Catalyst and preparation method thereof, and methanol preparation method

By using ZnO-M oxide solid solution catalyst, the problem of poor stability of traditional catalysts under high temperature and low pressure conditions is solved, the carbon dioxide conversion rate and methanol yield are improved, and the efficient methanol preparation is achieved.

CN118904324APending Publication Date: 2024-11-08CHINA NAT OFFSHORE OIL CORP +3
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411018479.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When traditional Cu-ZnO/Al2O3 catalysts are used to hydrogenate carbon dioxide to produce methanol under high temperature and low pressure conditions, there is a problem of sintering of active components of water-induced catalysts in poor stability and active phase, resulting in low carbon dioxide conversion and methanol yield.

Method used

ZnO-M oxide solid solution catalyst is used, where M includes ZrO2, TiO2 and CeO2, with a low-dimensional structure. It is prepared by precipitation, crystallization, calcination and other steps to form a catalyst with high activation and stability, which is used for high temperature and low pressure. Carbon dioxide hydrogenation to methanol reaction.

Benefits of technology

It improves the activation and conversion of carbon dioxide, inhibits the change of counterhydraulic gas and methanol decomposition reaction, extends the service life of the catalyst, and is suitable for the hydrogenation of carbon dioxide under high temperature and low pressure conditions to produce methanol, and improves the time and space yield of methanol.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of catalysts, in particular to a catalyst and a preparation method thereof, and a preparation method of methanol. The catalyst provided by the invention comprises a ZnO-M oxide solid solution, and the M oxide comprises at least one of ZrO2, TiO2 and CeO2; the ZnO-M oxide solid solution has a low-dimensional structure. The ZnO-M oxide solid solution catalyst with the low-dimensional structure, provided by the invention, greatly enhances activation and conversion of CO2, inhibits decomposition reaction of RWGS and methanol, inhibits toxic action of water on active sites in a methanol synthesis process, and can be suitable for a reaction for preparing methanol by hydrogenation of carbon dioxide at high temperature and low pressure; the catalyst has the advantages of high carbon dioxide conversion rate, high methanol space-time yield, good stability and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a catalyst and a preparation method thereof, and a preparation method of methanol. Background Art

[0002] As one of the main greenhouse gases, excessive emissions of carbon dioxide exacerbate the greenhouse effect and cause great harm to the global natural ecological environment. At present, countries around the world are paying attention to the issue of global warming and have actively formulated various emission reduction agreements to alleviate carbon dioxide emissions. Carbon dioxide hydrogenation to methanol technology can not only realize the resource conversion of carbon dioxide, but also help solve the storage problem of renewable energy, and at the same time can achieve carbon dioxide emission reduction and slow down ecological deterioration.

[0003] As a basic raw material for platform chemicals, methanol can produce many hydrocarbon products, including olefins, aromatics and alcohol oxides. At the same time, methanol can also be used as a hydrogen source for fuel cells and other application scenarios. These subsequent reactions or application processes are often carried out at higher temperatures and lower pressures. In conventional industry, CO2 hydrogenation to methanol is usually carried out under high pressure of 50-100 bar and 230-260 ° C. The catalyst usually uses traditional Cu-ZnO / Al2O3 catalyst. Therefore, it is necessary to study the catalyst for synthesizing methanol under high temperature and low pressure conditions. However, CO2 synthesis of methanol is limited by high temperature equilibrium. The higher the temperature, the less conducive it is to the formation of methanol. Traditional copper-based catalysts have been widely studied in CO2 hydrogenation reactions. However, due to their high activity in reverse water gas change (RWGS), the water-induced catalyst active components of the active phase sintering causes poor stability.

[0004] In view of this, this invention is proposed. Summary of the invention

[0005] The first purpose of the present invention is to provide a catalyst with good catalytic stability and long service life, which is suitable for the reaction of carbon dioxide hydrogenation to methanol under high temperature and low pressure, and improves the carbon dioxide conversion rate and methanol yield.

[0006] The second object of the present invention is to provide a method for preparing the above catalyst.

[0007] The third object of the present invention is to provide a method for preparing methanol.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] The present invention provides a catalyst, comprising a ZnO-M oxide solid solution, wherein the M oxide comprises at least one of ZrO2, TiO2 and CeO2; and the ZnO-M oxide solid solution has a low-dimensional structure.

[0010] Furthermore, in the ZnO-M oxide solid solution, the mass percentage of ZnO is 5% to 50%, and the mass percentage of M oxide is 50% to 95%.

[0011] Furthermore, the particle size of the catalyst is 40 to 60 meshes.

[0012] The present invention also provides a method for preparing the catalyst as described above, comprising the following steps:

[0013] S1, subjecting an M salt solution to a first precipitation reaction with an alkaline solution and aging the solution to obtain a first precipitate; the M salt solution comprises at least one of a Zr salt, a Ti salt and a Ce salt;

[0014] S2, subjecting a mixed solution containing zinc salt and urea, an alkaline solution and the solution A to a first precipitation reaction to obtain a reaction solution;

[0015] S3, the reaction solution is crystallized to obtain a crystallized solid;

[0016] S4. The crystallized solid is washed, dried, calcined and crushed in sequence to obtain the catalyst.

[0017] Further, in step S1 and step S2, the alkaline solution includes at least one of sodium carbonate, sodium hydroxide and ammonia water;

[0018] And / or, the concentration of the alkaline solution is 0.3-2.0 mol / L.

[0019] Further, step S1 includes at least one of the following features (1) to (4);

[0020] (1) The total metal ion concentration of the M salt solution is 0.3 to 2.0 mol / L;

[0021] (2) the first precipitation reaction comprises using a parallel flow co-precipitation method;

[0022] (3) The temperature of the precipitation reaction in the first question is 40-80°C, and the pH of the system is 8.0-12.0;

[0023] (4) The aging time is 2 to 8 hours.

