Samarium-iron-nitrogen magnet powder and samarium-iron-nitrogen magnet
By adding lanthanides, bismuth and tungsten to the samarium-iron-nitrogen magnet powder, the samarium-iron-bismuth-tungsten-nitrogen magnet powder is solved, and high magnetization and high The effect of stubborn force.
Patent Information
- Application Number
- CN202280093762.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2022-12-21
- Publication Date
- 2024-11-05
AI Technical Summary
The magnetic characteristics of the existing samarium-iron-nitrogen-based magnet powders are reduced during the sintering process, especially the refractory force is greatly reduced, making it difficult to have both high magnetization and high refractory force.
Add lanthanides, bismuth and tungsten to the samarium-iron-nitrogen magnet powder to control the atomic ratio to form samarium-iron-bismuth-tungsten-nitrogen magnet powder, and improve the magnetization of the magnet powder through reduction diffusion and nitriding treatment. and stubborn force.
It significantly improves the magnetization and refractory force of magnet powder, maintains high magnetization and enhances refractory force, and is suitable for the manufacturing of high-performance magnets.
Smart Images

Figure BDA0005046537340000151 
Figure BDA0005046537340000171 
Figure HDA0005046537350000011
Abstract
Description
Technical Field
[0001] The present invention relates to samarium-iron-nitrogen magnet powder and samarium-iron-nitrogen magnet. Background Art
[0002] Sm-Fe-N magnets are expected to be high-performance magnets because of their high Curie temperature of 477°C, small temperature variation of magnetic properties, and high anisotropic magnetic field of 260 kOe, which is considered to be the theoretical value of coercive force.
[0003] In order to manufacture high-performance magnets, it is necessary to sinter samarium-iron-nitrogen based magnet powder.
[0004] However, the samarium-iron-nitrogen magnet powder has a problem of deteriorating its magnetic properties when sintered at high temperatures. In particular, the coercive force of the samarium-iron-nitrogen magnet is greatly reduced by the sintering process.
[0005] In order to solve such a problem, Patent Document 1 discloses adding bismuth to samarium-iron-nitrogen magnet powder. That is, Patent Document 1 discloses that the coercive force of magnet powder can be increased by using samarium-iron-bismuth-nitrogen magnet powder.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2020-57779 Summary of the invention
[0009] Problems to be solved by the invention
[0010] Generally speaking, coercivity and magnetization are in a trade-off relationship, and it is difficult to improve both. For example, according to the inventors of the present application, the samarium-iron-bismuth-nitrogen magnet powder described in Patent Document 1 shows high coercivity, but it is difficult to say that the magnetization is sufficient.
[0011] Under such circumstances, there is a demand for samarium-iron-nitrogen-based magnet powder having both high magnetization and high coercivity.
[0012] The present invention has been made in view of such background, and an object of the present invention is to provide a samarium-iron-nitrogen magnet powder having both high magnetization and high coercivity. In addition, an object of the present invention is to provide a samarium-iron-nitrogen magnet having both high magnetization and high coercivity.
[0013] Methods for solving problems
[0014] The present invention provides a samarium-iron-nitrogen magnet powder, comprising:
[0015] Lanthanide (Ln), iron (Fe), bismuth (Bi), tungsten (W) and nitrogen (N),
[0016] The above lanthanoid elements include samarium (Sm),
[0017] The ratio of bismuth to the sum of lanthanide elements + iron + bismuth + tungsten ((Bi / (Ln+Fe+Bi+W))) is 1.00 at% or less in terms of atomic ratio.
[0018] In terms of atomic ratio, the ratio of tungsten to the sum of lanthanide elements + iron + bismuth + tungsten ((W / (Ln+Fe+Bi+W))) is 0.05 at% or more and 0.60 at% or less,
[0019] The ratio of tungsten to bismuth (W / Bi) is 1.0 to 30.0 in atomic ratio.
[0020] Effects of the Invention
[0021] The present invention can provide a samarium-iron-nitrogen magnet powder having both high magnetization and high coercivity. In addition, the present invention can provide a samarium-iron-nitrogen magnet having both high magnetization and high coercivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a flow chart schematically showing an example of a method for producing samarium-iron-nitrogen-based magnet powder according to one embodiment of the present invention.
[0023] Figure 2 The present invention is a flowchart schematically showing an example of a method for producing a samarium-iron-bismuth-tungsten-nitrogen based sintered magnet using the samarium-iron-nitrogen based magnet powder according to one embodiment of the present invention.
[0024] Figure 3 The present invention is a flowchart schematically showing an example of a method for producing a samarium-iron-bismuth-tungsten-nitrogen based unsintered magnet using the samarium-iron-nitrogen based magnet powder according to one embodiment of the present invention.
[0025] Figure 4 Graphs showing the relationship between the coercive force and magnetization obtained in each example.
[0026] Figure 5 This is a diagram schematically showing a graph obtained when measuring the nitrogen release temperature.
[0027] Figure 6 This is a diagram schematically showing a graph obtained when measuring the decomposition temperature.
[0028] Figure 7 It is a graph showing the change rate ΔPa (%) of the lattice constant in the a-axis direction and the change rate ΔPc (%) of the lattice constant in the c-axis direction in each magnet powder. DETAILED DESCRIPTION
[0029] Hereinafter, one embodiment of the present invention will be described.
[0030] As described above, according to the inventors of the present application, the samarium-iron-bismuth-nitrogen-based magnet powder described in Patent Document 1 has a problem that the magnetization is not sufficiently high, although it exhibits high coercivity.
