Multilayer ceramic capacitor
By using silver/palladium alloys and specific ceramic materials in the internal electrodes, such as (Ag0.7, Pd0.3)TiO3 and NaTiO3, the internal electrode coverage of the stacked ceramic capacitors is improved, and the problem of low coverage of thin-layered electrodes is solved. , realizes a large-capacity capacitor design.
Patent Information
- Application Number
- CN202380028710.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-26
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-05
AI Technical Summary
When manufacturing a laminated ceramic capacitor, the coverage ratio of the internal electrodes is difficult to maintain high, especially when the thickness is less than 1 μm, which leads to hindering the large capacity.
The internal electrode contains silver/palladium alloy as the conductive component, and ceramic materials such as (Ag0.7, Pd0.3)TiO3, NaTiO3 and EuTiO3 are added to increase the sintering temperature of the conductive paste film close to the sintering temperature of the ceramic dielectric layer. , thereby improving coverage.
The coverage of the internal electrodes is effectively improved, ensuring that the coverage can be maintained even in thin-layered conditions, and does not hinder the large capacity of the stacked ceramic capacitors.
Smart Images

Figure CN118901113A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a multilayer ceramic capacitor, and in particular to the composition of internal electrodes included in the multilayer ceramic capacitor. Background Art
[0002] Generally, a laminated ceramic capacitor comprises: a laminate having a plurality of laminated dielectric layers containing ceramics, and a plurality of internal electrodes respectively arranged along a plurality of interfaces between the dielectric layers; and a plurality of external electrodes provided on the outer surface of the laminate and electrically connected to the internal electrodes. The internal electrodes comprise a plurality of first internal electrodes and a plurality of second internal electrodes alternately arranged in the stacking direction of the laminate, and the external electrodes comprise a first external electrode electrically connected to the first internal electrode, and a second external electrode electrically connected to the second internal electrode.
[0003] In order to achieve the miniaturization and high capacity of the multilayer ceramic capacitor of this structure, it is required to thin the dielectric layer and the internal electrode and improve the coverage of the internal electrode (electrode continuity). Generally, in the firing process when manufacturing the multilayer ceramic capacitor, the sintering temperature of the conductive metal particles contained in the conductive paste film that should become the internal electrode is lower than the sintering temperature of the ceramic constituting the dielectric layer, so the metal particles contained in the internal electrode are sintered first. This causes the coverage of the internal electrode to decrease. In particular, in the internal electrode that is thinned to a thickness of less than 1μm, there is a problem that the coverage is easy to decrease, and such a decrease in coverage is easy to hinder the increase in capacity.
[0004] Therefore, in order to form thin-layered internal electrodes with high coverage, it is necessary to further increase the sintering temperature of the conductive metal particles contained in the conductive paste film that should become the internal electrodes during the firing process when manufacturing the laminated ceramic capacitor. As a result, the sintering temperature of the metal particles contained in the conductive paste film that should become the internal electrodes can be made close to the temperature at which the ceramic constituting the dielectric layer starts sintering, and the shrinkage timing during sintering can be made close between the internal electrode and the dielectric layer. As a result, the coverage of the internal electrode becomes higher, and a larger capacity can be achieved.
[0005] In order to increase the coverage of the internal electrode and realize a large capacity by the above-mentioned method, it is known to add a ceramic material having a composition similar to that of the ceramic constituting the dielectric layer, that is, a common material, to the conductive paste for forming the internal electrode, as described in, for example, paragraph 0004 of Patent Document 1 (Japanese Patent Publication No. 2016-31807). By adding the common material, the sintering timing of the metal particles contained in the conductive paste film to be the internal electrode can be moved to a higher temperature side, and the sintering temperature of the metal particles contained in the conductive paste film can be made close to the sintering temperature of the ceramic constituting the dielectric layer.
[0006] Prior Art Literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2016-31807 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] However, even if common materials are added to the conductive paste used to form the internal electrodes, it is undeniable that the sintering temperature of the metal particles contained in the conductive paste is still lower than the sintering temperature of the ceramic constituting the dielectric layer, and further improvement is desired. In particular, for example, with respect to the internal electrodes that are thinned to a thickness of less than 1 μm, an effective solution to the problem of reduced coverage that hinders the increase in capacity is strongly required.
