PVDF (Polyvinylidene Fluoride) polymer composite membrane for total heat exchanger and preparation method of PVDF polymer composite membrane
By adding GO, LiCl and CNTs additives to PVDF films, PVDF polymer composite films were prepared, which solved the problem of hydrophobicity limitation of PVDF materials and improved the heat exchange efficiency of total heat exchangers and the energy efficiency of air conditioning systems.
Patent Information
- Application Number
- CN202411056818.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-08
AI Technical Summary
The hydrophobicity of existing PVDF materials limits their application in total heat exchangers, and the modification effect and stability need to be improved.
PVDF polymer composite membranes were prepared by combining GO, LiCl and CNTs with PVDF films. By adjusting the composition of the casting solution and the film-making process, the hydrophilicity and mechanical strength of the membrane were improved, and the water vapor permeability and adsorption-desorption performance were enhanced.
It improves the heat exchange efficiency of the total heat exchanger, reduces the energy consumption of the air conditioning system, enhances the water vapor permeability and adsorption-desorption performance of the membrane, and improves the mechanical strength.
Smart Images

Figure CN118904117A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a novel polymer material, in particular to a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger and a preparation method thereof. Background Art
[0002] Under the background of "dual carbon goals", reducing the energy consumption of buildings has become the main goal. A total heat exchanger is a device used to recover energy between fresh air and exhaust air, which can significantly reduce the energy consumption of air-conditioning systems. Membrane total heat exchangers are widely used due to their high efficiency and compactness. Their core components are total heat exchange membranes. Polyvinylidene fluoride (PVDF) has excellent chemical corrosion resistance, heat resistance and other advantages, and is an ideal membrane material. Since PVDF itself is not hydrophilic, but has a certain hydrophobicity, its hydrophobicity limits its application, so it needs to be modified. At present, commonly used modification methods include blending modification, grafting modification, etc., but the modification effect and stability need to be improved. Summary of the invention
[0003] The present invention discloses a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger and a preparation method thereof. Three additives, GO, LiCl and CNTs, are combined with a PVDF film to increase the heat exchange effect of the total heat exchanger and reduce the energy consumption of the air-conditioning system. The composite membrane has high water vapor permeability, good adsorption and desorption properties and excellent mechanical strength.
[0004] The present invention is achieved through the following technical solutions: A method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger comprises the following steps: (1) Soaking the support layer in anhydrous ethanol, taking it out and drying it in an air drying oven to obtain support layer A; (2) Then, the support layer A is fixed on a clean glass plate, and the membrane A is wetted with N-N-dimethylacetamide to obtain the support layer B; (3) Coat the surface of the support layer B with the casting liquid, and use an adjustable coater with different gaps to scrape the film to obtain a film A of different thicknesses; the scraping film requires the use of an adjustable coater with a width of 200-350 μm and a uniform scraping speed.
[0005] (4) placing membrane A in 90% deionized water and 10% anhydrous ethanol at 20°C for solidification, and obtaining membrane B after forming; (5) Soak membrane B in deionized water for 24 hours to obtain membrane C; (6) Finally, dry to form a film.
[0006] Preferably, the support layer is a nonwoven fabric.
[0007] Preferably, the casting solution in step (3) comprises 13% PVDF, 72% DMAc, 8% DMF and 7% PVP; the casting solution also comprises one or more of GO, carbon nanotubes and LiCl.
[0008] More preferably, the mass ratio of GO / carbon nanotubes to casting solution is 0.05-0.2:100.
[0009] More preferably, the mass ratio of LiCl to the casting solution is 1-3:100.
[0010] Preferably, in the polymer film preparation method described in step (1), the drying oven temperature is 65° C. and the drying time is 1 h.
[0011] Preferably, the reaction temperature of the casting solution in step (3) is 70-75°C.
[0012] Preferably, the reaction conditions in step (3) are 70-75°C oil bath and stirring time is 24h-36h; Preferably, the film scraping in step (3) requires the use of an adjustable applicator of 200-350 μm, with a uniform film scraping speed; Preferably, in the preparation method described in step (6), the drying environment is 26° C. and the drying time is 24 hours.