[0031] In order to solve such problems, the inventors of the present application conducted intensive research and development on samarium-iron-nitrogen magnet powders having both high magnetization and high coercivity. As a result, the inventors of the present application found that when a predetermined amount of bismuth and tungsten are added to samarium-iron-nitrogen magnet powders to make samarium-iron-bismuth-tungsten-nitrogen magnet powders, the magnetization and coercivity of the magnet powders can be significantly improved, thereby completing the present invention.
[0032] That is, in one embodiment of the present invention, there is provided a samarium-iron-nitrogen magnet powder comprising:
[0033] Lanthanide (Ln), iron (Fe), bismuth (Bi), tungsten (W) and nitrogen (N),
[0034] The above lanthanoid elements include samarium (Sm),
[0035] The ratio of bismuth to the sum of lanthanide elements + iron + bismuth + tungsten ((Bi / (Ln+Fe+Bi+W))) is 1.00 at% or less in terms of atomic ratio.
[0036] In terms of atomic ratio, the ratio of tungsten to the sum of lanthanide elements + iron + bismuth + tungsten ((W / (Ln+Fe+Bi+W))) is 0.05 at% or more and 0.60 at% or less,
[0037] The ratio of tungsten to bismuth (W / Bi) is 1.0 to 30.0 in atomic ratio.
[0038] In addition, in the present application, the samarium-iron-bismuth-tungsten-nitrogen based magnet powder according to one embodiment of the present invention is also referred to as "samarium-iron-nitrogen based magnet powder".
[0039] In the samarium-iron-nitrogen magnet powder according to one embodiment of the present invention, bismuth is added in a manner such that the ratio of bismuth to the sum of lanthanide elements (Ln) + iron + bismuth + tungsten ((Bi / (Ln+Fe+Bi+W))) is 1.00at% or less. In addition, in the samarium-iron-nitrogen magnet powder according to one embodiment of the present invention, tungsten is added in a manner such that the ratio of tungsten to the sum of lanthanide elements + iron + bismuth + tungsten ((W / (Ln+Fe+Bi+W))) is 0.05at% to 0.60at%. In addition, the ratio of tungsten to bismuth (W / Bi) is 1.0 to 30.0.
[0040] By adding bismuth and tungsten in such a ratio, in one embodiment of the present invention, a magnet powder having high magnetization and high coercive force is obtained.
[0041] In addition, the reason why a magnet powder having high magnetization and high coercive force can be obtained by adding bismuth and tungsten together has not yet been fully elucidated. However, as described later, it is believed that in the samarium-iron-nitrogen magnet powder of one embodiment of the present invention, the lattice constant Pa in the a-axis direction and the lattice constant Pc in the c-axis direction are both larger than those of the basic samarium-iron-nitrogen magnet powder. Therefore, it is believed that by adding bismuth and tungsten together, at least a part of samarium and / or Fe is replaced by Bi and / or W, and the stability of the crystal structure of the particles constituting the magnet powder is improved, resulting in the possibility of increasing the coercive force without reducing the magnetization. In the samarium-iron-nitrogen magnet powder of one embodiment of the present invention, (Bi / (Ln+Fe+Bi+W) is preferably less than 0.1at%, and more preferably less than 0.05at%.
[0042] In the samarium-iron-nitrogen magnet powder according to one embodiment of the present invention, W / (Ln+Fe+Bi+W) is preferably 0.41 at % or less.
[0043] Furthermore, in the samarium-iron-nitrogen based magnet powder according to one embodiment of the present invention, the atomic ratio W / Bi is preferably 20.5 or less.
[0044] In addition, when (W / (Ln+Fe+Bi+W) is less than 0.05at% or greater than 0.60at%, no improvement in magnetization is observed. Similarly, when the atomic ratio W / Bi is less than 1.0 or greater than 30.0, no improvement in magnetization is observed.
[0045] (Samarium-Iron-Nitride Magnet Powder According to One Embodiment of the Present Invention)
[0046] Hereinafter, other features of the samarium-iron-nitrogen based magnet powder according to one embodiment of the present invention will be described.
[0047] (composition)
[0048] The samarium-iron-nitrogen magnet powder (hereinafter also referred to as "the magnet powder of the present invention") according to one embodiment of the present invention contains a lanthanoid element. The lanthanoid element may contain only samarium, but may further contain at least one additional element selected from the group consisting of lanthanum (La), cerium (Ce), erbium (Er), thulium (Tm) and ytterbium (Yb).
[0049] In the magnet powder of the present invention, the ratio of the lanthanoid element to the sum of the lanthanoid element + iron + bismuth + tungsten (Ln / (Ln+Fe+Bi+W)) is, for example, in the range of 10.0 at % to 15.0 at %.
[0050] On the other hand, in the magnet powder of the present invention, the ratio of iron to the sum of lanthanoid elements + iron + bismuth + tungsten (Fe / (Ln+Fe+Bi+W)) is, for example, in the range of 85.0 at% to 90.0 at%.
[0051] (form)
[0052] The magnet powder of the present invention comprises a large number of particles. The particles have a core portion, and at least a portion of the core portion may be provided with a coating layer. The coating layer may cover the entire core portion. However, particles not containing a coating layer and particles consisting only of a core portion may also exist.
[0053] Typically, the core of the particle comprises lanthanides, iron, bismuth, tungsten and nitrogen.
[0054] In addition, the core of the particle usually has Th2Zn 17 Crystal structure.
[0055] For example, the core of the particle has a lanthanide-iron-nitrogen compound phase, for example, Ln2Fe 17 N3 phase. In addition, Ln2Fe 17 At least a portion of the Ln in the N3 phase may be substituted by Bi and / or W. Similarly, Ln2Fe 17 At least a part of Fe in the N3 phase may be substituted by Bi and / or W.
[0056] On the other hand, the coating layer contains a lanthanoid element and / or iron, but has a crystal structure different from that of the core portion.
