubber composition according to the present invention or a tire comprising the rubber composition. The tire according to the present invention may include a tire tread, a belt, a belt reinforcement, a carcass, a carcass reinforcement, a sidewall, an inner liner, an apex, a shoulder, a hump strip, a chafer and a bead filler, wherein at least one of the above-mentioned components is made of the rubber composition according to the present invention or comprises the rubber composition according to the present invention. Such tires include, for example, but are not limited to, truck tires, passenger car tires, off-road tires, aircraft tires, agricultural tires and earth-moving machinery tires.
[0235] Preferably, the tire has a circumferential tread of a cap / base configuration, which includes a circumferential outer tread cap rubber layer comprising the running surface of the tire, and a tread base rubber layer at least partially covering the tread cap rubber layer, wherein at least one of the tread cap rubber layer and the tread base rubber layer is made of or comprises a rubber composition according to the present invention.
[0236] The invention also relates to an article made from or comprising the rubber composition according to the invention, which article is a cable sheath, a pipe, a transmission belt, a conveyor belt, a roller covering, a shoe sole, a hose, a seal, a profile, a damping element, a coating or a colored or printed article.
[0237] The present invention also relates to a plastic composition comprising at least one plastic material and at least one carbon black according to the present invention.
[0238] The at least one plastic material comprises a thermoplastic polymer, a thermosetting polymer, a thermoplastic elastomer, preferably low-density and high-density polyethylene and polypropylene, polyvinyl chloride, melamine-formaldehyde resins, phenolic resins, epoxy resins, polyamides, polyesters, polyoxymethylene, polymethyl methacrylate, polycarbonates, polystyrenes, polyurethanes, polyphenylene oxides, polysiloxanes, polyacrylamides, polyaryletherketones, polysulfones, polyetherimides, acrylonitrile-styrene-acrylates or acrylonitrile-butadiene-styrene polymers, and mixtures or copolymers of any of the above substances. BRIEF DESCRIPTION OF THE DRAWINGS
[0239] Figure 1 (Not to scale) shows a schematic cross-sectional view of a furnace carbon black reactor.
[0240] Example
[0241] The following examples will further illustrate the present invention. Unless otherwise specified, all parts and percentages mentioned herein are on a weight basis.
[0242] Carbon Black Production
[0243] A furnace carbon black reactor was used to produce the carbon black according to the invention. Rapeseed oil purchased from UCY Energy Group (Germany) was used as a renewable carbon black feedstock. ThermoTireOil RR (available from PyrumInnovations AG (Germany)) was used as a rubber derived pyrolysis oil. ThermoTireOil RR was fractionated. A ThermoTireOil RR distillation fraction having a flash point of at least 65° C. was used. The flash point was determined according to ASTM D93B.
[0244] The carbon black raw materials in Table 1 are used to produce carbon black.
[0245] Table 1:
[0246]
[0247] The carbon black feedstock in Examples 2-4 was circulated for 8 hours using a centrifugal pump to achieve uniform mixing.
[0248] use Figure 1 The furnace carbon black reactor shown produces a range of carbon blacks.
[0249] Figure 1 A longitudinal cross-section of a furnace carbon black reactor is shown. The reactor has a combustion chamber in which hot process gas for pyrolyzing the carbon black feedstock is produced by burning natural gas at a temperature of about 2,000°C with the introduction of atmospheric oxygen.
[0250] Combustion air and fuel are introduced through holes 1 at the end of the combustion chamber. The combustion chamber tapers in a conical manner toward the narrowest part. Carbon black feedstock is introduced into the narrowest part by means of a radial lance 3 from a nozzle and / or axially by means of a lance 2. After passing through the narrowest part, the reaction gas mixture expands into the reaction chamber.
[0251] In the termination zone, water is injected into the system via a quench-water lance 4.
[0252] The following table lists the dimensions of the reactor used (Table 2).
[0253] Table 2:
[0254]
[0255]
[0256] 1 Measure from the narrowest part of the entry (+: after entry, -: before entry)
[0257] Table 3 lists the reactor parameters used to produce the carbon black according to the present invention.
[0258] Table 3
[0259]
[0260] The carbon blacks in Examples 1 to 4 were wet-beaded according to the method described in EP 3960491 A1, paragraph
[0064] . The corresponding carbon black powder was introduced into a stationary batch mixer (so-called "Papenmeier", model GRP 625 / 1.0, available from Geppert Rührtechnik GmbH (Germany)). Deionized water was then slowly added under stirring (300 rpm) until the carbon black began to granulate, usually in a weight ratio of about 1:1, and the stirring speed was subsequently increased to 600-800 rpm. The mixture thus obtained was then homogenized in a roller block with a plastic barrel having a length of 600 mm and a diameter of 350 mm at 28 rpm for 10 minutes. The beaded material was then dried in an oven at 120° C. until the residual moisture content was <1%. The moisture content can be determined according to ASTM D1509-18.