[0024] Further, step S2 includes at least one of the following features (1) to (3);

[0025] (1) The mass ratio of the zinc salt to the urea is 1:(0.3-0.8);

[0026] (2) the second precipitation reaction comprises using a parallel flow co-precipitation method;

[0027] (3) The temperature of the second precipitation reaction is 40-80° C., and the pH of the system is 8.0-12.0.

[0028] Further, in step S3, the crystallization temperature is 150-200°C and the pressure is 0.5-4.0Mpa;

[0029] And / or, in step S4, the calcination includes: calcination at 300-600° C. for 10-24 hours.

[0030] The present invention also provides a method for preparing methanol, comprising the following steps:

[0031] The methanol is obtained by reacting H2, CO2 and the catalyst as described above.

[0032] Furthermore, the reaction temperature is 300-400° C., and the reaction pressure is 2.0-5.0 MPa.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The ZnO-M oxide solid solution catalyst with a low-dimensional structure provided by the present invention greatly enhances the activation and conversion of CO2, inhibits the RWGS and methanol decomposition reactions, and inhibits the poisoning effect of water on the active sites during the methanol synthesis process. It can be applied to the reaction of carbon dioxide hydrogenation to methanol under high temperature and low pressure, and has a high carbon dioxide conversion rate and methanol space-time yield. At the same time, the catalyst has good stability and a long service life.

[0035] 2. The catalyst of the present invention can be coupled with methanol downstream process products such as olefins, aromatics and alcohol oxides, or fuel cells and other application scenarios, and can connect the high temperature and low pressure conditions of the downstream product process, breaking the coupling limitations of traditional industrial methanol catalysts and downstream processes. DETAILED DESCRIPTION

[0036] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0037] In some embodiments of the present invention, a catalyst is provided, comprising a ZnO-M oxide solid solution, wherein the M oxide comprises at least one of ZrO2, TiO2 and CeO2; and the ZnO-M oxide solid solution has a low-dimensional structure.

[0038] The present invention takes the system of hydrogenating carbon dioxide to produce methanol under high temperature and low pressure as the research target and develops an efficient and stable catalyst. The ZnO-M oxide solid solution catalyst of the present invention has a low-dimensional structure, which can expose more ZnO-M oxide interfaces. On the one hand, the interface promotes the hydrogenation of carbonate intermediates into species with higher reactivity (such as formate and methoxyl groups) and greatly enhances the activation and conversion of CO2; on the other hand, there are a large number of active oxygen vacancies generated by Zn migration on the surface of the catalyst, forming oxygen-deficient ZnO x The active phase inhibits RWGS and methanol decomposition reactions; in addition, the hydrophobic ZrO2 crystals in the M oxide have the effect of inhibiting the poisoning effect of water on the active sites during the methanol synthesis process, and at the same time, the oxygen vacancies after the TiO2 or CeO2 in the M oxide can adsorb and activate CO2, thereby improving the CO2 conversion rate; the catalyst of the present invention is suitable for the reaction of hydrogenating carbon dioxide to produce methanol under high temperature and low pressure, and has a high carbon dioxide conversion rate and methanol space-time yield.

[0039] In the catalyst, the hydrophobic crystals in the M oxide have the ability to inhibit the poisoning effect of water on the active sites during the methanol synthesis process, thereby making the catalyst performance stable and having a long service life.

[0040] The catalyst can be coupled with methanol downstream process products such as olefins, aromatics and alcohol oxides, or fuel cells and other application scenarios. It can connect the high temperature and low pressure conditions of the downstream product process, breaking the coupling limitations of traditional industrial methanol catalysts and downstream processes. The application of CO2 hydrogenation to methanol under high temperature and low pressure conditions provides broad application prospects for coupling methanol's subsequent conversion process.

[0041] In some embodiments of the present invention, the ZnO-M oxide solid solution includes a ZnO-M oxide solid solution having a two-dimensional structure.

[0042] ZnO-M oxide is a low-dimensional material, mainly a two-dimensional structural material. The unique electronic properties at the edge of the low-dimensional material enhance the ability to activate hydrogen; at the same time, more active sites are exposed, which is more conducive to the diffusion of reactants and obtaining a larger specific surface area.

[0043] In some embodiments of the present invention, in the ZnO-M oxide solid solution, the mass percentage of ZnO is 5% to 50%, and the mass percentage of M oxide is 50% to 95%; typically but not limitatively, for example, in the ZnO-M oxide solid solution, the mass percentage of ZnO can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 45%, 50% or a range consisting of any two of them; the mass percentage of M oxide can be 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100% or a range consisting of any two of them.

[0044] In some embodiments of the present invention, the particle size of the catalyst is 40-60 mesh.

[0045] In some embodiments of the present invention, a method for preparing a catalyst is also provided, comprising the following steps:

[0046] S1, subjecting an M salt solution to a first precipitation reaction with an alkaline solution and aging the solution to obtain a first precipitate; the M salt solution includes at least one of a Zr salt, a Ti salt and a Ce salt;

[0047] S2, subjecting the mixed solution containing zinc salt and urea, the alkaline solution and the first precipitate to a second precipitation reaction to obtain a reaction solution;

[0048] S3, the reaction liquid is crystallized to obtain a crystallized solid;

[0049] S4. The crystallized solid is washed, dried, calcined and crushed in sequence to obtain a catalyst.