[0057] The coating layer may contain more lanthanoids than the core portion. That is, the atomic ratio of lanthanoids to iron (Ln / Fe) in the coating layer may be greater than the atomic ratio of lanthanoids to iron (Ln / Fe) in the core portion.
[0058] The average particle size of the particles is not particularly limited, and may be, for example, less than 1.5 μm. In this case, the coercive force of the magnet powder of the present invention can be further increased.
[0059] In addition, among the particles contained in the magnet powder of the present invention, the number of particles having an aspect ratio of 2.0 or more is 10% or less, preferably 8% or less. When the number of particles having an aspect ratio of 2.0 or more is 10% or less, the coercivity of the magnet powder of the present invention can be further increased.
[0060] Furthermore, the magnet powder of the present invention has a characteristic of having a high decomposition temperature. For example, the nitrogen release temperature of the magnet powder of the present invention is 610° C. or higher.
[0061] The coercive force of the magnet powder of the present invention before heat treatment is, for example, 17 kOe or more. In addition, the magnetization of the magnet powder of the present invention is, for example, 140 emu / g or more. Therefore, the magnet powder of the present invention can be used as a magnet powder having both high magnetization and high coercive force. In addition, in the present application, magnetization refers to the value of magnetization when a magnetic field of 90 kOe is applied.
[0062] The magnet powder of the present invention having the above-mentioned characteristics can be used for the production of high-performance samarium-iron-nitrogen-based magnets.
[0063] (Samarium-Iron-Nitride Magnet)
[0064] A samarium-iron-nitrogen magnet according to one embodiment of the present invention (hereinafter, also simply referred to as “the magnet according to the present invention”) contains the magnet powder according to the present invention.
[0065] The magnet of the present invention may be a samarium-iron-nitrogen based sintered magnet or a samarium-iron-nitrogen based bonded magnet.
[0066] Among the magnets of the present invention, the rare earth magnet according to the present embodiment may have a metal phase other than the Sm-Fe-N system magnet powder. Such a metal phase may be, for example, an Fe phase.
[0067] The rare earth magnet according to the present embodiment may further contain at least one element of, for example, C, Al, Si, P, Ti, Cr, Mn, Co, Cu, Zn, Y, Zr, and Sn in addition to Sm, Fe, and N. The content of elements other than Sm, Fe, and N is preferably 10% by mass or less, and more preferably 5% by mass or less.
[0068] (Method for producing samarium-iron-nitrogen magnet powder according to one embodiment of the present invention)
[0069] Next, refer to Figure 1 , an example of a method for producing a samarium-iron-nitrogen-based magnet powder according to an embodiment of the present invention (hereinafter referred to as “the first method”) is described.
[0070] In the following description, the first method is described by taking the case where only samarium is included as the lanthanoid element (Ln) as an example. However, it is clear that those skilled in the art can apply the same method when the lanthanoid element (Ln) includes other lanthanoid elements (at least one of La, Ce, Er, Tm and Yb) in addition to samarium.
[0071] Figure 1 An example of the flow of the first method is schematically shown.
[0072] Figure 1 As shown, the first method has:
[0073] The step of preparing a precursor powder (S110),
[0074] The step of reducing and diffusing the precursor powder in an inert gas atmosphere to prepare a samarium-iron-bismuth-tungsten alloy powder (S120) is performed.
[0075] a step of nitriding the samarium-iron-bismuth-tungsten alloy powder to prepare a samarium-iron-bismuth-tungsten-nitrogen alloy powder (S130); and
[0076] A step of washing the samarium-iron-bismuth-tungsten-nitrogen alloy powder (S140).
[0077] Hereinafter, each step will be described.
[0078] (Process S110)
[0079] First, a precursor powder is prepared.
[0080] The precursor powder may be, for example, a samarium-iron-bismuth-tungsten oxide powder or a samarium-iron-bismuth-tungsten hydroxide powder. In addition, the samarium-iron-bismuth-tungsten oxide powder and the samarium-iron-bismuth-tungsten hydroxide powder are collectively referred to as samarium-iron-bismuth-tungsten (hydr)oxide powder hereinafter.
[0081] The samarium-iron-bismuth-tungsten-based (hydr)oxide powder can be prepared by a spray pyrolysis method.
[0082] In this method, first, a solution containing samarium salt, iron salt, bismuth salt and tungsten salt is prepared. The composition of the samarium-iron-nitrogen magnet powder can be controlled to a desired value by adding the samarium salt, iron salt, bismuth salt and tungsten salt.
[0083] As the solvent contained in the solution, water can be used, or an organic solvent such as ethanol can be used.
[0084] In addition, the counter ions in the samarium salt, iron salt, bismuth salt and tungsten salt may be inorganic ions such as chloride ions, sulfate ions or nitrate ions, or the counter ions may be organic ions such as alkoxides.
[0085] In addition, when adding bismuth salt and tungsten salt to the solution, in order to dissolve them appropriately, it is preferred to adjust the pH to the acidic side. Such pH adjustment is preferably performed using nitric acid or the like. If the pH of the solution is neutral or alkaline, the bismuth salt and tungsten salt are easily dissolved and remain. Therefore, the ratio of bismuth to tungsten in the obtained samarium-iron-nitrogen magnet powder is easily deviated from the desired range. By appropriately dissolving the bismuth salt and tungsten salt in the solution, the bismuth and tungsten contents of the obtained samarium-iron-nitrogen magnet powder are controlled to be within the desired range.
[0086] Next, the modulated solution is supplied to the heated reaction tube, and the solution is thermally decomposed. When supplying the solution, a sprayer such as an ultrasonic method or a two-fluid nozzle method can be used. In this case, fine droplets are formed from the solution, and the droplets are introduced into the reaction tube together with the carrier gas. The supplied solution or droplets are thermally decomposed in the reaction tube. The temperature in the reaction tube is, for example, in the range of 400°C to 1000°C.