[0261] The properties of the beaded carbon blacks of Examples 1-4 were measured and are listed in Table 4.
[0262] Table 4:
[0263]
[0264]
[0265] The carbon blacks in Examples 1 to 4 and the following commercially available carbon blacks (obtained using conventional raw materials) were used to prepare rubber compositions.
[0266] N326: STSA is about 77m 2 / g, OAN of about 72 mL / 100 g, and COAN of about 69 mL / 100 g, which can be purchased from Orion Engineered Carbons GmbH.
[0267] N330: STSA is about 76m2 / g, furnace black with OAN of about 102 mL / 100 g and COAN of about 88 mL / 100 g, which can be purchased from Orion Engineered Carbons GmbH.
[0268] The STSA, OAN and COAN of commercially available carbon blacks were determined as described in Table 4.
[0269] Preparation of rubber composition
[0270] The rubber composition of the formulation listed in Table 5 was prepared using the above carbon black according to the following procedure.
[0271] Table 5:
[0272] Element Amount (phr) <![CDATA[ESBR Buna SB 1500 1 ]]> 100 Carbon Black 50 ZnO 3 Stearic acid 2 <![CDATA[Vulkanox 4020 / LG 2 ]]> 1 sulfur 1.5 <![CDATA[Vulkacit CZ / EG-C 3 ]]> 1.5
[0273] 1 : ESBR rubber, available from Resinex Deutschland GmbH
[0274] 2: Antioxidant, available from Lanxess
[0275] 3: Vulcanization accelerator, available from Lanxess
[0276] ESBR Buna SB 1500 was introduced into a laboratory mixer GK4N with tangential rotor geometry manufactured by Harburg Freudenberger and milled for 30 seconds at a chamber temperature of 40°C and a rotor speed of 33 rpm. Subsequently, half of the carbon black, ZnO, stearic acid and Vulkanox 4020 / LG were added in the specified amounts under stirring and mixed for 9β seconds. The other half of the carbon black and Vulkanox 4020 / LG were then added to the agitator. After another 90 seconds, the ram was lifted and cleaned, and the batch was then mixed again for 90 seconds. After a total of 5 minutes, the batch was poured into an open mill for cooling and additional distribution mixing. In the first mixing step, the batch temperature did not exceed 160°C. In the second mixing step, sulfur and accelerator (Vulkacit CZ / EG-Z) were then added to the masterbatch obtained in the first mixing step in the specified amounts. The resulting mixture was milled in a GK4N mixer at a chamber temperature of 40° C. for 2 minutes. The rotor speed was 23 rpm, ensuring that the batch temperature did not exceed 105° C. Subsequently, the mixture was processed again on an open mill. The resulting vulcanizable component (green compound) was cured at a temperature of 160° C. for about 13 minutes.
[0277] The physical properties of the rubber composition thus prepared were analyzed according to the methods in Table 6 below.
[0278] Table 6:
[0279]
[0280] The results are summarized in Table 7 below.
[0281] Table 7:
[0282]
Claims
1. A method for producing carbon black by thermal oxidative pyrolysis or thermal cracking of a carbon black feedstock, wherein the carbon black feedstock comprises (a) a renewable carbon black feedstock and (b) a rubber-derived pyrolysis oil.
2. The method according to claim 1 or 2, wherein the rubber derived pyrolysis oil (b) comprises tire derived pyrolysis oil (TPO).
3. The method according to any one of the preceding claims, wherein the rubber derived pyrolysis oil (b) has: Total carbon in the range of 80.0-90.0 mass %; Total hydrogen in the range of 8.0-15.0 mass %; as well as C / H atomic ratio in the range of 0.60-1.0; in, The mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, wherein total carbon and total hydrogen are determined according to ASTM D5291C-21; and / or The rubber derived pyrolysis oil has: Up to 1.00 mass % total nitrogen; and Up to 1.35 mass % total sulfur, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21; and / or The tire derived pyrolysis oil (TPO) has: Total carbon in the range of 85.0-90.0 mass %; Total hydrogen in the range of 8.0-11.0 mass %; and C / H ratio in the range of 0.65-1.0; Wherein, mass % is based on the total mass of TPO excluding water and ash content, and wherein the total carbon and the total hydrogen are determined according to ASTM D5291C-21.
4. The method according to any one of the preceding claims, wherein the renewable carbon black feedstock (a) comprises a plant-based feedstock.