[0050] The invention adopts a high-pressure hydrothermal crystallization method to prepare a ZnO-M oxide solid solution with a low-dimensional structure; an M salt solution is subjected to a precipitation reaction with an alkali solution to generate a basic carbonate, which is then further subjected to a precipitation reaction with a zinc salt to form a crystallized solid after crystallization; the crystallized solid is calcined to form a ZnO-M oxide solid solution, which can be used as an efficient and stable catalyst for preparing methanol by hydrogenating carbon dioxide at high temperature and low pressure.

[0051] In some embodiments of the present invention, in step S1, the M salt solution is an aqueous solution of M salt; and the M salt is a soluble salt.

[0052] In some embodiments of the present invention, in step S1, Zr salts include but are not limited to nitrates; Ti salts include but are not limited to titanium chloride and / or potassium titanium oxalate; Ce salts include but are not limited to nitrates.

[0053] In some embodiments of the present invention, in step S1, the total metal ion concentration of the M salt solution is 0.3 to 2.0 mol / L; typically but not limiting, for example, the total metal ion concentration of the M salt solution can be 0.3 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L or a range consisting of any two of them; preferably, the total metal ion concentration of the M salt solution is 0.3 to 1 mol / L.

[0054] In some embodiments of the present invention, in step S1, the alkaline solution includes at least one of sodium carbonate, sodium hydroxide and ammonia water.

[0055] In some embodiments of the present invention, in step S1, the concentration of the alkaline solution is 0.3-2 mol / L; preferably, the concentration of the alkaline solution is 0.5-1 mol / L.

[0056] In some embodiments of the present invention, in step S1, the first precipitation reaction comprises adopting a parallel flow co-precipitation method.

[0057] In some embodiments of the present invention, in step S1, the temperature of the first precipitation reaction is 40-80°C, and the system pH is 8.0-12.0; typically but not limitatively, for example, the temperature of the first precipitation reaction can be 40°C, 50°C, 60°C, 70°C, 80°C or a range consisting of any two thereof; the system pH can be 8.0, 9.0, 10.0, 11.0, 12.0 or a range consisting of any two thereof; preferably 9.0-10.0.

[0058] The present invention does not impose a strict limitation on the reaction time of the first precipitation reaction in step S1. For example, in step S1, the reaction time of the first precipitation reaction is 2 to 3 hours.

[0059] In some embodiments of the present invention, in step S1, the aging time is 2 to 8 hours; typically but not limitatively, for example, the aging time can be 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours or a range of any two thereof.

[0060] In some embodiments of the present invention, in step S2, in the mixed solution containing zinc salt and urea, the mass ratio of zinc salt to urea is 1:(0.3-0.8); typically but not limitatively, for example, the mass ratio of zinc salt to urea can be 1:0.3, 1:0.5, 1:0.8 or a range of any two thereof.

[0061] In some embodiments of the present invention, in step S2, the alkaline solution includes at least one of sodium carbonate, sodium hydroxide and ammonia water.

[0062] In some embodiments of the present invention, in step S2, the concentration of the alkaline solution is 0.3-2 mol / L; preferably, the concentration of the alkaline solution is 0.5-1 mol / L.

[0063] In some embodiments of the present invention, in step S2, the second precipitation reaction comprises using a parallel flow co-precipitation method.

[0064] In some embodiments of the present invention, in step S2, the temperature of the second precipitation reaction is 40-80°C, and the system pH is 8.0-12.0; typically but not limiting, for example, the temperature of the second precipitation reaction can be 40°C, 50°C, 60°C, 70°C, 80°C or a range consisting of any two thereof; the system pH can be 8.0, 9.0, 10.0, 11.0, 12.0 or a range consisting of any two thereof; preferably 11.0-12.0.

[0065] The present invention does not impose a strict limitation on the reaction time of the second precipitation reaction in step S2. For example, in step S2, the reaction time of the second precipitation reaction is 2 to 3 hours.

[0066] In some embodiments of the present invention, in step S3, the crystallization temperature is 150-200°C, and the pressure is 0.5-4.0 MPa; typically but not limitatively, for example, the crystallization temperature can be 150°C, 160°C, 170°C, 180°C, 190°C, 200°C or a range consisting of any two thereof; the crystallization pressure can be 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, 3.5 MPa, 4 MPa or a range consisting of any two thereof.

[0067] In some embodiments of the present invention, in step S3, the crystallization time is 8 to 36 hours; typically but not limitatively, for example, the crystallization time can be 8 hours, 15 hours, 20 hours, 25 hours, 30 hours, 36 hours or a range of any two thereof.

[0068] In some embodiments of the present invention, in step S3, crystallization includes: placing the reaction solution in a high-pressure hydrothermal autoclave, injecting N2 into the high-pressure hydrothermal autoclave until the pressure is 0.5 to 4.0 MPa, and crystallizing at 150 to 200° C. for 8 to 36 hours.

[0069] In some embodiments of the present invention, in step S4, washing includes washing the crystallized solid with deionized water until the washing liquid is neutral; preferably, the liquid-to-solid ratio of the washing is 50% to 80%, and the number of washing times is 3 to 5 times.

[0070] In some embodiments of the present invention, in step S4, the drying temperature is 60-120°C.

[0071] In some embodiments of the present invention, in step S4, roasting includes: roasting at 300-600°C for 10-24h; typically but not limitatively, for example, the roasting temperature can be 300°C, 400°C, 500°C, 600°C or a range of any two thereof; the roasting time can be 10h, 15h, 20h, 24h or a range of any two thereof; preferably, the roasting temperature is 400-500°C, and the roasting time is 15-18h.

[0072] In some embodiments of the present invention, in step S4, calcination is performed in an air atmosphere.

