Preparation method and regeneration process of renewable gas gel desulfurizer
Renewable aerogel desulfurizer was prepared by using silica nanofiber aerogel carrier and metal salt solution in the dry desulfurizer to carry out hydrothermal reaction, combined with microwave oxidation and NaF solution treatment, and solving the existing technology The problems of low utilization rate and poor regeneration performance of the desulfurizer active components have achieved efficient H2S adsorption and reaction, and extended service life.
Patent Information
- Application Number
- CN202411100141.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The existing dry desulfurizers are prone to volatilization during the high-temperature regeneration process, resulting in a degradation of performance, and a high regeneration temperature and a short service life, making it difficult to meet the requirements of industrial applications.
The silica nanofiber aerogel carrier was used to carry out hydrothermal reaction in a mixed solution of zinc nitrate and cobalt nitrate to produce ZnCo2O4 active components, and a renewable aerogel desulfurization agent was prepared by microwave oxidation treatment, combined with NaF solution soaking and Microwave plasma treatment reduces the regeneration reaction temperature and improves the recycling performance of the desulfurizer.
It realizes efficient H2S adsorption and reaction, improves the utilization rate and regeneration rate of the active components of the desulfurizer, reduces the regeneration reaction temperature, extends the service life of the desulfurizer, and significantly improves the sulfur capacity and regeneration performance.
Smart Images

Figure CN118904049A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coal chemical desulfurization agent preparation, and in particular to a preparation method and a regeneration process of a renewable aerogel desulfurization agent. Background Art
[0002] As one of the three major fossil energy sources, coal plays an important role in economic development. However, the various environmental problems caused by the direct combustion of coal have to attract people's attention. Integrated gasification combined cycle power generation technology (IGCC) is based on the clean and efficient use of coal and has been widely used in many countries and regions. As the power and raw material source in IGCC technology, coal gas contains a large amount of sulfide, of which more than 90% is hydrogen sulfide (H2S) gas. Hydrogen sulfide not only corrodes industrial equipment and poisons catalysts, but also threatens the ecological environment and human health when discharged into the atmosphere. Therefore, the hydrogen sulfide in coal gas must be removed before use.
[0003] Dry desulfurization uses the metal oxides in the solid phase desulfurizer to convert and remove H2S by chemical reaction. This method has the advantages of simple process flow, no wastewater and waste acid treatment problems, low energy consumption, low corrosion to equipment, and low cost. Studies have shown that desulfurizers with zinc oxide as the active component have higher desulfurization accuracy and desulfurization efficiency than other oxide desulfurizers, but zinc oxide is easy to volatilize during high-temperature regeneration, resulting in the loss of active components and serious performance degradation. Copper oxide has a strong affinity and adsorption capacity with hydrogen sulfide. Some scholars have found that copper oxide desulfurizers have high desulfurization accuracy, are less affected by temperature, and have good regeneration performance.
[0004] However, the dry desulfurization technology currently used has the disadvantages of large desulfurization agent loading, frequent desulfurization agent replacement, difficulty in regenerating waste desulfurization agents, and difficulty in solid waste treatment. Although the existing desulfurization agent preparation method and regeneration process are relatively mature, they still have the disadvantages of high regeneration temperature, short service life due to regeneration difficulties, and high operating costs. Therefore, the existing desulfurization agent cannot meet the requirements of actual industrial applications, and the development of a new type of highly efficient regenerable solid desulfurization agent with high desulfurization efficiency, speed and selectivity is still one of the goals of gas desulfurization technology. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation method and regeneration process of a regenerable aerogel desulfurizer to solve the problems of low utilization rate of active components in the desulfurizer reaction process and poor vulcanization-regeneration performance of the desulfurizer, and ultimately improve the vulcanization and recycling performance of the desulfurizer.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] One of the technical solutions of the present invention: a method for preparing a renewable aerogel desulfurizer, comprising the following steps: subjecting a silica nanofiber aerogel carrier to a hydrothermal reaction in a mixed solution of zinc nitrate and cobalt nitrate to generate an active component ZnCo2O4 in the silica nanofiber aerogel carrier to obtain a desulfurizer precursor; and subjecting the desulfurizer precursor to an oxidation treatment under a microwave field to obtain the renewable aerogel desulfurizer.
[0008] Furthermore, the porosity of the silica nanofiber aerogel carrier is 95-99.99%, and the diameter of the silica nanofibers is 100-1000 nm.
[0009] Furthermore, the molar ratio of zinc nitrate to cobalt nitrate in the mixed solution is 1:1-4, and the concentration of zinc nitrate is 0.1 mol / L.