[0011] Therefore, the present invention has been made in view of such a problem, and an object of the present invention is to provide a multilayer ceramic capacitor including internal electrodes capable of maintaining a relatively high coverage even when the internal electrodes are thinned.
[0012] Technical solutions to solve problems
[0013] A multilayer ceramic capacitor according to the present invention includes a laminate having a plurality of laminated dielectric layers made of ceramic and a plurality of internal electrodes disposed along a plurality of interfaces between the dielectric layers.
[0014] In order to solve the above technical problems, in the present invention, it is characterized in that the internal electrode contains a silver / palladium alloy as a conductive component and contains (Ag 0.7 ,Pd 0.3 )At least one selected from TiO3, NaTiO3 and EuTiO3.
[0015] Effects of the Invention
[0016] According to the present invention, the internal electrode contains (Ag 0.7 ,Pd 0.3 At least one selected from )TiO3, NaTiO3 and EuTiO3 helps to increase the coverage of the internal electrode containing the silver / palladium alloy as a conductive component. Therefore, even if the internal electrode is thinned, the coverage of the internal electrode does not decrease, which can prevent the increase in the capacity of the multilayer ceramic capacitor. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 1 is a cross-sectional view schematically showing a laminated ceramic capacitor 1 according to one embodiment of the present invention. DETAILED DESCRIPTION
[0018] Reference Figure 1 , the structure of a multilayer ceramic capacitor 1 according to one embodiment of the present invention will be described.
[0019] A laminated ceramic capacitor 1 includes a laminate 2. The laminate 2 includes a plurality of laminated dielectric layers 3 containing ceramics, and a plurality of internal electrodes 4 and 5 arranged along interfaces between the plurality of dielectric layers 3. The internal electrodes 4 and 5 are classified into a plurality of first internal electrodes 4 and a plurality of second internal electrodes 5 arranged alternately in the stacking direction of the laminate 3. A first external electrode 6 and a second external electrode 7 are provided on the outer surface of the laminate 2, more specifically, on each of the opposite end surfaces. The first external electrode 6 is electrically connected to the first internal electrode 4, and the second external electrode 7 is electrically connected to the second internal electrode 5.
[0020] The dielectric layer 3 includes, for example, a ceramic having ABO3 as a main component (A is at least one of Ba, Ca and Sr, and B is at least one of Ti and Zr). In addition, the ceramic may also include the above-mentioned ABO3 as a main component and further include at least one of Mn, Mg, Si, Y, Dy and Gd as a subcomponent.
[0021] The internal electrodes 4 and 5 contain a silver / palladium alloy as a conductive component. Furthermore, as a characteristic composition, the internal electrodes 4 and 5 contain (Ag 0.7 ,Pd 0.3 )At least one selected from TiO3, NaTiO3 and EuTiO3. (Ag 0.7 ,Pd 0.3 )TiO3, NaTiO3 and EuTiO3 have ilmenite crystal structure.
[0022] In addition, according to the experimental examples described later, in a preferred embodiment, the dielectric layer 3 includes a ceramic having at least one selected from BaTiO3, SrTiO3 and CaZrO3 as a main component, the internal electrodes 4 and 5 include a silver / palladium alloy as a conductive component, and the ceramic material includes (Ag 0.7 ,Pd 0.3 )At least one selected from TiO3, NaTiO3 and EuTiO3, and if necessary, at least one selected from BaTiO3, SrTiO3 and CaZrO3 contained in the dielectric layer 3.
[0023] The external electrodes 6 and 7 are formed, for example, by applying a conductive paste containing Ag or Cu as the main conductive component to the end faces of the stacked body 2 and then sintering it. If necessary, Ni plating, for example, may be performed on the thick film formed by sintering, and Sn plating may be performed thereon.
[0024] The multilayer ceramic capacitor 1 is manufactured, for example, through the following process. First, a ceramic slurry containing raw material powder of a ceramic having the composition as described above is prepared. Next, a suitable sheet forming method is applied to the ceramic slurry to form ceramic green sheets. Next, a conductive paste that should become each of the internal electrodes 4 and 5 is applied to a given ceramic green sheet among the plurality of ceramic green sheets by printing or the like. Next, after stacking the plurality of ceramic green sheets, they are crimped to obtain an unprocessed stack. Next, the unprocessed stack is fired. In this firing process, the ceramic green sheets become dielectric layers 3. Then, external electrodes 6 and 7 are formed on the end faces of the stack 3.