[0073] In some embodiments of the present invention, in step S4, the pulverizing includes pulverizing to a particle size of 40 to 60 meshes.

[0074] In some embodiments of the present invention, a method for preparing methanol is also provided, comprising the following steps:

[0075] H2, CO2 and the above catalyst are reacted to obtain methanol.

[0076] The catalyst of the present invention is used in the reaction of hydrogenating carbon dioxide to produce methanol under high temperature and low pressure, which improves the carbon dioxide conversion rate and the space-time yield of methanol; at the same time, the application of hydrogenating CO2 to produce methanol under high temperature and low pressure conditions provides broad application prospects for coupling the subsequent conversion process of methanol.

[0077] In some embodiments of the present invention, the method for preparing methanol comprises the following steps:

[0078] activating the catalyst to obtain an activated catalyst;

[0079] H2, CO2 and the activated catalyst are reacted to obtain methanol.

[0080] In some embodiments of the present invention, the method for preparing methanol comprises using a fixed bed reactor.

[0081] In some embodiments of the present invention, the method for preparing methanol specifically comprises the following steps:

[0082] The catalyst is loaded on a fixed bed reactor, and a reducing gas is introduced for reduction; after the reduction is completed, H2 and CO2 are introduced for reaction to obtain methanol.

[0083] In some embodiments of the present invention, the reducing gas includes hydrogen, and at least one of argon, nitrogen, and helium.

[0084] In some embodiments of the present invention, the reduction temperature is 200-600° C., and the reduction time is 0.5-24 h; preferably, the reduction temperature is 300-500° C., and the reduction time is 12-18 h.

[0085] In some embodiments of the present invention, the reaction temperature is 300-400°C; typically but not limiting, for example, the reaction temperature can be 300°C, 350°C, 400°C or a range of any two thereof.

[0086] In some embodiments of the present invention, the reaction pressure is 2.0-5.0 MPa; typically but not limiting, for example, the reaction pressure can be 2.0 MPa, 3.0 MPa, 4.0 MPa, 5.0 MPa or a range of any two thereof.

[0087] In some embodiments of the present invention, the volume ratio of H2 and CO2 is (2.5-5.0):1; typically but not limitatively, for example, the volume ratio of H2 and CO2 can be 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1 or a range of any two thereof.

[0088] Example 1

[0089] The preparation method of the catalyst Cat-1 provided in this embodiment comprises the following steps:

[0090] Weigh 42.5 g of potassium titanium oxalate and dissolve it in 240 mL of deionized water to prepare a Ti salt solution; weigh 44.6 g of sodium carbonate and 40.0 g of sodium hydroxide and dissolve them in 1 L of deionized water to prepare an alkaline solution; weigh 2.1 g of zinc nitrate and 1.5 g of urea and dissolve them in 20 mL of deionized water to prepare a mixed solution containing zinc salt and urea;

[0091] S1. Under mechanical stirring, the Ti salt solution and the alkaline solution were added dropwise to a beaker containing 50 mL of deionized water by a co-current co-precipitation method for a first precipitation reaction of 2 to 3 hours. The reaction temperature was controlled to be 60°C and the system pH was 11.5. After aging for 2 hours, a first precipitate was obtained.

[0092] S2, using a parallel flow co-precipitation method, adding a mixed solution containing zinc salt and urea and an alkaline solution dropwise to the first precipitate to continue a second precipitation reaction for 2 to 3 hours, controlling the reaction temperature to 60° C. and the system pH to 11.5, stirring evenly after the dropwise addition to obtain a reaction solution;

[0093] S3, the reaction solution was transferred to an autoclave, pressurized with N2 to 2MPa, placed in an oven at 165°C for crystallization for 15h, cooled, emptied and centrifuged to obtain a crystallized solid;

[0094] S4. Add deionized water to the crystallized solid at a liquid-to-solid ratio of 80%, wash 5 times, and then place it in an oven to dry at 60-100°C, and then roast it at 400°C for 18 hours in an air atmosphere, and crush it to a particle size of 40-60 mesh to obtain a ZnO-TiO2 solid solution catalyst, wherein the mass ratio of ZnO to TiO2 is 5:95.

[0095] Example 2

[0096] The preparation method of the catalyst Cat-2 provided in this embodiment comprises the following steps:

[0097] Weigh 42.4 g of potassium titanium oxalate and dissolve it in 240 mL of deionized water to prepare a Ti salt solution; weigh 44.6 g of sodium carbonate and 40.0 g of sodium hydroxide and dissolve them in 1 L of deionized water to prepare an alkaline solution; weigh 4.5 g of zinc nitrate and 3.2 g of urea and dissolve them in 30 mL of deionized water to prepare a mixed solution containing zinc salt and urea;

[0098] S1. Under mechanical stirring, the Ti salt solution and the alkaline solution are added dropwise to a beaker containing 50 mL of deionized water by a co-current co-precipitation method for a first precipitation reaction of 2 to 3 hours. The reaction temperature is controlled to be 80°C and the system pH is 9.5. After aging for 2 hours, a first precipitate is obtained;

[0099] S2, using a parallel flow co-precipitation method, adding a mixed solution containing zinc salt and urea and an alkaline solution dropwise to the first precipitate to continue a second precipitation reaction for 2 to 3 hours, controlling the reaction temperature to 80° C. and the system pH to 11.5, stirring evenly after the dropwise addition to obtain a reaction solution;

[0100] S3, the reaction solution was transferred to an autoclave, pressurized with N2 to 0.5MPa, placed in an oven at 200°C for crystallization for 36h, cooled, emptied and centrifuged to obtain a crystallized solid;

[0101] S4. Add deionized water to the crystallized solid at a liquid-to-solid ratio of 50%, wash 5 times, and then place it in an oven to dry at 60-100°C, and then roast it at 400°C for 15 hours in an air atmosphere, and crush it to a particle size of 40-60 mesh to obtain a ZnO-TiO2 solid solution catalyst, wherein the mass ratio of ZnO to TiO2 is 10:90.