[0010] Furthermore, the temperature of the hydrothermal reaction is 80-110° C. and the time is 1-4 hours.
[0011] Furthermore, the amount ratio of the silica nanofiber aerogel carrier to the mixed solution of zinc nitrate and cobalt nitrate during the hydrothermal reaction is 0.4 g:100 mL. The active component ZnCo2O4 is generated during the hydrothermal reaction.
[0012] Furthermore, the microwave condition of the microwave field is 1000W.
[0013] Furthermore, the specific parameters of the oxidation treatment include: oxygen concentration of 1-4 vol%, calcination temperature of 200-350° C., and calcination time of 1 h.
[0014] The second technical solution of the present invention: a renewable aerogel desulfurizer prepared by the above-mentioned preparation method.
[0015] Furthermore, the renewable aerogel desulfurizer uses silica nanofiber aerogel as a carrier, and the carrier is loaded with an active component ZnCo2O4, which can be called a ZnCo2O4 / silicon dioxide nanofiber aerogel composite desulfurizer.
[0016] Furthermore, the content of ZnCo2O4 in the renewable aerogel desulfurizer is 56.6-57.9wt%.
[0017] The third technical solution of the present invention: A method for regenerating the above-mentioned renewable aerogel desulfurizer comprises the following steps: soaking the renewable aerogel desulfurizer after the desulfurization reaction in a NaF solution for 12 hours, placing it under a microwave field after drying, and sequentially introducing hydrogen, argon, and oxygen for heat treatment to obtain a regenerated desulfurizer.
[0018] Furthermore, the renewable aerogel desulfurizer after the desulfurization reaction is specifically a renewable aerogel desulfurizer after absorbing H2S to saturation, that is, the desulfurization reaction is carried out until the renewable aerogel desulfurizer is saturated with H2S.
[0019] Furthermore, the concentration of the NaF solution is 1-4 mmol / L.
[0020] Furthermore, the concentration of hydrogen is 2-8 vol%, the concentration of oxygen is 1-4 vol%, and the balance gas when hydrogen and oxygen are introduced is nitrogen. That is, when hydrogen is introduced, a mixed gas of hydrogen and nitrogen is introduced, and when oxygen is introduced, a mixed gas of oxygen and nitrogen is introduced.
[0021] Furthermore, the argon gas is pure argon gas.
[0022] Furthermore, the microwave condition of the microwave field is 1000W.
[0023] Furthermore, when hydrogen is introduced for heat treatment, the heat treatment temperature is 500°C, and the heat treatment time is 30 minutes; when argon is introduced for heat treatment, the heat treatment temperature is 500°C, and the heat treatment time is 30 minutes; when oxygen is introduced for heat treatment, the heat treatment temperature is 400°C, and the heat treatment time is 2 hours.
[0024] The first two gases will generate plasma under the action of microwave field, which will modify the surface and bulk of the desulfurizer after desulfurization, making its chemical properties more active and easier to undergo chemical reactions; the role of oxygen is to regenerate the desulfurizer.
[0025] Furthermore, the specific operation of the desulfurization reaction is: placing the renewable aerogel desulfurizer in a fixed bed reaction device for 2000h -1 Coal gas is introduced at a space velocity of , and desulfurization reaction is carried out at 500°C.
[0026] The present invention discloses the following technical effects:
[0027] The present invention uses silicon dioxide nanofiber aerogel as a carrier and prepares a ZnCo2O4 / silicon dioxide nanofiber aerogel composite desulfurizer by means of metal salt solution hydrothermal reaction, oxidation treatment, etc. It has the following advantages:
[0028] (1) The present invention uses nanofiber aerogel as a carrier to prepare a desulfurizer. The nanofiber aerogel has the characteristics of open pore structure, high flexibility, and stable physical structure. It can not only provide support for the overall structure of the desulfurizer, but also promote the H2S adsorption and reaction process and maintain the long-term cyclic performance of the desulfurizer.
[0029] (2) The process steps of the present invention are simple, highly controllable, and easy to operate, which can meet the large market demand. The nanofiber aerogel has good support, high flexibility, toughness, strength, high porosity, and large specific surface area, and can achieve multi-component composite and multi-level structural synergy.