[0025] The conductive paste to be used as the internal electrodes 4 and 5 when manufacturing the above-mentioned multilayer ceramic capacitor 1 is preferably prepared as follows.
[0026] When preparing the conductive paste, a first step is implemented to prepare a ceramic powder slurry containing ceramic powder, an organic solvent and a dispersant, a second step is implemented to prepare a metal powder slurry containing conductive metal powder, an organic solvent and a dispersant, a third step is implemented to prepare an organic vehicle containing an organic resin component and an organic solvent, and a fourth step is implemented to mix the above-mentioned ceramic powder slurry, metal powder slurry and organic vehicle.
[0027] More specifically, in the first step, ceramic powder and a dispersant are mixed in an organic solvent to prepare a ceramic powder slurry.
[0028] As the ceramic powder, for example, a powder containing (Ag) as ABO3 oxide can be used. 0.7 ,Pd 0.3 )Ceramic powder containing at least one selected from among TiO3, NaTiO3 and EuTiO3, and in addition thereto, ceramic powder containing at least one selected from among BaTiO3, SrTiO3 and CaZrO3 as common materials may be used.
[0029] The conductive metal powder contained in the metal powder paste prepared in the second step described later contains a silver / palladium alloy, so the above-mentioned ABO3 oxide (Ag 0.7 ,Pd 0.3 )TiO3, NaTiO3 and EuTiO3 are ABO3 type oxides with a specific ionic radius in which the ratio of the ionic radius of the element at the A position in ABO3 at 6 coordination to the ionic radius of the silver / palladium alloy at 6 coordination is greater than 0.96 and less than 1.10.
[0030] According to the inclusion of (Ag 0.7 ,Pd 0.3) At least one ceramic powder selected from TiO3, NaTiO3 and EuTiO3 can suppress the reaction that may occur with the conductive metal powder contained in the metal powder slurry prepared in the second step during firing. The ceramic powder can also contain the above-mentioned ABO3 oxide as a main component and further contain at least one of Mn, Mg, Si, Y, Dy and Gd as a secondary component. When such secondary components are contained, the particle growth of ceramic particles can be suppressed, and sometimes the sintering of metal particles can be effectively suppressed.
[0031] As the dispersant to be mixed with the ceramic powder in the first step, for example, an anionic polymer dispersant can be used, and as the organic solvent, for example, dihydroterpineol can be used.
[0032] In the second step, a metal powder slurry is prepared by mixing a conductive metal powder and a dispersant in an organic solvent. As the conductive metal powder, for example, a powder of an alloy containing 70 atm% of silver and 30 atm% of palladium can be used. As the dispersant and organic solvent used in the second step, the same dispersant and organic solvent as those used in the first step can be used.
[0033] In the third step, an organic vehicle is prepared by mixing an organic resin component with an organic solvent. As the organic resin component, for example, ethyl cellulose resin can be used. The organic solvent used in the third step can also be the same as the organic solvent used in the first step.
[0034] In the fourth step, the ceramic powder slurry, metal powder slurry and organic vehicle are mixed. Thus, a conductive paste to be used as the internal electrodes 4 and 5 is obtained. The conductive paste contains the ceramic powder slurry, and the ceramic powder slurry contains (Ag) containing ABO3 oxides of a specific ionic radius as described above. 0.7 ,Pd 0.3 )TiO3, NaTiO3 and EuTiO3, the internal electrodes 4 and 5 included in the laminated ceramic capacitor 1 manufactured through the firing step become composed of (Ag 0.7 ,Pd 0.3 )At least one selected from TiO3, NaTiO3 and EuTiO3.
[0035] [Experimental example]
[0036] Next, an experimental example conducted to confirm the effects of the present invention will be described.
[0037] In this experimental example, as the conductive metal powder contained in the conductive paste for forming the internal electrode, a silver / palladium alloy powder containing an alloy of 70 atm % of silver and 30 atm % of palladium was prepared.