[0102] Example 3

[0103] The preparation method of the catalyst Cat-3 provided in this embodiment comprises the following steps:

[0104] Weigh 42.2 g of potassium titanium oxalate and dissolve it in 240 mL of deionized water to prepare a Ti salt solution; weigh 115.0 g of sodium hydroxide and dissolve it in 1 L of deionized water to prepare an alkaline solution; weigh 8.9 g of zinc nitrate and 6.2 g of urea and dissolve them in 60 mL of deionized water to prepare a mixed solution containing zinc salt and urea;

[0105] S1. Under mechanical stirring, the Ti salt solution and the alkaline solution were added dropwise to a beaker containing 50 mL of deionized water by a co-current co-precipitation method for a first precipitation reaction of 2 to 3 hours. The reaction temperature was controlled to be 40°C and the system pH was 9.5. After aging for 8 hours, a first precipitate was obtained.

[0106] S2, using a parallel flow co-precipitation method, adding a mixed solution containing zinc salt and urea and an alkaline solution dropwise to the first precipitate to continue a second precipitation reaction for 2 to 3 hours, controlling the reaction temperature to 40° C. and the system pH to 11.5, stirring evenly after the dropwise addition to obtain a reaction solution;

[0107] S3, the reaction solution was transferred to an autoclave, pressurized with N2 to 2MPa, placed in an oven at 165°C for crystallization for 15h, cooled, emptied and centrifuged to obtain a crystallized solid;

[0108] S4. Add deionized water to the crystallized solid at a liquid-to-solid ratio of 80%, wash 5 times, and then place it in an oven to dry at 60-100°C, and then roast it at 400°C for 18 hours in an air atmosphere, and crush it to a particle size of 40-60 mesh to obtain a ZnO-TiO2 solid solution catalyst, wherein the mass ratio of ZnO to TiO2 is 20:80.

[0109] Example 4

[0110] The preparation method of the catalyst Cat-4 provided in this embodiment comprises the following steps:

[0111] Weigh 16.1g zirconium oxynitrate and dissolve it in 120mL deionized water to prepare a Zr salt solution; use 25% concentrated ammonia water to prepare a 2% ammonia solution, i.e., an alkaline solution; weigh 3.6g zinc nitrate and 1.4g urea and dissolve them in 25mL deionized water to prepare a mixed solution containing zinc salt and urea;

[0112] S1. Under mechanical stirring, the Zr salt solution and the alkali solution were added dropwise to a beaker containing 50 mL of deionized water by a co-current co-precipitation method for a first precipitation reaction of 2 to 3 hours. The reaction temperature was controlled to be 50°C and the system pH was 9.5. After aging for 6 hours, a first precipitate was obtained.

[0113] S2, using a parallel flow co-precipitation method, adding a mixed solution containing zinc salt and urea and an alkaline solution to the first precipitate to continue the second precipitation reaction for 2 to 3 hours, controlling the reaction temperature to 50° C. and the system pH to 11.5, stirring evenly after the dropwise addition to obtain a reaction solution;

[0114] S3, the reaction solution was transferred to an autoclave, pressurized with N2 to 3MPa, placed in an oven at 150°C for crystallization for 12h, cooled, emptied and centrifuged to obtain a crystallized solid;

[0115] S4. Add deionized water to the crystallized solid at a liquid-to-solid ratio of 80%, wash 5 times, and then place it in an oven to dry at 60-100°C, and then roast it at 500°C for 15 hours in an air atmosphere, and crush it to a particle size of 40-60 mesh to obtain a ZnO-ZrO2 solid solution catalyst, wherein the mass ratio of ZnO to ZrO2 is 10:90.

[0116] Example 5

[0117] The preparation method of the catalyst Cat-5 provided in this embodiment comprises the following steps:

[0118] Weigh 16.0g of zirconium oxynitrate and dissolve it in 120mL of deionized water to prepare a Zr salt solution; use 25% concentrated ammonia water to prepare a 2% ammonia solution, that is, an alkaline solution; weigh 7.1g of zinc nitrate and 2.1g of urea and dissolve them in 50mL of deionized water to prepare a mixed solution containing zinc salt and urea;

[0119] S1. Under mechanical stirring, the Zr salt solution and the alkaline solution were added dropwise to a beaker containing 50 mL of deionized water by a co-current co-precipitation method for a first precipitation reaction of 2 to 3 hours. The reaction temperature was controlled to be 40°C and the system pH was 11.5. After aging for 2 hours, a first precipitate was obtained.

[0120] S2, using a parallel flow co-precipitation method, adding a mixed solution containing zinc salt and urea and an alkaline solution dropwise to the first precipitate to continue a second precipitation reaction for 2 to 3 hours, controlling the reaction temperature to 40° C. and the system pH to 11.5, stirring evenly after the dropwise addition to obtain a reaction solution;

[0121] S3, the reaction solution was transferred to an autoclave, pressurized with N2 to 4 MPa, placed in an oven at 150°C for crystallization for 8 h, cooled, emptied, and centrifuged to obtain a crystallized solid;

[0122] S4. Add deionized water to the crystallized solid at a liquid-to-solid ratio of 60%, wash 5 times, and then place it in an oven to dry at 60-100°C, and then calcine it at 500°C for 15 hours in an air atmosphere, and crush it to a particle size of 40-60 mesh to obtain a ZnO-ZrO2 solid solution catalyst, wherein the mass ratio of ZnO to ZrO2 is 20:80.