[0030] (3) More importantly, the present invention combines zinc and cobalt, which can not only form a composite oxide, improve the stability of zinc and the regeneration performance of the desulfurizer, but also reduce the stability of the composite oxide lattice structure based on the difference in the size of zinc and cobalt ions. On this basis, the lattice diffusion of zinc and cobalt ions and the promotion of metal ion migration by microwave radiation during the low-temperature oxidation treatment process produce a significant Kirkendall effect, thereby causing the zinc-cobalt composite oxide to produce a large number of lattice defects (metal ion defects and oxygen vacancies) and even transform into a hollow structure. During the regeneration of the desulfurizer, by immersing in NaF solution, the addition of fluorine element can form a close bond with the metal and weaken the metal-sulfur chemical bond. At the same time, hydrogen and argon generate plasma under the action of microwave radiation, which can treat the surface defects of the desulfurizer after adsorption saturation and produce a large number of sulfur vacancies (such as Figure 1 As shown). On this basis, the lattice defects and surface defects contained in the desulfurizer are conducive to the adsorption and dissociation of oxygen by the desulfurizer during the oxidation regeneration process, and are also conducive to weakening the chemical bond between metal and sulfur and reducing the bond breaking activation energy, thereby reducing the regeneration reaction temperature, reducing the diffusion resistance of oxygen and sulfur ions, and preventing the desulfurizer from the adverse effects of high-temperature sintering, maintaining a high-efficiency gas-solid reaction rate and mass transfer efficiency, and improving the recycling performance of the desulfurizer. According to tests, the desulfurizer prepared by the method of the present invention not only has a sulfur capacity of 28.3% and an active component utilization rate of 99.9%, but also the oxidation regeneration reaction temperature is reduced to 400°C when the desulfurizer regeneration rate reaches 99.0%; after the regenerated desulfurizer is used for ten times of sulfurization-regeneration cycles, the sulfur capacity can still reach 28.2%. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 The figure is a comparison of the sulfur vacancy concentrations of the desulfurizer after absorption saturation in Example 1 before and after being immersed in a NaF solution and heat-treated by passing hydrogen and argon. DETAILED DESCRIPTION
[0033] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0034] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0035] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0036] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0037] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0038] The silica nanofiber aerogel carrier used in the following examples and comparative examples has a porosity of 99%, and the average diameter of the silica nanofibers therein is 500 nm. The silica nanofiber aerogel carrier can be purchased on the market, or prepared by conventional methods, such as using airflow-assisted electrostatic spinning, nanofiber body reconstruction, and freeze-drying technology to prepare SiO2 into silica nanofiber aerogel. The specific preparation details are not limited, as long as the requirements for porosity and average diameter of nanofibers are met, and the specific preparation details do not affect the presentation of the technical effect of this solution.
[0039] The test and calculation methods of the sulfur capacity, active component utilization rate and desulfurizer regeneration rate in the following examples and comparative examples are as follows:
[0040] The desulfurization performance of the sample is evaluated by the breakthrough sulfur capacity. The H2S concentration in the inlet gas is 1000ppm. When the H2S concentration in the outlet gas reaches 300ppm, it is considered that the desulfurizer has penetrated, and the time consumed at this time is considered as the breakthrough time. The breakthrough sulfur capacity is converted into the mass (g) of elemental sulfur absorbed by 100g of desulfurizer from the start of the experiment to the breakthrough time. The detailed calculation method is as follows:
[0041]
[0042] Where: F is the flow rate of simulated gas (mL / min), M s is the molar mass of S (32.06 g / mol), V m is the molar volume of the gas at 25°C and 101.325 kPa (24.5 L / mol); C0 and C represent the inlet and outlet concentrations of H2S, respectively (ppm); M 脱硫剂 Corresponding to the mass of desulfurizer (g).
[0043] Active component utilization rate = actual sulfur capacity / theoretical sulfur capacity × 100%.
[0044] Regeneration rate = (mass lost by the desulfurizer during regeneration / mass increased by the desulfurizer during the desulfurization reaction) × 100%.
[0045] Example 1
[0046] (1) Preparation of renewable aerogel desulfurizer, the steps are as follows:
[0047] 1) Preparation of desulfurizer precursor: 2.97 g zinc nitrate (specifically Zn(NO3)2·6H2O, 0.01 mol) and 11.64 g cobalt nitrate (specifically Co(NO3)2·6H2O, 0.04 mol), precursors of the active component ZnCo2O4, were dissolved in 100 mL of water to obtain a mixed solution of zinc nitrate and cobalt nitrate as a hydrothermal reaction solution; a silica nanofiber aerogel carrier was subjected to a hydrothermal reaction in the hydrothermal reaction solution (the amount ratio of silica nanofiber aerogel to hydrothermal reaction solution was 0.4 g:100 mL), the hydrothermal reaction temperature was 80°C, the time was 1 h, and the active component ZnCo2O4 was generated in the silica nanofiber aerogel carrier during the hydrothermal reaction. After the hydrothermal reaction, the carrier was dried to obtain a desulfurizer precursor;
[0048] 2) Preparation of desulfurizer: The desulfurizer precursor prepared in step 1) was oxidized under a 1000 W microwave field (a mixed gas with an oxygen concentration of 1 vol% was introduced, the balance gas was nitrogen, and it was calcined at 200°C for 1 h to obtain a renewable aerogel desulfurizer (the ZnCo2O4 content in the desulfurizer was 57.9 wt%).