[0038] On the other hand, as the ABO3 oxide with a specific ionic radius constituting the ceramic powder contained in the conductive paste for forming the internal electrode, in addition to (Ag 0.7 , Pd 0.3 )TiO3, NaTiO3 and EuTiO3, BaTiO3, CaZrO3 and SrTiO3 were also prepared. In Table 1, "Crystal Structure", "Coordination Number", "A-site Element" and "Ionic Radius" are shown for these ABO3 oxides. In addition, Ba, Ca and Sr are 12-coordinated in the original perovskite structure, but Ba, Ca and Sr are also 6-coordinated when they are continuously dissolved in the 6-coordinated elements (Ag / Pd, Na, Eu) of the ilmenite structure, so the "Ionic Radius" in Table 1 shows the value under 6-coordinated.
[0039] [Table 1]
[0040] Table 1
[0041]
[0042] Hereinafter, Experimental Examples 1, 2, and 3 which were carried out by changing the ceramic raw material constituting the dielectric layer will be described.
[0043] (Experimental Example 1) Main component of ceramic constituting dielectric layer: BaTiO3
[0044] 1. Preparation of BaTiO3-based ceramic raw materials constituting the dielectric layer
[0045] As starting materials, powders of BaCO3 and TiO2 as main components were weighed, mixed for 72 hours by ball mill, and then heat treated for 2 hours at a maximum temperature of 1000°C to obtain heat-treated powder. On the other hand, powders of MnO, Dy2O3, MgO, SiO2 and BaCO3 were prepared as auxiliary components, and the heat-treated powders were weighed so that the auxiliary component powders had a composition ratio of 100BaTiO3+0.5Mn+1.0Dy+1.0Mg+1.0Si+2.0Ba. These auxiliary component powders were added to the heat-treated powders, mixed for 24 hours by ball mill, and then dried to obtain BaTiO3-based ceramic raw material powders.
[0046] 2. Preparation of conductive paste for internal electrode formation
[0047] As ceramic powders contained in the conductive paste for forming the internal electrode, powders of "ABO 3 oxides" shown in Table 2 described later and the BaTiO 3 -based ceramic raw material powder for the dielectric layer were used.
[0048] The powders of these "ABO3 oxides" and BaTiO3-based ceramic raw material powders were weighed to obtain the "addition ratio" shown in Table 2. These powders, dihydropinene as an organic solvent, and anionic polymer dispersant as a dispersant were premixed in a medium-free stirring mill, and then dispersed in a medium stirring mill to prepare a ceramic powder slurry (first step).
[0049] Meanwhile, a silver / palladium alloy powder as a conductive metal powder, dihydroterpineol as an organic solvent, and an anionic polymer dispersant as a dispersant were dispersed using a triple roll mill to prepare a metal powder slurry (second step).
[0050] Furthermore, ethyl cellulose resin as an organic resin component and dihydroterpineol as an organic solvent were mixed to obtain an organic vehicle (third step).
[0051] Next, the metal powder slurry and the ceramic powder slurry are added to the organic vehicle and mixed and dispersed to prepare a conductive paste for forming an internal electrode (fourth step).
[0052] Table 2 shows the ratio of the ionic radius of the A-site element at hexacoordination to the ionic radius of the silver / palladium alloy to be contained in the internal electrode at hexacoordination, that is, the “ionic radius ratio (A-site element / Ag 0.7 Pd 0.3 Alloy)". In addition, for sample 7, the ionic radius of the Ba element at 6 coordination as shown in Table 1 is shown. Relative to the ionic radius of the silver / palladium alloy under 6 coordination ratio.
[0053] 3. Fabrication of multilayer ceramic capacitors
[0054] A ceramic slurry containing the BaTiO3-based ceramic raw material powder prepared in the above 1 is prepared, and then a ceramic green sheet is formed by applying a doctor blade method to the ceramic slurry. Next, the conductive paste for forming the internal electrode prepared in the above 2 is applied to a given ceramic green sheet among the plurality of ceramic green sheets by screen printing. Next, a plurality of ceramic green sheets are stacked and then crimped to obtain an unprocessed laminate. Next, the unprocessed laminate is fired. Then, external electrodes are formed on the end faces of the sintered laminate to produce a laminated ceramic capacitor as a sample.