[0087] The particles generated by thermal decomposition of the solution or liquid droplets are then collected by a filter at the outlet of the reaction tube, thereby obtaining a samarium-iron-bismuth-tungsten-based (hydr)oxide powder.
[0088] The obtained precursor powder can be handled in a non-oxidizing atmosphere such as a glove box until the samarium-iron-nitrogen magnet powder is produced. When an inert gas atmosphere is used as the non-oxidizing atmosphere, the oxygen concentration is preferably 1 ppm or less.
[0089] The obtained precursor powder is preferably pre-reduced in a reducing atmosphere, thereby reducing the amount of calcium used in the subsequent reduction diffusion step (step S120) and suppressing the generation of coarse samarium-iron-bismuth-tungsten alloy particles.
[0090] Pre-reduction of the precursor powder can be performed, for example, by heating the precursor powder to 400° C. or higher in a hydrogen atmosphere. The treatment temperature is preferably in the range of 500° C. to 800° C. When pre-reduction is performed in this temperature range, samarium-iron-bismuth-tungsten alloy particles having a uniform particle size can be obtained in the subsequent steps.
[0091] (Process S120)
[0092] Next, the precursor powder is subjected to reduction diffusion treatment in an inert gas atmosphere to form a samarium-iron-bismuth-tungsten alloy powder (hereinafter, also referred to as “alloy powder I”).
[0093] Examples of a method for reducing and diffusing the precursor powder include a method in which the precursor powder is mixed with calcium (Ca) or calcium hydride (CaH 2 ) and then heated to a temperature higher than the melting point of Ca (approximately 850° C.).
[0094] During this treatment, samarium reduced by calcium diffuses into the calcium melt and reacts with iron, bismuth, and tungsten to form alloy powder I.
[0095] There is a correlation between the temperature of the reduction diffusion treatment and the particle size of the particles included in the alloy powder I. The higher the temperature of the reduction diffusion treatment, the larger the particle size of the particles included in the alloy powder I.
[0096] The average particle size of the particles contained in the alloy powder I is preferably 3.0 μm or less. When the average particle size is 3.0 μm or less, the coercive force of the magnet powder finally obtained is further improved.
[0097] In order to obtain alloy powder I including particles having uniform particle sizes, the precursor powder is preferably subjected to reduction diffusion treatment at 850° C. to 1050° C. for about 1 minute to 2 hours in an inert gas atmosphere.
[0098] Each particle of the alloy powder I crystallizes as the reduction diffusion proceeds, for example, to form a Th2Zn 17 In this case, the coating layer is formed on at least a portion of the surface of the core portion.
[0099] (Process S130)
[0100] Next, the obtained alloy powder I is nitrided to form a samarium-iron-bismuth-tungsten-nitrogen alloy powder (hereinafter, also simply referred to as "alloy powder II").
[0101] Examples of a method for nitriding the alloy powder I include a method of heat treating the alloy powder I at 300° C. to 500° C. in an atmosphere of ammonia, a mixed gas of ammonia and hydrogen, nitrogen, or a mixed gas of nitrogen and hydrogen.
[0102] When ammonia is used, alloy powder I can be nitrided in a short time. However, there is a possibility that the nitrogen content in alloy powder II is higher than the optimal value. In this case, after nitriding, alloy powder II is preferably annealed in hydrogen. Thereby, excess nitrogen can be discharged from the crystal lattice.
[0103] The composition of the particles contained in the alloy powder II is preferably Sm2Fe 17 N3.
[0104] For example, alloy powder I is heat treated at 350°C to 450°C for 10 minutes to 2 hours in an ammonia-hydrogen mixed atmosphere, and then annealed at 350°C to 450°C for 30 minutes to 2 hours in a hydrogen atmosphere. In this way, the nitrogen content in alloy powder II can be optimized.
[0105] (Process S140)
[0106] Next, the alloy powder II formed in step S130 is washed.
[0107] The alloy powder II formed in step S130 contains a calcium compound. In order to remove such a calcium compound, a washing treatment is performed.
[0108] The washing treatment is performed using a washing liquid such as water and / or alcohol. For example, most of the calcium compound contained in the alloy powder II can be removed by repeatedly performing stirring and decantation after adding water to the alloy powder II.
[0109] Alternatively, a cleaning step may be performed before the nitriding treatment.
[0110] Through the above steps, samarium-iron-bismuth-tungsten-nitrogen based magnet powder can be produced.
[0111] However, the following additional step (step S150 ) may be performed on the samarium-iron-bismuth-tungsten-nitrogen based magnet powder (hereinafter also simply referred to as “production powder”) obtained in step S140 .
[0112] (Process S150)
[0113] The produced powder obtained in step S140 is preferably subjected to vacuum drying treatment.
[0114] The drying temperature is not particularly limited, but is preferably in the range of room temperature to 100° C. By setting the drying temperature to 100° C. or less, oxidation of the produced powder can be suppressed.
[0115] Furthermore, the produced powder may be subjected to a dehydrogenation treatment, which can remove hydrogen that has entered the crystal lattices during the washing process.
[0116] The method of dehydrogenation treatment is not particularly limited. For example, the dehydrogenation treatment can be performed by heating the manufactured powder under vacuum or in an inert gas atmosphere. For example, the dehydrogenation treatment can be performed by heat-treating the manufactured powder at 150° C. to 450° C. for 1 hour under an argon atmosphere.
[0117] Furthermore, the production powder can be subsequently comminuted, thereby increasing the residual magnetization and the maximum energy product of the production powder.