[0049] (2) Application of desulfurizer: The desulfurizer prepared in this example (0.1 g) was placed in a fixed bed reactor at a space velocity of 2000 h -1 Texaco simulated coal gas was introduced and desulfurization reaction was carried out at 500°C until absorption saturation.
[0050] After the desulfurization reaction was completed, the sulfur capacity of the desulfurizer was detected to reach 28.3%, and the utilization rate of active components was 99.9%.
[0051] (3) Regeneration of desulfurizer: After the desulfurization reaction is completed, the desulfurizer saturated with H2S is placed in a 1mmol / L NaF solution and immersed for 12h. After drying, a mixed gas with a hydrogen concentration of 2vol% (2vol% hydrogen + 98vol% nitrogen), argon, and a mixed gas with an oxygen concentration of 1vol% (1vol% oxygen + 99vol% nitrogen) are introduced in sequence under a 1000W microwave field for heat treatment (the heat treatment temperature when hydrogen is introduced for heat treatment is 500°C and the heat treatment time is 30min; the heat treatment temperature when argon is introduced for heat treatment is 500°C and the heat treatment time is 30min; the heat treatment temperature when oxygen is introduced for heat treatment is 400°C and the heat treatment time is 2h; the space velocity is 2000h / s. -1 ) to obtain a completely regenerated desulfurizer. The regenerated desulfurizer is further used in the desulfurization reaction of Texaco simulated coal gas, and the desulfurization reaction conditions are the same as above. After the desulfurization reaction is completed, regeneration is performed again under the same regeneration conditions.
[0052] After ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer was detected to be 99.0% and the sulfur capacity was 28.2%.
[0053] Figure 1 This is a comparison of the sulfur vacancy concentration of the desulfurizer after absorption saturation in this embodiment before and after the heat treatment by passing hydrogen and argon. The sample before modification represents the sample after the desulfurization reaction to absorption saturation, and the sample after modification represents the sample after the absorption saturation desulfurizer is soaked in NaF solution and heat treated by passing hydrogen and argon. Figure 1 It can be seen that the sulfur vacancy concentration in the sample increases after being immersed in NaF solution and heat treated by passing hydrogen and argon.
[0054] Example 2
[0055] (1) Preparation of renewable aerogel desulfurizer, the steps are as follows:
[0056] 1) Preparation of desulfurizer precursor: 2.97 g zinc nitrate (specifically Zn(NO3)2·6H2O, 0.01 mol) and 8.73 g cobalt nitrate (specifically Co(NO3)2·6H2O, 0.03 mol), precursors of the active component ZnCo2O4, were dissolved in 100 mL of water to obtain a mixed solution of zinc nitrate and cobalt nitrate as a hydrothermal reaction solution; a silica nanofiber aerogel carrier was subjected to a hydrothermal reaction in the hydrothermal reaction solution (the amount ratio of silica nanofiber aerogel to hydrothermal reaction solution was 0.4 g:100 mL), the hydrothermal reaction temperature was 90°C, the time was 1 h, and the active component ZnCo2O4 was generated in the silica nanofiber aerogel carrier during the hydrothermal reaction. After the hydrothermal reaction, the carrier was dried to obtain a desulfurizer precursor;
[0057] 2) Preparation of desulfurizer: The desulfurizer precursor prepared in step 1) was oxidized under a 1000 W microwave field (a mixed gas with an oxygen concentration of 2 vol% was introduced, the balance gas was nitrogen, and it was calcined at 250°C for 1 h) to obtain a renewable aerogel desulfurizer (the ZnCo2O4 content in the desulfurizer was 57.3 wt%).
[0058] (2) Application of desulfurizer: The desulfurizer prepared in this example (0.1 g) was placed in a fixed bed reactor at a space velocity of 2000 h -1 Texaco simulated coal gas was introduced and desulfurization reaction was carried out at 500°C until absorption saturation.