5. The method according to any one of the preceding claims, wherein the renewable carbon black feedstock (a) comprises wood, grass, cellulose, hemicellulose, lignin, black liquor, tall oil, rubber seed oil, tobacco seed oil, castor oil, karanja oil, crambe oil, neem oil, almond oil, rice bran oil, cashew nut shell liquid, cyperus oleifera oil, rice bran oil, rapeseed oil, linseed oil, palm oil, coconut oil, canola oil, soybean oil, sunflower seed oil, cottonseed oil, pine nut oil, olive oil, corn oil, grape seed oil, safflower oil, acai oil, petai oil, sesame oil, chia seed oil, hemp seed oil, perilla oil, peanut oil, Chinese tallow oil, cashew oil, Brazil nut oil, macadamia oil, walnut oil, almond oil, hazelnut oil, beech nut oil, candlenut oil, chestnut oil or a mixture or combination of any of the above, preferably soybean oil, rapeseed oil or a mixture or combination of any of the above, more preferably rapeseed oil.
6. The method according to any one of the preceding claims, wherein the carbon black feedstock has a ratio of the renewable carbon black feedstock (a) to the rubber derived pyrolysis oil of 0.1:1 to 1:0.1, preferably 0.3:1 to 1:0.3, more preferably 0.5:1 to 1:0.5; and / or The carbon black raw material comprises (a) 10-90 wt. %, preferably 20-80 wt. %, more preferably 40-60 wt. %, most preferably 45-55 wt. % of the renewable carbon black feedstock, based on the total weight of the carbon black feedstock; and / or (b) 10-90 wt %, preferably 20-80 wt %, more preferably 40-60 wt %, most preferably 45-55 wt % of the rubber derived pyrolysis oil, based on the total weight of the carbon black feedstock.
7. A method according to any one of the preceding claims, comprising: Inputting an O2-containing gas stream and a fuel stream containing a combustible substance into a reactor; combusting the combustible substance in a combustion step to provide a combustion gas stream, wherein the O2-containing gas stream and the fuel stream containing the combustible substance are provided to the combustion step in an amount corresponding to a k factor in the range of 0.5-1.0, wherein the k factor is the ratio of the O2 theoretically required for the stoichiometric combustion of all the combustible substances in the combustion step to the total O2 provided for the combustion step; contacting the carbon black feedstock with the combustion gas stream in a reaction step to form carbon black; and terminating the carbon black forming reaction in a termination step; wherein the k factor is preferably in the range of 0.6-1.0, more preferably 0.7-1.0, even more preferably 0.75-1.0, most preferably 0.8-1.0; and / or Wherein, the reaction is carried out in a furnace black reactor.
8. Carbon black obtainable by the process according to any one of the preceding claims.
9. The carbon black according to claim 8, wherein the carbon black has at least one, more than one or all of the following characteristics: Oil absorption number (OAN) equal to or greater than 70 mL / 100 g; The difference (gap) between OAN and COAN in the range of 10-45mL / 100g; Not more than or equal to 90m 2 / g of statistical adsorption layer thickness surface area (STSA); At 20-120m 2 BET specific surface area in the range of / g; and Percentage of modern carbon (pMC) above 30% Wherein OAN is measured according to ASTM D2414-21, COAN is measured according to ASTM D3493-21, STSA is measured according to ASTM D6556-19a, BET specific surface area is measured according to ASTM D6556-19a, and pMC is measured according to ASTM D6866-20 Method B (AMS).
10. Use of the carbon black according to any one of claims 8 to 9 as a reinforcing filler or additive, UV stabilizer, conductive carbon black or pigment, preferably as a reinforcing filler or additive.
11. Use of the carbon black according to any one of claims 8 to 9 in rubber and rubber mixtures, plastics, inks, such as printing inks, inkjet inks or other inks, toners, paints, coatings, paper, adhesives, batteries or black matrix applications, preferably in rubber and rubber mixtures or plastics.
12. A rubber composition comprising at least one rubber material and at least one carbon black according to any one of claims 8 to 9.
13. The rubber composition according to claim 12 is used for producing tires, preferably pneumatic tires, tire treads, belts, belt reinforcements, carcasses, carcass reinforcements, sidewalls, inner liners, apex strips, tire shoulders, peak strips, bead covers, bead cover rubber, cable sheaths, tubes, drive belts, conveyor belts, roller coverings, soles, hoses, seals, profiles, damping elements, coatings or colored or printed products.
14. A tire made from the rubber composition according to claim 12.
15. A plastic composition comprising at least one plastic material and at least one carbon black according to any one of claims 8 to 9.