[0118] In addition, in this application, "crushing" is used as another term of "crushing".
[0119] That is, "disintegration" means separating one or more particles from agglomerates when a plurality of particles are aggregated. On the other hand, "crushing" means dividing a single particle into a plurality of smaller pieces.
[0120] When the powder is produced by pulverization, a jet mill, a dry or wet ball mill, a vibration mill, a medium stirring mill, or the like can be used.
[0121] In addition, the crushing step does not necessarily need to be performed at this stage. For example, the crushing step can be performed on the alloy powder I obtained in step S120.
[0122] (Method for producing samarium-iron-bismuth-tungsten-nitrogen based sintered magnet)
[0123] Next, refer to Figure 2 An example of a method for producing a samarium-iron-bismuth-tungsten-nitrogen based sintered magnet using the magnet powder of the present invention (hereinafter referred to as the "second method") is described.
[0124] In the following description, the second method is described by taking the case where only samarium is included as the lanthanide element (Ln) as an example. However, it is clear that those skilled in the art can apply the same method when the lanthanide element (Ln) includes other lanthanide elements (at least one of La, Ce, Er, Tm and Yb) in addition to samarium.
[0125] Figure 2 An example of the flow of the second method is schematically shown.
[0126] Figure 2 As shown, the second method has:
[0127] a step of compacting the samarium-iron-bismuth-tungsten-nitrogen magnet powder to form a compact (step S210); and
[0128] A step of sintering the molded body (step S220).
[0129] Hereinafter, each step will be described.
[0130] (Step S210)
[0131] First, a samarium-iron-bismuth-tungsten-nitrogen-based magnet powder having the above-mentioned characteristics is prepared, and the magnet powder is compacted to form a compact.
[0132] The molding method is not particularly limited, and a general molding method for magnet powder can be used. The pressure applied during molding is, for example, in the range of 10 MPa to 3000 MPa.
[0133] In addition, the magnet powder may be molded while a magnetic field is applied to the magnet powder during molding. In this case, the magnet powder contained in the molded body is oriented in a specific direction, thereby obtaining an anisotropic magnet with high magnetic properties.
[0134] (Process S220)
[0135] Next, the molded body is sintered.
[0136] The method of the sintering treatment is not particularly limited, and a general sintering treatment method such as a discharge plasma method and a hot press method can be used.
[0137] The sintering temperature may be, for example, in the range of 300°C to 650°C.
[0138] In addition, step S210 and step S220 can be implemented using the same device.
[0139] Through the above steps, a samarium-iron-bismuth-tungsten-nitrogen based sintered magnet can be manufactured.
[0140] (Method for producing samarium-iron-bismuth-tungsten-nitrogen system non-sintered magnet)
[0141] Next, refer to Figure 3 , an example of a method for producing a samarium-iron-bismuth-tungsten-nitrogen based non-sintered magnet (hereinafter referred to as the "third method") is described.
[0142] In the following description, the third method is described by taking the case where only samarium is included as the lanthanoid element (Ln) as an example. However, it is clear that those skilled in the art can apply the same method when the lanthanoid element (Ln) includes other lanthanoid elements (at least one of La, Ce, Er, Tm and Yb) in addition to samarium.
[0143] Figure 3 An example of the flow of the third method is schematically shown.
[0144] Figure 3 As shown, the third method has:
[0145] a step of preparing particles from samarium-iron-bismuth-tungsten-nitrogen magnet powder (step S310), and
[0146] A step of molding the above-mentioned particles (step S320).
[0147] Hereinafter, each step will be described.
[0148] (Process S310)
[0149] First, particles are prepared from samarium-iron-bismuth-tungsten-nitrogen magnet powder.
[0150] Therefore, the magnet powder is mixed with a resin. The resin used may be a thermosetting resin or a thermoplastic resin. A thermoplastic resin is particularly preferred. Suitable thermoplastic resins include polyamide (PA) and polyphenylene sulfide (PPS).
[0151] Next, the mixture is heated and kneaded, and the kneaded product is pelletized using a pelletizer, etc. The heating temperature may be, for example, in the range of 150°C to 330°C.
[0152] (Process S320)
[0153] Next, the pellets produced in step S310 are molded.
[0154] The molding process may be performed by injection molding, in which case a molded body formed by injection molding into a predetermined shape can be obtained from pellets introduced into an injection molding device.
[0155] In this way, a molded bond magnet can be obtained.
[0156] In addition, the particles can be molded in a state where a magnetic field is applied to a mold, thereby obtaining an anisotropic bonded magnet.
[0157] Through the above steps, a samarium-iron-bismuth-tungsten-nitrogen based non-sintered magnet can be manufactured.
[0158] Example
[0159] Hereinafter, examples of the present invention will be described. In the following description, Examples 1 to 9 are examples, and Examples 11 to 16 are comparative examples.
[0160] (Example 1)
[0161] The magnet powder was prepared by the following method.
[0162] (Preparation of precursor powder)
[0163] After adding 63.10 g of iron nitrate nonahydrate, 12.63 g of samarium nitrate hexahydrate, 0.62 g of lanthanum nitrate hexahydrate, 0.77 g of bismuth nitrate pentahydrate and 0.20 g of ammonium tungstate pentahydrate to 1800 ml of water, 10.50 ml of nitric acid was added while stirring to dissolve the salts.
[0164] Next, the prepared solution is dropletized using a spray pyrolysis device, and the droplets are pyrolyzed. The device has an ultrasonic sprayer and a heated reaction tube at the inlet side, and a filter is provided at the outlet of the reaction tube.
[0165] The solution introduced into the device is transformed into fine droplets by an ultrasonic nebulizer. The droplets are supplied into the reaction tube together with the carrier gas (atmosphere). The reaction tube is preheated, and the droplets are thermally decomposed in the reaction tube. Then, the thermal decomposition product is captured by a filter. The temperature of the reaction tube is 900°C.