[0059] After the desulfurization reaction was completed, the sulfur capacity of the desulfurizer was detected to reach 27.9%, and the utilization rate of active components was 99.6%.
[0060] (3) Regeneration of desulfurizer: After the desulfurization reaction is completed, the desulfurizer saturated with H2S is placed in a 2mmol / L NaF solution and immersed for 12h. After drying, a mixed gas with a hydrogen concentration of 4vol% (4vol% hydrogen + 96vol% nitrogen), argon, and a mixed gas with an oxygen concentration of 2vol% (2vol% oxygen + 98vol% nitrogen) are introduced in sequence under a 1000W microwave field for heat treatment (the heat treatment temperature when hydrogen is introduced for heat treatment is 500°C and the heat treatment time is 30min; the heat treatment temperature when argon is introduced for heat treatment is 500°C and the heat treatment time is 30min; the heat treatment temperature when oxygen is introduced for heat treatment is 400°C and the heat treatment time is 2h; the space velocity is 2000h / s. -1 ) to obtain a completely regenerated desulfurizer. The regenerated desulfurizer is further used in the desulfurization reaction of Texaco simulated coal gas, and the desulfurization reaction conditions are the same as above. After the desulfurization reaction is completed, regeneration is performed again under the same regeneration conditions.
[0061] After ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer was detected to be 96% and the sulfur capacity was 27.6%.
[0062] Example 3
[0063] (1) Preparation of renewable aerogel desulfurizer, the steps are as follows:
[0064] 1) Preparation of desulfurization agent precursor: 2.97 g zinc nitrate (specifically Zn(NO3)2·6H2O, 0.01 mol) and 5.82 g cobalt nitrate (specifically Co(NO3)2·6H2O, 0.02 mol), precursors of the active component ZnCo2O4, were dissolved in 100 mL of water to obtain a mixed solution of zinc nitrate and cobalt nitrate as a hydrothermal reaction solution; a silica nanofiber aerogel carrier was subjected to a hydrothermal reaction in the hydrothermal reaction solution (the amount ratio of silica nanofiber aerogel to hydrothermal reaction solution was 0.4 g:100 mL), the hydrothermal reaction temperature was 100°C, the time was 1 h, and the active component ZnCo2O4 was generated in the silica nanofiber aerogel carrier during the hydrothermal reaction. After the hydrothermal reaction, the carrier was dried to obtain a desulfurization agent precursor;
[0065] 2) Preparation of desulfurizer: The desulfurizer precursor prepared in step 1) was oxidized under a 1000 W microwave field (a mixed gas with an oxygen concentration of 3 vol%, the balance gas being nitrogen, and calcined at 300° C. for 1 h) to obtain a renewable aerogel desulfurizer (the ZnCo2O4 content in the desulfurizer was 57.0 wt%).
[0066] (2) Application of desulfurizer: The desulfurizer prepared in this example (0.1 g) was placed in a fixed bed reactor at a space velocity of 2000 h -1 Texaco simulated coal gas was introduced and desulfurization reaction was carried out at 500°C until absorption saturation.
[0067] After the desulfurization reaction was completed, the sulfur capacity of the desulfurizer was detected to reach 27.5%, and the utilization rate of active components was 98.6%.
[0068] (3) Regeneration of desulfurizer: After the desulfurization reaction is completed, the desulfurizer saturated with H2S is placed in a 3mmol / L NaF solution and immersed for 12h. After drying, a mixed gas with a hydrogen concentration of 6vol% (6vol% hydrogen + 94vol% nitrogen), argon, and a mixed gas with an oxygen concentration of 3vol% (3vol% oxygen + 97vol% nitrogen) are introduced in sequence under a 1000W microwave field for heat treatment (the heat treatment temperature when hydrogen is introduced for heat treatment is 500°C and the heat treatment time is 30min; the heat treatment temperature when argon is introduced for heat treatment is 500°C and the heat treatment time is 30min; the heat treatment temperature when oxygen is introduced for heat treatment is 400°C and the heat treatment time is 2h; the space velocity is 2000h / s. -1 ) to obtain a completely regenerated desulfurizer. The regenerated desulfurizer is further used in the desulfurization reaction of Texaco simulated coal gas, and the desulfurization reaction conditions are the same as above. After the desulfurization reaction is completed, regeneration is performed again under the same regeneration conditions.
[0069] After ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer was detected to be 92% and the sulfur capacity was 27.0%.