[0123] Example 6

[0124] The preparation method of the catalyst Cat-6 provided in this embodiment comprises the following steps:

[0125] Weigh 16.0g of zirconium oxynitrate and dissolve it in 120mL of deionized water to prepare a Zr salt solution; use 25% concentrated ammonia water to prepare a 2% ammonia solution, that is, an alkaline solution; weigh 11.9g of zinc nitrate and 4.8g of urea and dissolve them in 80mL of deionized water to prepare a mixed solution containing zinc salt and urea;

[0126] S1. Under mechanical stirring, the Zr salt solution and the alkali solution were added dropwise to a beaker containing 50 mL of deionized water by a co-current co-precipitation method for a first precipitation reaction of 2 to 3 hours. The reaction temperature was controlled to be 40°C and the system pH was 9.5. After aging for 2 hours, a first precipitate was obtained.

[0127] S2, using a parallel flow co-precipitation method, adding a mixed solution containing zinc salt and urea and an alkaline solution dropwise to the first precipitate to continue a second precipitation reaction for 2 to 3 hours, controlling the reaction temperature to 40° C. and the system pH to 11.5, stirring evenly after the dropwise addition to obtain a reaction solution;

[0128] S3, the reaction solution was transferred to an autoclave, pressurized with N2 to 3MPa, placed in an oven at 165°C for crystallization for 15h, cooled, emptied and centrifuged to obtain a crystallized solid;

[0129] S4. Add deionized water to the crystallized solid at a liquid-to-solid ratio of 60%, wash 5 times, and then place it in an oven to dry at 60-100°C, and then calcine it at 500°C for 15 hours in an air atmosphere, and crush it to a particle size of 40-60 mesh to obtain a ZnO-ZrO2 solid solution catalyst, wherein the mass ratio of ZnO to ZrO2 is 30:70.

[0130] Example 7

[0131] The preparation method of the catalyst Cat-7 provided in this embodiment comprises the following steps:

[0132] Weigh 26.1 g of cerium nitrate and dissolve it in 120 mL of deionized water to prepare a Ce salt solution; weigh 44.6 g of sodium carbonate and 40.0 g of sodium hydroxide and dissolve them in 1 L of deionized water to obtain an alkaline solution; weigh 17.8 g of zinc nitrate and 14.2 g of urea and dissolve them in 70 mL of deionized water to prepare a mixed solution containing zinc salt and urea;

[0133] S1. Under mechanical stirring, the Ce salt solution and the alkaline solution are added dropwise to a beaker containing 50 mL of deionized water by a co-current co-precipitation method for a first precipitation reaction for 2 to 3 hours. The reaction temperature is controlled to be 80°C and the system pH is 9.5. After aging for 4 hours, a first precipitate is obtained.

[0134] S2, using a parallel flow co-precipitation method, adding a mixed solution containing zinc salt and urea and an alkaline solution dropwise to the first precipitate to continue a second precipitation reaction for 2 to 3 hours, controlling the reaction temperature to 40° C. and the system pH to 11.5, stirring evenly after the dropwise addition to obtain a reaction solution;

[0135] S3, the reaction solution was transferred to an autoclave, pressurized with N2 to 4 MPa, placed in an oven at 150°C for crystallization for 15 h, cooled, emptied, and centrifuged to obtain a crystallized solid;

[0136] S4. Add deionized water to the crystallized solid at a liquid-to-solid ratio of 60%, wash 5 times, and then place it in an oven to dry at 60-100°C, and then calcine it at 500°C for 15 hours in an air atmosphere, and crush it to a particle size of 40-60 mesh to obtain a ZnO-CeO2 solid solution catalyst, wherein the mass ratio of ZnO to CeO2 is 20:80.

[0137] Example 8

[0138] The preparation method of the catalyst Cat-8 provided in this embodiment comprises the following steps:

[0139] Weigh 42.5 g of potassium titanium oxalate and dissolve it in 240 mL of deionized water to prepare a Ti salt solution; weigh 44.6 g of sodium carbonate and 40.0 g of sodium hydroxide and dissolve them in 1 L of deionized water to prepare an alkaline solution; weigh 35.7 g of zinc nitrate and 28.6 g of urea and dissolve them in 70 mL of deionized water to prepare a mixed solution containing zinc salt and urea;

[0140] S1. Under mechanical stirring, the Ti salt solution and the alkaline solution are added dropwise to a beaker containing 50 mL of deionized water by a co-current co-precipitation method for a first precipitation reaction of 2 to 3 hours. The reaction temperature is controlled to be 80°C and the system pH is 9.5. After aging for 4 hours, a first precipitate is obtained.

[0141] S2, using a parallel flow co-precipitation method, adding a mixed solution containing zinc salt and urea and an alkaline solution dropwise to the first precipitate to continue a second precipitation reaction for 2 to 3 hours, controlling the reaction temperature to 40° C. and the system pH to 11.5, stirring evenly after the dropwise addition to obtain a reaction solution;

[0142] S3, the reaction solution was transferred to an autoclave, pressurized with N2 to 3MPa, placed in an oven at 150°C for crystallization for 15h, cooled, emptied and centrifuged to obtain a crystallized solid;

[0143] S4. Add deionized water to the crystallized solid at a liquid-to-solid ratio of 60%, wash 5 times, and then place it in an oven to dry at 60-100°C, and then calcine it at 500°C for 15 hours in an air atmosphere, and crush it to a particle size of 40-60 mesh to obtain a ZnO-TiO2 solid solution catalyst, wherein the mass ratio of ZnO and TiO2 is 50:50.