[0166] The thermal decomposition product was collected by a filter at the outlet of the reaction tube.
[0167] Next, the obtained thermal decomposition product was subjected to a preliminary reduction treatment in a hydrogen atmosphere at a treatment temperature of 600° C. and a treatment time of 6 hours. Thus, a precursor powder containing samarium and lanthanum as lanthanoid elements was obtained.
[0168] (Reduction diffusion treatment)
[0169] Next, 5 g of the precursor powder and 2.5 g of metal calcium were placed in an iron crucible, and then heated at 975° C. for 1 hour to reduce and diffuse the precursor powder.
[0170] In this way, alloy powder (hereinafter referred to as "alloy powder A") was prepared.
[0171] (Nitriding treatment)
[0172] Next, the alloy powder A was cooled to room temperature, and then heated to 420° C. in a mixed atmosphere of ammonia and hydrogen at a volume ratio of 1:2, and maintained at this temperature for 1 hour to perform a nitriding treatment.
[0173] In this way, alloy powder B was produced.
[0174] Next, in order to optimize the nitrogen content contained in the alloy powder B, the alloy powder B was further subjected to heat treatment. The heat treatment was performed by annealing the alloy powder B at 420° C. for 1 hour in a hydrogen atmosphere and then annealing the alloy powder B at 420° C. for 0.5 hour in an argon atmosphere.
[0175] (Washing treatment)
[0176] Next, the alloy powder B having the optimized nitrogen content was washed five times with pure water to remove calcium compounds and the like. Thus, an alloy powder C was obtained.
[0177] (Vacuum drying treatment)
[0178] Next, in order to remove the water remaining in the alloy powder C, the alloy powder C was immersed in a 2-propanol solution, and then the alloy C was vacuum dried at room temperature.
[0179] Furthermore, after the vacuum drying treatment, the alloy powder C was subjected to a dehydrogenation treatment at 200° C. for 3 hours under vacuum.
[0180] In this way, magnet powder is produced.
[0181] In the above method, each step after the preliminary reduction treatment is performed in a glove box set to an argon atmosphere.
[0182] (Example 2~Example 6)
[0183] The magnet powder was produced by the same method as in Example 1. However, in Examples 2 to 6, the composition of the precursor powder was changed from that in Example 1 to produce the magnet powder. The other production conditions were the same as in Example 1.
[0184] (Example 7)
[0185] Magnet powder was prepared by the same method as in Example 1. However, in Example 7, no lanthanum compound was added when preparing the precursor powder. That is, the precursor powder containing only samarium as the lanthanoid element Ln was prepared. In addition, the reduction diffusion treatment temperature was 1025°C.
[0186] The other manufacturing conditions were the same as those in Example 1.
[0187] (Example 8~Example 9)
[0188] The magnet powder was produced by the same method as in Example 1. However, in Examples 8 and 9, the composition of the precursor powder was changed from that in Example 1 to produce the magnet powder. The other production conditions were the same as in Example 1.
[0189] (Example 11~Example 13)
[0190] Magnet powder was prepared by the same method as in Example 1. However, in Examples 11 to 13, no lanthanum compound, bismuth compound, and tungsten compound were added when preparing the precursor powder. That is, in Examples 11 to 13, samarium-iron-based precursor powder was prepared. Other manufacturing conditions were the same as in Example 1.
[0191] (Example 14)
[0192] Magnet powder was prepared by the same method as in Example 1. However, in Example 14, no lanthanum compound and tungsten compound were added when preparing the precursor powder. That is, in Example 14, a precursor powder of samarium-iron-bismuth system was prepared. In addition, the reduction diffusion treatment temperature was 920°C. Other manufacturing conditions were the same as in Example 1.
[0193] (Example 15~Example 16)
[0194] The magnet powder was produced by the same method as in Example 1. However, in Examples 15 and 16, the addition amount of each component contained in the precursor powder was changed compared with that in Example 1 to produce the magnet powder. In addition, the reduction diffusion temperature was 930°C in Example 15 and 975°C in Example 16. The other production conditions were the same as in Example 1.
[0195] (evaluate)
[0196] The following evaluations were performed using the magnet powder obtained in each example.
[0197] (X-ray diffraction measurement)
[0198] The X-ray diffraction (XRD) spectra were measured using the magnet powders in each example. The results showed that the main phase of all magnet powders contained Th2Zn 17 structure.
[0199] Furthermore, the nitrogen content of each magnet powder was measured by the inert gas fusion-thermal conductivity method. As a result, the nitrogen content of each magnet powder was about 3.3 mass %.
[0200] (Composition Analysis)
[0201] The composition of each magnet powder was analyzed by high-frequency inductively coupled plasma emission spectrometry. The results confirmed that the magnet powders involved in Examples 1 to 6 were samarium-lanthanum-iron-bismuth-tungsten-nitrogen magnet powders, the magnet powder involved in Example 7 was samarium-iron-bismuth-tungsten-nitrogen magnet powders, and the magnet powders involved in Examples 8 and 9 were samarium-lanthanum-iron-bismuth-tungsten-nitrogen magnet powders.
[0202] In addition, it was confirmed that the magnet powder involved in Examples 11 to 13 was a samarium-iron-nitrogen magnet powder, the magnet powder involved in Example 14 was a samarium-iron-bismuth-nitrogen magnet powder, and the magnet powder involved in Examples 15 to 16 was a samarium-lanthanum-iron-bismuth-tungsten-nitrogen magnet powder.
[0203] Table 1 below summarizes the composition and other properties of each magnet powder.