[0070] Example 4
[0071] (1) Preparation of renewable aerogel desulfurizer, the steps are as follows:
[0072] 1) Preparation of desulfurizer precursor: 2.97 g zinc nitrate (specifically Zn(NO3)2·6H2O, 0.01 mol) and 2.91 g cobalt nitrate (specifically Co(NO3)2·6H2O, 0.01 mol), precursors of the active component ZnCo2O4, were dissolved in 100 mL of water to obtain a mixed solution of zinc nitrate and cobalt nitrate as a hydrothermal reaction solution; a silica nanofiber aerogel carrier was subjected to a hydrothermal reaction in the hydrothermal reaction solution (the amount ratio of silica nanofiber aerogel to hydrothermal reaction solution was 0.4 g:100 mL), the hydrothermal reaction temperature was 110°C, the time was 1 h, and the active component ZnCo2O4 was generated in the silica nanofiber aerogel carrier during the hydrothermal reaction. After the hydrothermal reaction, the carrier was dried to obtain a desulfurizer precursor;
[0073] 2) Preparation of desulfurizer: The desulfurizer precursor prepared in step 1) was oxidized under a 1000 W microwave field (a mixed gas with an oxygen concentration of 4 vol% was introduced, the balance gas was nitrogen, and it was calcined at 350°C for 1 h) to obtain a renewable aerogel desulfurizer (the ZnCo2O4 content in the desulfurizer was 56.6 wt%).
[0074] (2) Application of desulfurizer: The desulfurizer prepared in this example (0.1 g) was placed in a fixed bed reactor at a space velocity of 2000 h -1Texaco simulated coal gas was introduced and desulfurization reaction was carried out at 500°C until absorption saturation.
[0075] After the desulfurization reaction was completed, the sulfur capacity of the desulfurizer was detected to reach 27.1%, and the utilization rate of active components was 97.9%.
[0076] (3) Regeneration of desulfurizer: After the desulfurization reaction is completed, the desulfurizer saturated with H2S is placed in a 4mmol / L NaF solution and immersed for 12h. After drying, a mixed gas with a hydrogen concentration of 8vol% (8vol% hydrogen + 92vol% nitrogen), argon, and a mixed gas with an oxygen concentration of 4vol% (4vol% oxygen + 96vol% nitrogen) are introduced in sequence under a 1000W microwave field for heat treatment (the heat treatment temperature when hydrogen is introduced for heat treatment is 500°C and the heat treatment time is 30min; the heat treatment temperature when argon is introduced for heat treatment is 500°C and the heat treatment time is 30min; the heat treatment temperature when oxygen is introduced for heat treatment is 400°C and the heat treatment time is 2h; the space velocity is 2000h / s. -1 ) to obtain a completely regenerated desulfurizer. The regenerated desulfurizer is further used in the desulfurization reaction of Texaco simulated coal gas, and the desulfurization reaction conditions are the same as above. After the desulfurization reaction is completed, regeneration is performed again under the same regeneration conditions.
[0077] After ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer was 89% and the sulfur capacity was 25.8%.
[0078] Comparative Example 1
[0079] The purchased commercial ZnCo2O4 was used as the active component, and the desulfurizer was prepared by mechanically mixing ZnCo2O4 and silica nanofiber aerogel in a certain mass ratio (57.9:42.1).
[0080] The specific operation of mechanical mixing is: disperse ZnCo2O4 in water to prepare a ZnCo2O4 dispersion with a concentration of 0.1 mol / L, add silica nanofiber aerogel, take out the silica nanofiber aerogel after mechanical stirring for 3 hours, dry it, and obtain a desulfurizer (the ZnCo2O4 content in the desulfurizer is 57.9wt%).
[0081] Under the same desulfurization reaction experimental conditions as in Example 1, the initial sulfur capacity of the mechanically mixed ZnCo2O4 / silicon dioxide nanofiber aerogel desulfurizer prepared in this comparative example was tested to be 12.3%, and the active component utilization rate was 47.6%.
[0082] After desulfurization, regeneration was carried out under the same conditions as in Example 1. After ten cycles of sulfurization / regeneration, the regeneration rate of the mechanically mixed ZnCo2O4 / silicon dioxide nanofiber aerogel desulfurizer was 60.1%, and the sulfur capacity decreased by 6.8%.
[0083] In addition, the desulfurizer after the first desulfurization was tested in a mixed gas with an oxygen concentration of 2 vol% (2 vol% + 98 vol% nitrogen) and a space velocity of 2000 h -1 Under the above conditions, the regeneration reaction temperature at which a regeneration rate of 99% can be achieved is 850°C.