[0055] 4. Evaluation
[0056] [Table 2]
[0057] Table 2
[0058]
[0059] The internal electrode and the dielectric layer located at the center of the stacked body in the height direction of the stacked ceramic capacitor serving as a sample were separated from each other by electric field separation.
[0060] Next, the central part (the position of 1 / 2 in the width direction and 1 / 2 in the length direction) of the exposed internal electrode was observed at a magnification of 100 times using a microscope. Then, the obtained image was analyzed to find the ratio of the area occupied by the conductor film as the internal electrode in the exposed part, which was given as the "coverage" shown in Table 2. Samples with a "coverage" of 80% or more were judged to be good and were marked with "○" in the "Evaluation" column, and samples with a "coverage" of less than 80% were judged to be poor and were marked with "×" in the "Evaluation" column.
[0061] 5. Inspection
[0062] The "Evaluation" of Samples 1 to 6 in Table 2 is "○". In these Samples 1 to 6, the internal electrodes contain (Ag 0.7 ,Pd 0.3 )TiO3, NaTiO3 and EuTiO3 are used as ABO3 oxides. In addition, the internal electrodes contain silver / palladium alloy as a conductive component.
[0063] Here, if we focus on the ionic radius, first, as shown in the "(Ag, Pd)TiO3" item in Table 1, the ionic radius of the silver / palladium alloy under hexacoordination is On the other hand, as the ABO3 oxide contained in the internal electrodes of samples 1 to 6, (Ag 0.7 , Pd 0.3 The ionic radii of the elements at the A-position of )TiO3, NaTiO3 and EuTiO3 under 6 coordination are shown in Table 1. as well as
[0064] In samples 1 to 6 evaluated as "○", the ratio of the ionic radius of the element at the A-site in ABO3 at hexacoordination to the ionic radius of the silver / palladium alloy at hexacoordination, i.e., the "ionic radius ratio" was 0.96 or more and 1.10 or less.
[0065] As such, the ABO3 oxides (Ag 0.7 ,Pd 0.3)TiO3, NaTiO3 and EuTiO3 have an ionic radius of 6 coordination of the element at the A position in ABO3 equal to or close to the ionic radius of 6 coordination of the silver / palladium alloy as the conductive metal to be contained in the internal electrode, so the energy difference with the silver / palladium alloy in the internal electrode is 0 or becomes small, so it will not be ejected from the internal electrode part and remain, playing a role in improving the heat resistance of the internal electrode. As a result, in samples 1 to 6, it is estimated that the coverage rate becomes as high as 82% or more.
[0066] In addition, as in samples 4 to 6, (Ag 0.7 ,Pd 0.3 The addition ratio of TiO3, NaTiO3 and EuTiO3 is not necessarily 100%, as long as it is 10% or more, and the addition ratio of Ag 0.7 ,Pd 0.3 )When compared with any of TiO3, NaTiO3 and EuTiO3, the effect of improving the coverage was confirmed.
[0067] In contrast to these samples, in sample 7 evaluated as "×", only BaTiO3, which is a common material, is added to the internal electrode. In this case, Ba, which is an element at the A position in ABO3 of the perovskite structure, is 12-coordinated, but when solid-dissolving in the A position of the ilmenite structure, it is necessary to compare the ionic radius at the 6-coordinated position, which is the coordination number of the A position of the ilmenite structure. The ionic radius of Ba at the 6-coordinated position is shown in Table 1. Therefore, the ratio of the ionic radius of Ba in hexacoordination to the ionic radius of the silver / palladium alloy in hexacoordination, that is, the "ionic radius ratio" is 1.27. Therefore, the "ionic radius ratio" deviates from the range of 0.96 to 1.10, and the coverage is reduced to 75%.
[0068] In Sample 7, the "ion radius ratio" deviated from the range of 0.96 to 1.10, presumably because BaTiO 3 was ejected from the internal electrode portion, the heat resistance of the internal electrode was not improved, and the coverage was reduced.