[0144] Example 9

[0145] The preparation method of the catalyst Cat-9 provided in this embodiment comprises the following steps:

[0146] Weigh 21.2 g of potassium titanium oxalate and 160.3 g of zirconium oxynitrate and dissolve them in 240 mL of deionized water to prepare a solution containing Ti salt and Zr salt; weigh 44.6 g of sodium carbonate and 40.0 g of sodium hydroxide and dissolve them in 1 L of deionized water to prepare an alkaline solution; weigh 11.3 g of zinc nitrate and 7.9 g of urea and dissolve them in 80 mL of deionized water to prepare a mixed solution containing zinc salt and urea;

[0147] S1. Under mechanical stirring, a solution containing Ti salt and Zr salt and an alkaline solution are added dropwise to a beaker containing 50 mL of deionized water by a co-current co-precipitation method for a first precipitation reaction for 2 to 3 hours. The reaction temperature is controlled to be 80°C and the system pH is 9.5. After aging for 4 hours, a first precipitate is obtained;

[0148] S2, using a parallel flow co-precipitation method, adding a mixed solution containing zinc salt and urea and an alkaline solution dropwise to the first precipitate to continue a second precipitation reaction for 2 to 3 hours, controlling the reaction temperature to 40° C. and the system pH to 11.0, stirring evenly after the dropwise addition to obtain a reaction solution;

[0149] S3, the reaction solution was transferred to an autoclave, pressurized with N2 to 4 MPa, placed in an oven at 150°C for crystallization for 15 h, cooled, emptied, and centrifuged to obtain a crystallized solid;

[0150] S4. Add deionized water to the crystallized solid at a liquid-to-solid ratio of 60%, wash 5 times, and then place it in an oven to dry at 60-100°C, and then calcine it at 500°C for 18 hours in an air atmosphere, and crush it to a particle size of 40-60 mesh to obtain a ZnO-ZrO2-TiO2 solid solution catalyst, wherein the mass ratio of ZnO, ZrO2 and TiO2 is 20:48:32.

[0151] Embodiments 10 to 18

[0152] The method for preparing methanol provided in this example comprises the following steps:

[0153] A 5mL fixed bed reactor was used, the catalyst loading was 1.0g, diluted with 1.0g fine quartz sand, the reducing atmosphere was 5% H2-95% N2, the flow rate was 80mL / min, the reduction temperature was 350℃, and the reduction time was 8h; after the reduction process was completed, the pressure was increased to 3.0MPa with N2, the reaction temperature was maintained at 350℃, and the feed gas space velocity was 24000h -1 The raw gas composition is H2 / CO2=3.0 (volume ratio). The reaction is started after the temperature and pressure are stabilized. The reaction tail gas product is analyzed by online chromatography. The tail gas analysis conditions are: the chromatographic column is Porapak-T, the column temperature is 90°C, the carrier gas is argon, the flow rate is 25mL / min, and the current is 60mA. The liquid phase product is collected by a cold trap and taken out for chromatographic analysis. The analysis conditions are: the spectral column is TDX-01, the column temperature is 160°C, the carrier gas is argon, the flow rate is 30mL / min, and the current is 60mA.

[0154] The types of catalysts used in Examples 10 to 18 are shown in Table 1.

[0155] In Table 1, MeOH selectivity is the mass percentage of methanol to carbon-containing products;

[0156] STY MeOH Refers to the mass of methanol produced per unit time and per unit catalyst.

[0157] Table 1

[0158] catalyst <![CDATA[CO2 conversion rate (%)]]> MeOH selectivity (%) <![CDATA[STY M eOH g / (gcat·h)]]> Example 10 Cat-1 6.98 39.84 0.153 Embodiment 11 Cat-2 7.14 47.88 0.217 Example 12 Cat-3 7.79 53.97 0.228 Embodiment 13 Cat-4 6.55 50.14 0.287 Embodiment 14 Cat-5 8.80 58.20 0.315 Embodiment 15 Cat-6 5.78 61.52 0.251 Example 16 Cat-7 14.66 4.48 0.024 Embodiment 17 Cat-8 3.48 65.74 0.124 Embodiment 18 Cat-9 5.35 14.83 0.070

[0159] Examples 19 to 22

[0160] The method for preparing methanol provided in this example comprises the following steps:

[0161] A 5mL fixed bed reactor was used, the catalyst was Cat-5, the loading amount was 1.0g, diluted with 1.0g fine quartz sand, the reducing atmosphere was 5% H2-95% N2, the flow rate was 80mL / min, the reduction temperature was 350℃, and the reduction time was 8h; after the reduction process was completed, the pressure was increased to 3.0MPa with N2, and then at the reaction temperature, the raw gas was fed at a space velocity of 24000h -1 The raw gas composition is H2 / CO2=3.0 (volume ratio). The reaction is started after the temperature and pressure are stabilized. The reaction tail gas product is analyzed by online chromatography. The tail gas analysis conditions are: the chromatographic column is Porapak-T, the column temperature is 90°C, the carrier gas is argon, the flow rate is 25mL / min, and the current is 60mA. The liquid phase product is collected by a cold trap and taken out for chromatographic analysis. The analysis conditions are: the spectral column is TDX-01, the column temperature is 160°C, the carrier gas is argon, the flow rate is 30mL / min, and the current is 60mA.

[0162] The reaction temperatures of Examples 19 to 22 are shown in Table 2.

[0163] In Table 2, MeOH selectivity is the mass percentage of methanol to carbon-containing products;

[0164] STY MeOH Refers to the mass of methanol produced per unit time and per unit catalyst.