[0084] Comparative Example 2
[0085] The same as Example 1, the only difference is that the use of microwave field is omitted in step 2) of preparing the renewable aerogel desulfurizer, and the oxidation treatment is carried out under non-microwave conditions.
[0086] Under the same desulfurization reaction experimental conditions as those in Example 1, the initial sulfur capacity of the desulfurizer prepared in this comparative example was tested to be 15.6%, and the utilization rate of the active component was 58.1%.
[0087] After desulfurization, regeneration was carried out under the same conditions as in Example 1. After ten cycles of sulfurization / regeneration, the regeneration rate of the desulfurizer was 98.0%, and the sulfur capacity decreased to 12.4%.
[0088] Comparative Example 3
[0089] The preparation steps of the regenerable aerogel desulfurizer are the same as those in Example 1, the conditions of the desulfurization reaction are the same as those in Example 1, and the regeneration steps of the desulfurizer are different from those in Example 1.
[0090] The regeneration step of this comparative example is as follows: after the desulfurization reaction is completed, the desulfurizer saturated with H2S is sequentially introduced into a mixed gas with a hydrogen concentration of 2 vol% (2 vol% hydrogen + 98 vol% nitrogen), argon, and a mixed gas with an oxygen concentration of 1 vol% (1 vol% oxygen + 99 vol% nitrogen) under a 1000 W microwave field for heat treatment (the heat treatment temperature when hydrogen is introduced for heat treatment is 500°C, and the heat treatment time is 30 min; the heat treatment temperature when argon is introduced for heat treatment is 500°C, and the heat treatment time is 30 min; the heat treatment temperature when oxygen is introduced for heat treatment is 400°C, and the heat treatment time is 2 h; the space velocity is 2000 h -1 ) to obtain a completely regenerated desulfurizer. The regenerated desulfurizer was further used in the desulfurization reaction of Texaco simulated coal gas, and the desulfurization reaction conditions were the same as above (space velocity 2000h -1 , temperature 500°C). After the desulfurization reaction is completed, regeneration is carried out again under the same regeneration conditions.
[0091] After ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer was detected to be 80.1% and the sulfur capacity was 20.8%.
[0092] Comparative Example 4
[0093] The preparation steps of the regenerable aerogel desulfurizer are the same as those in Example 1, the conditions of the desulfurization reaction are the same as those in Example 1, and the regeneration steps of the desulfurizer are different from those in Example 1.
[0094] The regeneration step of this comparative example is as follows: after the desulfurization reaction is completed, the desulfurizer saturated with H2S is placed in a 1mmol / L NaF solution and immersed for 12h, and then dried and heat-treated in a 1000W microwave field by sequentially introducing argon and a mixed gas with an oxygen concentration of 1vol% (1vol% oxygen + 99vol% nitrogen) (the heat treatment temperature when introducing argon for heat treatment is 500°C and the heat treatment time is 30min; the heat treatment temperature when introducing oxygen for heat treatment is 400°C and the heat treatment time is 2h; the space velocity is 2000h / s. -1 ) to obtain a completely regenerated desulfurizer. The regenerated desulfurizer was further used in the desulfurization reaction of Texaco simulated coal gas, and the desulfurization reaction conditions were the same as above (space velocity 2000h -1 , temperature 500°C). After the desulfurization reaction is completed, regeneration is carried out again under the same regeneration conditions.
[0095] After ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer was 85.7% and the sulfur capacity was 21.2%.
[0096] Comparative Example 5
[0097] The preparation steps of the regenerable aerogel desulfurizer are the same as those in Example 1, the conditions of the desulfurization reaction are the same as those in Example 1, and the regeneration steps of the desulfurizer are different from those in Example 1.
[0098] The regeneration step of this comparative example is as follows: after the desulfurization reaction is completed, the desulfurizer saturated with H2S is placed in a 1mmol / L NaF solution and soaked for 12h, and then dried and sequentially introduced into a mixed gas with a hydrogen concentration of 2vol% (2vol% hydrogen + 98vol% nitrogen), argon, and a mixed gas with an oxygen concentration of 1vol% (1vol% oxygen + 99vol% nitrogen) for heat treatment (the heat treatment temperature when hydrogen is introduced for heat treatment is 500°C, and the heat treatment time is 30min; the heat treatment temperature when argon is introduced for heat treatment is 500°C, and the heat treatment time is 30min; the heat treatment temperature when oxygen is introduced for heat treatment is 400°C, and the heat treatment time is 2h, which is carried out in a non-microwave field; the air velocity is 2000h / s. -1 ) to obtain a completely regenerated desulfurizer. The regenerated desulfurizer was further used in the desulfurization reaction of Texaco simulated coal gas, and the desulfurization reaction conditions were the same as above (space velocity 2000h-1 , temperature 500°C). After the desulfurization reaction is completed, regeneration is carried out again under the same regeneration conditions.