[0204] [Table 1]
[0205]
[0206] In Table 1, "W / Bi" means the ratio (atomic ratio) of the amount of tungsten contained in the magnet powder to the amount of bismuth.
[0207] (Determination of average particle size and aspect ratio)
[0208] The average particle size of each magnet powder was measured using a scanning electron microscope (FE-SEM).
[0209] During the measurement, more than 200 particles are randomly selected, and a contour line is obtained in each selected particle. The diameter of a circle with the same area as the area surrounded by the contour line is set as the particle size of the particle. The value of the arithmetic average of the particle sizes obtained in each selected particle is set as the average particle size of the particles contained in each magnet powder.
[0210] Similarly, each selected particle is used to calculate the aspect ratio. The result shows the ratio of particles with an aspect ratio of more than 2.0. In addition, the aspect ratio is defined by dividing the length of the long side by the length of the short side in a quadrilateral with the smallest area circumscribed with the contour line of the particle.
[0211] (Observation of coating layer)
[0212] In the magnet powders according to Examples 1 to 9, whether or not a coating layer was formed on the surface of the core portion of the particles was evaluated by the following method.
[0213] First, a portion of each magnet powder is collected, kneaded with a thermosetting epoxy resin, and thermally cured to produce a sample, and then the sample is irradiated with a focused ion beam (FIB) and etched to expose a cross section of the sample.
[0214] The cross section of the sample was observed using a scanning transmission electron microscope (STEM) and energy dispersive X-ray spectroscopy (EDS) to confirm the presence or absence of a coating layer.
[0215] As a result of the observation, it was found that in the magnet powders according to Examples 1 to 9, a coating layer existed on the surface of the core portion of the particles.
[0216] The compositions of the core and the coating layer were analyzed by energy dispersive X-ray spectroscopy (EDS). As a result, the atomic ratio of lanthanide elements to iron (Ln / Fe) in the coating layer was greater than the atomic ratio of lanthanide elements to iron (Ln / Fe) in the core.
[0217] (Determination of coercive force and magnetization)
[0218] Using the magnet powder according to each example, the coercive force and magnetization were measured.
[0219] First, magnet powder and thermoplastic resin were mixed and then oriented in a magnetic field of 20 kOe to prepare a sample for measurement.
[0220] Next, the coercive force and magnetization of the sample were measured using a vibrating sample magnetometer (VSM). The measurement temperature was 27° C. and the maximum applied magnetic field was 90 kOe. The applied magnetic field was applied along the magnetization prone axis of the sample.
[0221] Here, the magnetization refers to a value of magnetization obtained when a magnetic field of 90 kOe is applied.
[0222] The following Table 2 summarizes the evaluation results obtained for each magnet powder.
[0223] [Table 2]
[0224]
[0225] also, Figure 4 The relationship between the coercive force and magnetization obtained in each magnet powder is shown.
[0226] Depend on Figure 4 It was confirmed that the magnet powders according to Examples 1 to 9 had both higher coercive force and higher magnetization than the magnet powders according to Examples 11 to 16.
[0227] (Determination of Nitrogen Release Temperature and Decomposition Temperature)
[0228] The nitrogen release temperature and decomposition temperature of each magnet powder were measured using a thermogravimetric measuring device connected to a mass spectrometer. The measurement conditions were an argon atmosphere and a temperature increase rate of 20°C / min.
[0229] Figure 5 A graph obtained when measuring the nitrogen release temperature is schematically shown. Figure 5 In the figure, the horizontal axis is temperature, and the vertical axis is N2 with a mass-to-charge ratio (m / z) of 28. + of ion current.
[0230] The nitrogen release temperature is determined as follows:
[0231] first, Figure 5 As shown in FIG. 1 , a first approximate straight line LP1 is drawn in a manner corresponding to the change in ion current in the temperature range of 500° C. to 550° C. Next, the change in ion current ( Figure 5 The positive slope of the curve in the figure) becomes the maximum temperature T 1max , at the temperature T 1max Center T 1max In the region of ±10° C., a second approximate straight line LP2 is drawn.
[0232] The nitrogen release temperature T is calculated from the intersection of the extension lines of the two approximate straight lines LP1 and LP2. N In addition, when the first approximate straight line is greatly deviated by the actual change in ion current, a temperature region with relatively small changes is obtained in the temperature range of 400°C to 600°C, and the first approximate straight line LP1 is drawn in this region (temperature width is 50°C. For example, 450°C to 500°C, etc.).
[0233] The measurement results show that the nitrogen release temperatures of the magnet powders of Examples 1 to 9 are all 610° C. or higher.
[0234] Figure 6 The graph obtained when measuring the decomposition temperature is schematically shown. Figure 6 In the graph, the horizontal axis is temperature and the vertical axis is weight change.
[0235] The decomposition temperature is determined as follows:
[0236] first, Figure 6 In the figure, a first approximate straight line LQ1 is drawn corresponding to the weight change in the temperature range of 500°C to 550°C. Next, the negative change ( Figure 6 The negative slope of the curve in the figure) becomes the maximum temperature T 2max , at the temperature T 2max Center T 2max In the region of ±10° C., a second approximate straight line LQ2 is drawn.
[0237] From the intersection of the two approximate straight lines LQ1 and LQ2, find the decomposition temperature T d In addition, when the first approximate straight line is greatly deviated from the actual change in decomposition temperature, a temperature region with relatively small changes is obtained in the temperature range of 400°C to 600°C, and the first approximate straight line LQ1 is drawn in this region (temperature width is 50°C. For example, 450°C to 500°C, etc.).
[0238] The results of the measurement showed that the decomposition temperatures of the magnet powders of Examples 1 to 9 were all 630° C. or higher.