[0013] Beneficial Effects The water vapor permeability of all groups of non-woven fabric-polyvinylidene fluoride composite membranes is greater than that of commercial films, which shows the key role of polymer films in the field of total heat exchange; when modified alone, the addition of graphene oxide promotes the water vapor permeability of the composite membrane, and reaches a peak value when the addition content is 0.1%, with a maximum water vapor permeability of 3641.2998g / (m 2 ·24h); in the adsorption and desorption performance test, the adsorption and desorption amount of M3 is better than that of M0 under various working conditions, and the required humidity approaching the saturation limit is higher. The water vapor permeability of M16 after composite modification is higher. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The preparation process of the composite membrane; Figure 2 This is a comparison chart of water vapor permeability between composite film and commercial paper film; Figure 3 It is a comparison diagram of adsorption isotherms at 21°C; Figure 4 It is a comparison diagram of adsorption isotherms at 35°C; Figure 5 It is a comparison diagram of desorption isotherms at -3℃; Figure 6 It is a comparison diagram of desorption isotherms at 22°C; Figure 7 The surface structure of the composite membrane; Figure 8 This is a thickness comparison chart between composite film and commercial paper film. DETAILED DESCRIPTION
[0015] The following is a detailed description of an embodiment of the present invention. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.
[0016] Example 1 The raw materials and reagents used in the experiment are shown in Table 1: Table 1 Raw materials and reagents Preparation process The production process of polyvinylidene fluoride-non-woven composite membrane is as follows: (1) Soak the non-woven fabric in anhydrous ethanol for 4 hours, take it out and put it into a forced air drying oven at 65°C for 1 hour; (2) The composition of the casting solution was 13% PVDF, 72% DMAc, 8% DMF, and 7% PVP after weighing the weight of each additive. (3) Then the above solution was placed in a 75°C oil bath and mechanically stirred for 48 hours to obtain a homogeneous casting solution, which was then allowed to stand for 24 hours for complete degassing; (4) Fix the non-woven fabric on a clean glass plate, and then use N-N-dimethylacetamide to wet the non-woven fabric. The purpose of this step is to prevent bubbles from being retained between the non-woven fabric and the glass plate, which will affect the quality of the film. Then, pour the casting liquid on the non-woven fabric, use a scraper with a specification of 200 μm to scrape the film, and place the device in the air for 30 seconds; (5) Using 90% deionized water and 10% anhydrous ethanol at 20°C as a coagulation bath, soak the formed membrane in deionized water for 24 h, changing the water several times during the coagulation to remove the residual solvent; (6) Finally, dry at room temperature for 24 hours to obtain the final film.
[0017] The specific membrane production process is as follows: Figure 1 shown.
[0018] The information of the films prepared with different solvent contents is shown in Table 2. Among them, the four groups of experiments M1, M2, M3, and M4 formed a graphene oxide addition content control group; the three groups of experiments M5, M6, and M7 formed a lithium chloride addition content control group; the three groups of experiments M8, M9, and M10 formed a carbon nanotube addition content control group; the three groups of experiments M1, M11, and M12 formed a polyvinyl pyrrolidone addition content control group, and at the same time formed different porogen controls with M13, M14, and M15.
[0019] Table 2 Composite membrane component information Composite membrane characterization 1. Water vapor permeability test The prepared membrane was tested to measure the water vapor permeability per unit area within 24 hours to characterize the latent heat exchange performance of the membrane. The test was carried out under the dehumidification method experimental conditions specified in the GB / T 21087-2020 "Heat Recovery Fresh Air Unit" standard (temperature 38℃±0.5℃, relative humidity 90%±2%). The test results are as follows: Figure 2 and Table 3.
[0020] 2. Thin film adsorption and desorption test The test process is to fix the film sample in a constant temperature and humidity environment, maintain a certain wind speed on the sample, weigh it at a certain interval, and monitor the weight change curve of the sample over time until the weight of the sample no longer changes, which means that the sample has been adsorbed to saturation under the air parameters in this state. In this experiment, when the weight of the sample changes by no more than 1 mg within 10 minutes, it is considered that the weight of the sample has stopped changing.
[0021] Commercial film M0 and homemade film M3 with high water vapor permeability were selected as test objects, and two films of the same weight were cut out for testing. When testing the adsorption process, the film must first be placed in a blast drying oven for 4 hours, and the water content in the sample is considered to be zero after the treatment. Similarly, when testing the desorption process, the film must be placed in a constant temperature and humidity chamber to maintain a relative humidity environment of 100% for 4 hours, and the sample is considered to be saturated with adsorption after the treatment.
[0022] The test is divided into two working conditions, winter and summer, and representative air state parameters of the two are selected for testing. Under summer conditions, the adsorption test temperature is 35°C; under winter conditions, the adsorption temperature is 21°C. The relative humidity is selected as 30%, 40%, 50%, 60%, 70%, and 80%, respectively. Connect the points of the maximum equilibrium adsorption amount of each relative humidity to form a line, and the adsorption / desorption isotherm at the corresponding temperature can be obtained. Then, desorption tests are carried out from 80% to 30% under the temperature conditions of 22°C in summer and -3°C in winter, and the corresponding desorption isotherms can also be obtained, as shown below Figure 3-Figure 6 shown.