[0099] After ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer was detected to be 75.5% and the sulfur capacity was 20.8%.
[0100] Comparative Example 6
[0101] The preparation steps of the regenerable aerogel desulfurizer are the same as those in Example 1, the conditions of the desulfurization reaction are the same as those in Example 1, and the regeneration steps of the desulfurizer are different from those in Example 1.
[0102] The regeneration steps of this comparative example are: using a mixed gas with an oxygen volume concentration of 2 vol% (2 vol% oxygen + 98 vol% nitrogen), at a temperature of 650°C and a space velocity of 2000 h -1 The desulfurizer was regenerated for 2 hours after absorbing H2S to obtain a regenerated desulfurizer. The regenerated desulfurizer was used to desulfurize the simulated Texaco gas under the same conditions as above (space velocity 2000h -1 , temperature 500°C). After the desulfurization reaction is completed, regeneration is carried out again under the same regeneration conditions.
[0103] After ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer was 66.3% and the sulfur capacity was 17.6%.
[0104] Comparative Example 7
[0105] The same as comparative example 6, the only difference is that the regeneration temperature is 850°C. After ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer is detected to be 98% and the sulfur capacity is 27.1%.
[0106] Comparative Example 8
[0107] The same as comparative example 6, except that the regeneration temperature is 400° C., after ten times of sulfurization / regeneration cycles, the regeneration rate of the desulfurizer is detected to be 66.6% and the sulfur capacity is 18.0%.
[0108] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a renewable aerogel desulfurizer, It is characterized in that The following steps are involved: The silica nanofiber aerogel carrier is subjected to a hydrothermal reaction in a mixed solution of zinc nitrate and cobalt nitrate to generate an active component ZnCo in the silica nanofiber aerogel carrier. 2 O 4 , obtaining a desulfurizer precursor; and subjecting the desulfurizer precursor to oxidation treatment under a microwave field to obtain the renewable aerogel desulfurizer.
2. The preparation method according to claim 1, It is characterized in that The porosity of the silicon dioxide nanofiber aerogel carrier is 95-99.99%, and the diameter of the silicon dioxide nanofibers is 100-1000nm.
3. The preparation method according to claim 1, It is characterized in that The molar ratio of zinc nitrate to cobalt nitrate in the mixed solution of zinc nitrate and cobalt nitrate is 1:1-4, and the concentration of zinc nitrate is 0.1 mol / L.
4. The preparation method according to claim 1, It is characterized in that The temperature of the hydrothermal reaction is 80-110° C. and the time is 1-4 hours.
5. The preparation method according to claim 1, It is characterized in that The microwave condition of the microwave field is 1000W.
6. The preparation method according to claim 1, It is characterized in that The specific parameters of the oxidation treatment include: oxygen concentration of 1-4 vol%, calcination temperature of 200-350° C., and calcination time of 1 hour.
7. A renewable aerogel desulfurizer prepared by the preparation method according to any one of claims 1 to 6.
8. A method for regenerating the regenerable aerogel desulfurizer as claimed in claim 7, It is characterized in that The following steps are involved: The regenerated aerogel desulfurizer after the desulfurization reaction was immersed in a NaF solution for 12 hours, dried and placed under a microwave field, and hydrogen, argon and oxygen were introduced in sequence for heat treatment to obtain a regenerated desulfurizer.
9. The regeneration method according to claim 8, It is characterized in that The concentration of the NaF solution is 1-4 mmol / L.
10. The regeneration method according to claim 8, It is characterized in that The concentration of hydrogen is 2-8 vol%, the concentration of oxygen is 1-4 vol%, and the balance gas when hydrogen and oxygen are introduced is nitrogen.
Citation Information
Patent Citations
Method for preparing regenerable normal-temperature nano-desulfurizer
CN101716449A
Fine desulfurizer for zinc oxide at room temperature, preparation method and application
CN109432999A
Preparation method and desulfurization application of cobalt-doped carbon aerogel
CN113877529A
Preparation method of zinc cobaltate composite gas desulfurizer
CN114702989A
Preparation method of high-performance oxide / nanofiber composite gas desulfurizer
CN118185674A