[0069] (Experimental Example 2) Main component of ceramic constituting dielectric layer: CaZrO3
[0070] 1. Preparation of CaZrO3-based ceramic raw materials constituting the dielectric layer
[0071] As starting materials, powders of CaCO3 and ZrO2 as main components and powders of MnO, SiO2 and MgO as auxiliary components were weighed, mixed for 72 hours in a ball mill, and then heat treated at a maximum temperature of 1000°C for 2 hours to obtain CaZrO3-based ceramic raw material powder.
[0072] 2. Preparation of conductive paste for internal electrode formation
[0073] As ceramic powders contained in the conductive paste for forming the internal electrode, powders of "ABO 3 oxides" shown in Table 3 described later and the CaZrO 3 -based ceramic raw material powder for the dielectric layer were used.
[0074] These "ABO3 oxide" powders and CaZrO3-based ceramic raw material powders were weighed so as to achieve the "addition ratio" shown in Table 3, and a conductive paste for forming internal electrodes was prepared through the same steps as in the above-mentioned Experimental Example 1.
[0075] In Table 3, as in Table 2, the “ion radius ratio (A-site element / Ag 0.7 Pd 0.3 Alloy)". In addition, for sample 17, the ionic radius of the Ca element at 6 coordination as shown in Table 1 is shown. Relative to the ionic radius of the silver / palladium alloy under 6 coordination ratio.
[0076] 3. Fabrication of multilayer ceramic capacitors
[0077] A ceramic slurry containing the CaZrO3-based ceramic raw material powder prepared in the above step 1 was prepared, and then a ceramic green sheet was formed by applying a doctor blade method to the ceramic slurry. Thereafter, a laminated ceramic capacitor serving as a sample was prepared through the same steps as in Experimental Example 1.
[0078] 4. Evaluation
[0079] [Table 3]
[0080] Table 3
[0081]
[0082] According to the same procedure as in Experimental Example 1, the “coverage ratio” was obtained as shown in Table 3, and evaluation was performed in the same manner.
[0083] 5. Inspection
[0084] The "Evaluation" of Samples 11 to 16 in Table 3 is "○". In these Samples 11 to 16, the internal electrodes contain (Ag 0.7 ,Pd 0.3 )TiO3, NaTiO3 and EuTiO3 are used as ABO3 oxides. In addition, the internal electrodes contain silver / palladium alloy as a conductive component.
[0085] Here, if we focus on the ionic radius, first, as shown in the "(Ag, Pd)TiO3" item in Table 1, the ionic radius of the silver / palladium alloy under hexacoordination is On the other hand, as the ABO3 oxide contained in the internal electrodes of samples 11 to 16, (Ag 0.7 ,Pd 0.3 The ionic radii of the elements at the A-position of )TiO3, NaTiO3 and EuTiO3 under 6 coordination are shown in Table 1. as well as
[0086] In samples 11 to 16 evaluated as "○", the ratio of the ionic radius of the element at the A-site in ABO3 at hexacoordination to the ionic radius of the silver / palladium alloy at hexacoordination, i.e., the "ionic radius ratio" was 0.96 or more and 1.10 or less.
[0087] As such, the ABO3 oxides (Ag 0.7 ,Pd 0.3 )TiO3, NaTiO3 and EuTiO3 have an ionic radius of 6-coordinated elements at the A position in ABO3 that is equal to or close to the ionic radius of 6-coordinated silver / palladium alloy, which is a conductive metal that should be included in the internal electrode. Therefore, the energy difference with the silver / palladium alloy in the internal electrode is 0 or becomes smaller, so they will not be ejected from the internal electrode portion but remain, which plays a role in improving the heat resistance of the internal electrode. As a result, in samples 11 to 16, it is estimated that the coverage rate is increased to more than 81%.
[0088] In addition, as in samples 14 to 16, (Ag 0.7 , Pd0.3)TiO3, NaTiO3 and EuTiO3 do not have to be added in an amount of 100%, but as long as it is 10% or more, it is equivalent to not containing (Ag 0.7 , Pd 0.3 )When compared with any of TiO3, NaTiO3 and EuTiO3, the effect of improving the coverage was confirmed.