[0165] Table 2

[0166] Reaction temperature (℃) <![CDATA[CO2 conversion rate (%)]]> MeOH selectivity (%) <![CDATA[STY M eOH g / (gcat·h)]]> Embodiment 19 300 4.42 48.86 0.089 Embodiment 20 320 6.73 68.74 0.152 Embodiment 14 350 8.80 58.20 0.315 Embodiment 21 380 12.86 16.37 0.142 Embodiment 22 400 15.73 8.96 0.064

[0167] Embodiments 23 to 26

[0168] The method for preparing methanol provided in this example comprises the following steps:

[0169] A 5mL fixed bed reactor was used, the catalyst was Cat-3, the loading amount was 1.0g, diluted with 1.0g fine quartz sand, the reducing atmosphere was 5% H2-95% N2, the flow rate was 80mL / min, the reduction temperature was 350℃, and the reduction time was 8h; after the reduction process was completed, the temperature was lowered to 320℃, the pressure was flushed to the reaction pressure with N2, and the feed gas space velocity was 24000h -1 The raw gas composition is H2 / CO2=3.0 (volume ratio). The reaction is started after the temperature and pressure are stabilized. The reaction tail gas product is analyzed by online chromatography. The tail gas analysis conditions are: the chromatographic column is Porapak-T, the column temperature is 90°C, the carrier gas is argon, the flow rate is 25mL / min, and the current is 60mA. The liquid phase product is collected by a cold trap and taken out for chromatographic analysis. The analysis conditions are: the spectral column is TDX-01, the column temperature is 160°C, the carrier gas is argon, the flow rate is 30mL / min, and the current is 60mA.

[0170] The reaction pressures of Examples 23 to 26 are shown in Table 3.

[0171] In Table 3, MeOH selectivity is the mass percentage of methanol to carbon-containing products;

[0172] STY MeOH Refers to the mass of methanol produced per unit time and per unit catalyst.

[0173] Table 3

[0174] Reaction pressure (MPa) <![CDATA[CO2 conversion rate (%)]]> MeOH selectivity (%) <![CDATA[STY M eOH g / (gcat·h)]]> Embodiment 23 2 2.13 12.53 0.046 Embodiment 24 3 7.79 53.97 0.218 Embodiment 25 4 8.96 64.58 0.264 Embodiment 26 5 12.35 78.98 0.332

[0175] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A catalyst, characterized in that It comprises a ZnO-M oxide solid solution, wherein the M oxide comprises at least one of ZrO2, TiO2 and CeO2; and the ZnO-M oxide solid solution has a low-dimensional structure.

2. The catalyst according to claim 1, characterized in that In the ZnO-M oxide solid solution, the mass percentage of ZnO is 5% to 50%, and the mass percentage of M oxide is 50% to 95%.

3. The catalyst according to claim 1, characterized in that The particle size of the catalyst is 40 to 60 meshes.

4. The method for preparing the catalyst according to any one of claims 1 to 3, characterized in that: The steps include: S1, subjecting an M salt solution to a first precipitation reaction with an alkaline solution and aging the solution to obtain a first precipitate; the M salt solution comprises at least one of a Zr salt, a Ti salt and a Ce salt; S2, subjecting the mixed solution containing zinc salt and urea, the alkaline solution and the first precipitate to a second precipitation reaction to obtain a reaction solution; S3, the reaction solution is crystallized to obtain a crystallized solid; S4. The crystallized solid is washed, dried, calcined and crushed in sequence to obtain the catalyst.

5. The method for preparing the catalyst according to claim 4, characterized in that: In step S1 and step S2, the alkaline solution includes at least one of sodium carbonate, sodium hydroxide and ammonia water; And / or, the concentration of the alkaline solution is 0.3-2 mol / L.

6. The method for preparing the catalyst according to claim 4, characterized in that: In step S1, at least one of the following features (1) to (4) is included; (1) The total metal ion concentration of the M salt solution is 0.3 to 2.0 mol / L; (2) the first precipitation reaction comprises using a parallel flow co-precipitation method; (3) The temperature of the first precipitation reaction is 40 to 80° C., and the pH of the system is 8.0 to 12.0; (4) The aging time is 2 to 8 hours.

7. The method for preparing a catalyst according to claim 4, characterized in that: In step S2, at least one of the following features (1) to (3) is included; (1) The mass ratio of the zinc salt to the urea is 1:(0.3-0.8); (2) the second precipitation reaction comprises using a parallel flow co-precipitation method; (3) The temperature of the second precipitation reaction is 40-80° C., and the pH of the system is 8.0-12.

0.

8. The method for preparing a catalyst according to claim 4, characterized in that: In step S3, the crystallization temperature is 150-200°C and the pressure is 0.5-4.0Mpa; And / or, in step S4, the calcination includes: calcination at 300-600° C. for 10-24 hours.

9. A method for preparing methanol, characterized in that: The steps include: The methanol is obtained by reacting H2, CO2 and the catalyst described in any one of claims 1 to 3.

10. The method for preparing methanol according to claim 9, characterized in that: The reaction temperature is 300-400° C., and the reaction pressure is 2.0-5.0 MPa.

Citation Information

Patent Citations

  • Metal oxide-like solid solution catalyst as well as preparation and application thereof

    CN109420484A

  • Method for preparing mesoporous ZnO-ZrO2 solid solution catalyst and application of mesoporous ZnO-ZrO2 solid solution catalyst

    CN111841524A

  • Carbon dioxide hydrogenation catalyst and preparation method and application thereof

    CN113145113A

  • Catalyst for preparing methanol through CO2 hydrogenation as well as preparation method and application of catalyst

    CN114160117A

  • Catalyst for synthesizing carbon dioxide into methanol, preparation method therefor, and use thereof

    WO2023071244A1