Denitration catalyst with low sulfur dioxide oxidation rate and preparation method thereof
Supercrosslinked asphalt and porous carbon support were prepared through cross-linking reaction, and nanotitanium dioxide was modified and iron, manganese, cerium and other components were added, which solved the problem of existing catalysts being inactivated at high temperatures and achieved high efficiency in low temperatures. Flue gas denitrition and low SO2 oxidation rate are suitable for low-temperature denitrification of high-temperature flue gas.
Patent Information
- Application Number
- CN202411201535.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-08
AI Technical Summary
Existing SCR denitrification catalysts are prone to sintering and inactivation at high temperatures, resulting in problems such as decreasing denitrification activity, low selectivity, and high SO2/SO3 oxidation rate, which cannot meet the denitrification needs of high-temperature flue gases.
The supercrosslinked asphalt is prepared by cross-linking reaction, forming a porous carbon support through carbonization, and modifying nanotitanium dioxide on its surface, adding active components such as iron, manganese, cerium and urea, thereby improving the low-temperature activity of the catalyst and low SO2 oxidation through synergistic effects. Rate.
The denitrification activity is significantly improved within the range of 120-200℃, extend the service life of the catalyst, reduce the SO2 oxidation rate, slow down equipment blockage and corrosion, and achieve low-temperature and efficient flue gas denitrition.
Smart Images

Figure BDA0005017963280000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of waste gas treatment, and in particular to a denitration catalyst with a low sulfur dioxide oxidation rate and a preparation method thereof. Background Art
[0002] At present, SCR denitration catalysts have been put into use on a large scale, and the most widely used commercial catalyst is vanadium-tungsten-titanium-based SCR catalyst V 2 O 5 -WO 3 (MoO 3 ) / TiO 2 The activity window is 320-420℃. When the flue gas temperature exceeds the catalyst activity range, the catalyst will be sintered and deactivated, which will lead to decreased denitrification activity, low selectivity, and SO 2 / SO 3 The oxidation rate is high. This is due to the fact that anatase TiO 2 At high temperatures (>450°C), it is easy to transform into rutile. 2 O 5 The strong oxidation effect of SO in flue gas 2 Often converted to SO 3 , and then combines with ammonia and water in the flue gas to generate NH 4 HSO 4 , causing corrosion to the flue and equipment, and at the same time, V 2 O 5 It is toxic in itself and will cause secondary pollution to the environment. Therefore, this type of denitrification catalyst cannot meet the needs of high-temperature flue gas denitrification in distributed energy, boiling furnaces, industrial kilns, etc.
[0003] Therefore, the traditional denitrification catalyst has high reaction temperature and SO 2 / SO 3 Due to the high oxidation rate and other problems, the development of a low-sulfur oxidation and low-temperature denitrification catalyst is a technical problem that technicians in this field urgently need to solve. Summary of the invention
[0004] In order to solve the above problems, the present application provides a denitration catalyst with low sulfur dioxide oxidation rate and a preparation method thereof. The denitration catalyst with low sulfur dioxide oxidation rate prepared in the present application has good activity and low SO in the range of 120-200°C. 2 The oxidation rate shows excellent low-temperature denitrification performance, prolongs the service life of the catalyst, reduces equipment clogging and corrosion, and solves the problems of easy poisoning and deactivation, SO 2The problem of high oxidation rate. A super-crosslinked asphalt with large specific surface area, excellent performance and good stability is prepared through cross-linking reaction. Then, by precisely controlling the carbonization temperature and heating rate of the super-crosslinked asphalt, the pore structure of the porous carbon carrier can be well adjusted to obtain an ideal carrier for denitrification catalysis. Attaching nano-titanium dioxide to the surface of the porous carbon carrier can improve the dispersion of active components on the surface of the porous carbon carrier, promote the exposure of more catalytic active sites, and help improve the catalytic efficiency and low-temperature activity of the catalyst. It also has a certain anti-poisoning effect. The denitrification catalyst carrier loaded with iron, manganese, vanadium and cerium is mixed with urea, has a part of nitrogen element after nitrogen doping, has a very large specific surface area after calcination, and contains oxygen and nitrogen groups and a very large specific surface area, which is more conducive to NO and NH 3 The addition of iron, manganese and cerium active components and the synergistic effect between them make the denitrification catalyst have low-temperature and high-efficiency catalytic activity and low SO 2 The preparation method of the present application has simple process, low production cost, and is easy for industrial production, and has broad application prospects in the field of low-temperature flue gas denitrification.