[0089] In contrast to these samples, in sample 17, which was evaluated as "×", only CaZrO3, which is a common material, was added to the internal electrode. In this case, Ca, which is an element at the A site in ABO3 of the perovskite structure, is 12-coordinated, but when solid-dissolving in the A site of the ilmenite structure, it is necessary to compare the ionic radius at the 6-coordinated site, which is the coordination number of the A site of the ilmenite structure. The ionic radius of Ca at the 6-coordinated site is shown in Table 1. Therefore, the ratio of the ionic radius of Ca in hexacoordination to the ionic radius of the silver / palladium alloy in hexacoordination, that is, the "ionic radius ratio" is 0.94. Therefore, the "ionic radius ratio" deviates from the range of 0.96 to 1.10, and the coverage rate decreases to 72%.
[0090] In Sample 17, the “ion radius ratio” deviated from the range of 0.96 to 1.10, presumably because CaZrO 3 was ejected from the internal electrode portion, the heat resistance of the internal electrode was not improved, and the coverage rate was reduced.
[0091] (Experimental Example 3) Main component of ceramic constituting dielectric layer: SrTiO3
[0092] 1. Preparation of SrTiO3-based ceramic raw materials constituting the dielectric layer
[0093] As starting materials, powders of SrCO3 and TiO2 as main components and powders of MnO, SiO2 and MgO as auxiliary components were weighed, mixed for 72 hours in a ball mill, and then heat treated at a maximum temperature of 1000°C for 2 hours to obtain SrTiO3-based ceramic raw material powder.
[0094] 2. Preparation of conductive paste for internal electrode formation
[0095] As ceramic powders contained in the conductive paste for forming the internal electrode, powders of "ABO 3 oxides" shown in Table 4 described later and the SrTiO 3 -based ceramic raw material powder for the dielectric layer were used.
[0096] These "ABO3 oxide" powders and SrTiO3-based ceramic raw material powders were weighed so as to achieve the "addition ratio" shown in Table 4, and a conductive paste for forming an internal electrode was prepared through the same steps as in the above-mentioned Experimental Example 1.
[0097] In Table 4, as in Table 2, the “ion radius ratio (A-site element / Ag 0.7 Pd 0.3 Alloy)". In addition, for sample 27, the ionic radius of the Sr element at 6 coordination as shown in Table 1 is shown. Relative to the ionic radius of the silver / palladium alloy under 6 coordination ratio.
[0098] 3. Fabrication of multilayer ceramic capacitors
[0099] A ceramic slurry containing the SrTiO3-based ceramic raw material powder prepared in the above 1 was prepared, and then a ceramic green sheet was formed by applying a doctor blade method to the ceramic slurry. Thereafter, a laminated ceramic capacitor serving as a sample was prepared through the same steps as in Experimental Example 1.
[0100] 4. Evaluation
[0101] [Table 4]
[0102] Table 4
[0103]
[0104] According to the same procedure as in Experimental Example 1, the “coverage ratio” was obtained as shown in Table 4, and evaluation was performed in the same manner.
[0105] 5. Inspection
[0106] The "Evaluation" of Samples 21 to 26 in Table 4 is "○". In these Samples 21 to 26, the internal electrodes contain (Ag 0.7 ,Pd 0.3 )TiO3, NaTiO3 and EuTiO3 are used as ABO3 oxides. In addition, the internal electrodes contain silver / palladium alloy as a conductive component.
[0107] Here, if we focus on the ionic radius, first, as shown in the "(Ag, Pd)TiO3" item in Table 1, the ionic radius of the silver / palladium alloy under hexacoordination is On the other hand, as the ABO3 oxide contained in the internal electrodes of samples 21 to 26, (Ag 0.7 ,Pd 0.3 The ionic radii of the elements at the A-position of )TiO3, NaTiO3 and EuTiO3 under 6 coordination are shown in Table 1. as well as
[0108] In samples 21 to 26 evaluated as "○", the ratio of the ionic radius of the element at the A-site in ABO3 at hexacoordination to the ionic radius of the silver / palladium alloy at hexacoordination, i.e., the "ionic radius ratio" was 0.96 or more and 1.10 or less.