[0239] (lattice constant)
[0240] The lattice constant of each magnet powder was measured by the following method.
[0241] A borosilicate glass capillary tube with an inner diameter of 0.3 mm was filled with magnet powder.
[0242] Next, the diffraction peaks were measured by the X-ray diffraction method (transmission method) at beamline BL19B2 of SPring-8 (manufactured by the High Brightness Photonics Research Center (JASRI)) using a large Debye-Scherrer camera. The wavelength of the X-ray is A semiconductor detector was used as the detector. The exposure time was 60 seconds per exposure, and the exposure results were accumulated four times. The measurement was performed at room temperature.
[0243] The lattice constant of the magnet powder was calculated from the obtained measurement results by Rietveld analysis.
[0244] Figure 7 The measurement results of the lattice constants obtained for the respective magnet powders are shown.
[0245] Figure 7 In the graph, the horizontal axis represents the change rate ΔPa (%) of the lattice constant of the magnet powder in the a-axis direction, and the vertical axis represents the change rate ΔPc (%) of the lattice constant of the magnet powder in the c-axis direction.
[0246] ΔPa and ΔPc are obtained as follows.
[0247] First, a magnet powder to be evaluated (for example, the magnet powder according to Example 1) is determined. The magnet powder in question will be referred to as "target powder" hereinafter.
[0248] Next, a base powder corresponding to the target powder is prepared. The base powder is a samarium-iron-nitrogen magnet powder, and therefore does not contain lanthanide elements (Ln) other than samarium, bismuth, and tungsten. In addition, samarium, iron, and nitrogen in the base powder have the same composition ratio as the target powder.
[0249] Next, the lattice constant Pa(ref) in the a-axis direction and the lattice constant Pc(ref) in the c-axis direction of the base powder are measured. In addition, the lattice constant Pa in the a-axis direction and the lattice constant Pc in the c-axis direction of the target powder are measured.
[0250] From the results obtained,
[0251] As ΔPa={Pa / Pa(ref)}×100 and
[0252] ΔPc={Pc / Pc(ref)}×100
[0253] The lattice constant change rates ΔPa and ΔPc were evaluated.
[0254] Therefore, when the lattice constant change rate ΔPa exceeds 100%, it means that the a-axis direction of the target powder is expanded compared with the a-axis direction of the base powder. On the contrary, when the lattice constant change rate ΔPa is less than 100%, it means that the a-axis direction of the target powder is contracted compared with the a-axis direction of the base powder.
[0255] The same can be said about the lattice constant change rate ΔPc.
[0256] Depend on Figure 7 It is found that the lattice constant change rates ΔPa and ΔPc are both 100% in the magnet powder according to Example 11. Therefore, it is assumed that the magnet powder according to Example 11 has the same crystal lattice structure as the base powder.
[0257] On the other hand, it is found that the lattice constant change rates ΔPa and ΔPc of the magnet powders of Examples 1 to 4 are both greater than 100%. In other words, it is found that the magnet powders of Examples 1 to 4 have lattices that are expanded in the a-axis direction and the c-axis direction compared to the base powders.
[0258] From this result, it is considered that in the magnet powder of one embodiment of the present invention, the crystal lattice expands in both the a-axis and the c-axis, and the stability of the crystal structure of the particles is improved, so that both the magnetization and the coercive force are improved.
[0259] This application claims the priority based on Japanese Patent Application No. 2022-050743 for which it applied on March 25, 2022, and all the contents of this Japanese application are incorporated by reference into this application.
Claims
1. A samarium-iron-nitrogen magnet powder comprising: Lanthanide (Ln), iron (Fe), bismuth (Bi), tungsten (W) and nitrogen (N), The lanthanide element comprises samarium (Sm), In terms of atomic ratio, the ratio of bismuth to the sum of lanthanide elements + iron + bismuth + tungsten, i.e., Bi / (Ln+Fe+Bi+W), is less than 1.00 at%, In terms of atomic ratio, the ratio of tungsten to the sum of lanthanide elements + iron + bismuth + tungsten, i.e., W / (Ln+Fe+Bi+W), is 0.05 at% to 0.60 at%. The ratio of tungsten to bismuth, that is, W / Bi, is in the range of 1.0 to 30.0 in atomic ratio.
2. The samarium-iron-nitrogen magnet powder according to claim 1, The lanthanoid element further has at least one additional element selected from the group consisting of lanthanum, cerium, erbium, thulium and ytterbium.
3. The samarium-iron-nitrogen magnet powder according to claim 1 or 2, The samarium-iron-nitrogen magnet powder comprises particles, wherein the particles have a core portion and a coating layer covering at least a portion of the core portion. The core of the particle has Th2Zn 17 Crystal structure, The coating layer of the particle has a crystal structure different from that of the core portion.
4. The samarium-iron-nitrogen magnet powder according to claim 3, The core of the particle has Ln2Fe 17 N3 phase, in, In this phase, at least a part of Ln and / or Fe is substituted by Bi and / or W.
5. The samarium-iron-nitrogen magnet powder according to claim 3 or 4, The coating layer of the particle contains a lanthanide element and iron.
6. The samarium-iron-nitrogen magnet powder according to claim 5, The atomic ratio of the lanthanoid element to iron in the coating layer, ie, Ln / Fe, is greater than the atomic ratio of the lanthanoid element to iron in the core portion, ie, Ln / Fe.
7. The samarium-iron-nitrogen magnet powder according to any one of claims 3 to 6, The average particle size of the particles is less than 1.5 μm, The number of particles having an aspect ratio of 2.0 or more is 10% or less.
8. The samarium-iron-nitrogen magnet powder according to any one of claims 1 to 7, The nitrogen release temperature of the samarium-iron-nitrogen based magnet powder is 610° C. or higher.