[0023] The modified composite membrane M16 has better adsorption performance than M3. The modification enhances the hydrophilicity of the membrane. This change strengthens the first stage of the dissolution-diffusion process of the composite membrane - the process of water molecules dissolving on the film, which enhances the water vapor permeability of the composite membrane itself, thereby strengthening the adsorption process. At the same time, it also increases the pore size of the composite membrane and the contact area between the composite membrane and the air on both sides, which has a positive effect on the adsorption and desorption of the composite membrane.
[0024] 3. Film microstructure characterization The surface structure of the film was observed using an optical microscope. Figure 7 The porous filamentous structure of the nonwoven fabric and the holes distributed on the polyvinylidene fluoride underneath the nonwoven fabric can be observed.
[0025] The filamentous structure of non-woven fabric is the basis for it to serve as a supporting material. This structure is conducive to the attachment of membrane materials and provides excellent mechanical strength for the composite membrane. The surface of polyvinylidene fluoride is full of pore structures. This is a structure formed by the diffusion of porogens from the casting solution during the membrane making process. This pore not only increases the contact area between the air and the composite membrane, but also provides a larger platform for the adsorption process of the composite membrane. However, polyvinylidene fluoride itself is hydrophobic and prone to wrinkles on the surface. Therefore, the surface porosity is not high and the pore distribution is uneven. Some additives (such as lithium chloride) will aggravate this phenomenon, causing the surface wrinkles of the film to seriously affect the heat and mass transfer process. Modification can speed up the precipitation rate of polyvinylidene fluoride, resulting in the characteristic of increased pore size, so the addition of modifiers can avoid this problem to a certain extent.
[0026] 4. Film thickness measurement The film thickness was measured using a digital micrometer with an accuracy of 0.001 mm. Five points were selected on each film for testing, one at the center of the film and the other four test points at four points on the edge of the film. The film thickness was determined by the average of the five times. The test results are as follows: Figure 8 shown.
[0027] The thickness of the composite membranes is basically the same, both between 270-310 μm, which indicates that during the membrane making process, the casting liquid is applied more evenly during the scraping process of the composite membrane, which is conducive to the comparison of water vapor permeation.
[0028] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger, characterized in that: The following steps are involved: (1) Soaking the support layer in anhydrous ethanol, taking it out and drying it in an air drying oven to obtain support layer A; (2) Then, the support layer A is fixed on a clean glass plate, and the membrane A is wetted with N-N-dimethylacetamide to obtain the support layer B; (3) coating the casting liquid on the surface of the support layer B, and using an adjustable applicator to scrape the film to obtain films A of different thicknesses; (4) placing membrane A in deionized water and anhydrous ethanol to solidify, and obtaining membrane B after forming; (5) Soak membrane B in deionized water to obtain membrane C; (6) Finally, dry to form a film.
2. The method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger according to claim 1, characterized in that: The supporting layer is non-woven fabric.
3. The method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger according to claim 1, characterized in that: The composition of the casting solution in step (3) is 13% PVDF, 72% DMAc, 8% DMF, and 7% PVP; the casting solution also includes one or more of GO, carbon nanotubes, and LiCl.
4. The method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger according to claim 2, characterized in that: The mass ratio of GO / carbon nanotubes to the casting solution is 0.05-0.2:
100.
5. The method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger according to claim 2, characterized in that: The mass ratio of LiCl to the casting solution is 1-3:
100.
6. The method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger according to claim 1, characterized in that: In the polymer film preparation method described in step (1), the drying oven temperature is 65° C. and the drying time is 1 hour.
7. The method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger according to claim 1, characterized in that: The reaction temperature of the casting solution in step (3) is 70-75°C.
8. The method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger according to claim 1, characterized in that: The reaction conditions of step (3) are 70-75° C. oil bath and stirring time is 24 h-36 h.
9. The method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger according to claim 1, characterized in that: The scraping of the film in step (3) requires the use of an adjustable coater of 200-350 μm.
10. The method for preparing a PVDF polymer composite membrane for improving the heat exchange efficiency of a total heat exchanger according to claim 1, characterized in that: The preparation method described in step (6) is characterized in that the drying environment is 26° C. and the drying time is 24 hours.