[0109] Thus, the ABO3 oxides (Ag 0.7 ,Pd 0.3 )TiO3, NaTiO3 and EuTiO3 have an ionic radius of 6-coordinated elements at the A position in ABO3 that is equal to or close to the ionic radius of 6-coordinated silver / palladium alloy, which is a conductive metal that should be included in the internal electrode. Therefore, the energy difference with the silver / palladium alloy in the internal electrode is 0 or becomes smaller, so they will not be ejected from the internal electrode portion but remain, which plays a role in improving the heat resistance of the internal electrode. As a result, in samples 21 to 26, it is estimated that the coverage rate is increased to more than 80%.
[0110] In addition, as in samples 24 to 26, (Ag 0.7 ,Pd 0.3 The addition ratio of TiO3, NaTiO3 and EuTiO3 is not necessarily 100%, as long as it is 10% or more, and the addition ratio of Ag 0.7 ,Pd 0.3)When compared with any of TiO3, NaTiO3 and EuTiO3, the effect of improving the coverage was confirmed.
[0111] In contrast to these samples, in sample 27, which was evaluated as "×", only SrTiO3, which is a common material, was added to the internal electrode. In this case, Sr, which is an element at the A site in ABO3 of the perovskite structure, is 12-coordinated, but when solid-dissolving in the A site of the ilmenite structure, it is necessary to compare the ionic radius at the 6-coordinated site, which is the coordination number of the A site of the ilmenite structure. The ionic radius of Sr at the 6-coordinated site is shown in Table 1. Therefore, the ratio of the ionic radius of Sr at 6 coordination to the ionic radius of the silver / palladium alloy at 6 coordination, that is, the "ionic radius ratio" is 1.11. Therefore, the "ionic radius ratio" deviates from the range of 0.96 to 1.10, and the coverage is reduced to 70%.
[0112] In Sample 27, the “ion radius ratio” deviated from the range of 0.96 to 1.10, presumably because SrTiO 3 was ejected from the internal electrode portion, the heat resistance of the internal electrode was not improved, and the coverage was reduced.
[0113] The present invention may be implemented as follows.
[0114] <1>
[0115] A laminated ceramic capacitor comprises: a laminate having a plurality of laminated dielectric layers containing ceramics, and a plurality of internal electrodes respectively arranged along a plurality of interfaces between the dielectric layers,
[0116] The internal electrode includes a silver / palladium alloy as a conductive component and includes (Ag 0.7 ,Pd 0.3 )At least one selected from TiO3, NaTiO3 and EuTiO3.
[0117] <2>
[0118] according to <1> The multilayer ceramic capacitor, wherein:
[0119] The internal electrode has a thickness of 1 μm or less.
[0120] <3>
[0121] according to <1> or <2> The multilayer ceramic capacitor, wherein:
[0122] The internal electrodes have a coverage rate of 80% or more.
[0123] <4>
[0124] according to <1> to <3> The multilayer ceramic capacitor according to any one of the preceding claims, wherein:
[0125] The dielectric layer includes ceramics containing at least one selected from BaTiO 3 , SrTiO 3 , and CaZrO 3 as a main component, and the internal electrode further includes at least one selected from BaTiO 3 , SrTiO 3 , and CaZrO 3 included in the dielectric layer.
[0126] Description of Reference Numerals
[0127] 1: Multilayer ceramic capacitor;
[0128] 2: laminate;
[0129] 3: Dielectric layer;
[0130] 4, 5: internal electrodes;
[0131] 6, 7: External electrodes.
Claims
1. A laminated ceramic capacitor comprising: a laminate having a plurality of laminated dielectric layers containing ceramics, and a plurality of internal electrodes respectively arranged along a plurality of interfaces between the dielectric layers; The internal electrode includes a silver / palladium alloy as a conductive component and includes (Ag 0.7 , Pd 0.3 )At least one selected from TiO3, NaTiO3 and EuTiO3.
2. The multilayer ceramic capacitor according to claim 1, wherein The internal electrode has a thickness of 1 μm or less.
3. The multilayer ceramic capacitor according to claim 1 or 2, wherein: The internal electrodes have a coverage rate of 80% or more.
4. The multilayer ceramic capacitor according to any one of claims 1 to 3, wherein The dielectric layer includes ceramics containing at least one selected from BaTiO 3 , SrTiO 3 , and CaZrO 3 as a main component, and the internal electrode further includes at least one selected from BaTiO 3 , SrTiO 3 , and CaZrO 3 included in the dielectric layer.