[0005] In a first aspect, the present application provides a method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate, using the following technical scheme: A method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate comprises the following steps: S1. According to the mass fractions, coal tar pitch, p-phenylenedimethyl ether and concentrated sulfuric acid with a mass concentration of 98% are added to dichloromethane in sequence, and then the temperature is raised to 80-85°C, and the cross-linking reaction is carried out at this temperature for 10-14 hours. The product obtained by the reaction is first washed with anhydrous ethanol for 3 times, and then extracted with tetrahydrofuran for 4-6 hours, and then dried at a temperature of 75-85°C for 10-16 hours to obtain a super cross-linked asphalt; S2. In a high-temperature tube furnace, a certain amount of super-crosslinked asphalt is added and carbonized under an argon atmosphere. After the high-temperature tube furnace is completely cooled, a porous carbon carrier is obtained; S3, dissolving tetraethyl titanate in ethanol, adding a mixed solution containing ethanol, deionized water and nitric acid thereto, mixing evenly, adding a porous carbon carrier thereto, stirring and mixing evenly, drying after aging, and then calcining in an air atmosphere at 350-400° C. for 2-3 hours to obtain a denitration catalyst carrier; S4. Dissolve the iron source, manganese source, cerium source and vanadium source in deionized water, then add the denitration catalyst carrier thereto, disperse it evenly by ultrasonication, wash and dry it, mix it with urea, place it in a tubular furnace, roast it under a nitrogen atmosphere, grind it and pass it through a 80-mesh sieve to obtain a denitration catalyst with a low sulfur dioxide oxidation rate.
[0006] By adopting the above technical scheme, S1: Preparation of super cross-linked asphalt, super cross-linked asphalt is generated by cross-linking reaction of coal tar pitch, dimethyl paraben and concentrated sulfuric acid. The key to this step is to synthesize precursor materials with large specific surface area, excellent performance and good stability, laying the foundation for the subsequent preparation of porous carbon carriers. The optimization of the cross-linking reaction not only improves the physical structure of the material, but also provides support for the uniform distribution and stability of the active sites of the catalyst, thereby enhancing the performance of the final catalyst. S2: Preparation of porous carbon carrier, super cross-linked asphalt is carbonized in a high-temperature tubular furnace, and the obtained porous carbon carrier has a highly developed pore structure and a large specific surface area, providing a large number of attachment points and reaction interfaces for the catalyst. The optimization of the pore structure of the porous carbon carrier is conducive to improving the efficiency and selectivity of the catalytic reaction, and its stable chemical properties ensure the durability of the catalyst in harsh environments. S3: Preparation of denitration catalyst carrier, precursors such as tetraethyl titanate are combined with porous carbon carriers, and nano-titanium dioxide modified carbon carriers are formed by calcination. This step not only increases the active points of the catalyst, but also improves the anti-poisoning ability and low-temperature activity of the catalyst. The combination of nano-titanium dioxide and carbon carrier produces new active centers, which are crucial for the reduction reaction of NOx, while improving the catalytic activity of the catalyst and reducing SO 2 Oxidation rate. S4: The final preparation of the denitration catalyst is to introduce active components such as iron, manganese, cerium and vanadium into the catalyst system, and then mix with urea, roast and screen to obtain the final denitration catalyst. The denitration catalyst carrier loaded with iron, manganese, vanadium and cerium is mixed with urea, has a part of nitrogen element after nitrogen doping, has a very large specific surface area after roasting, and contains oxygen, nitrogen groups and a very large specific surface area, which is more conducive to NO and NH 3 The addition of iron, manganese and cerium active components and the synergistic effect between them make the denitrification catalyst have low-temperature and high-efficiency catalytic activity and low SO 2 In general, the preparation method of the present application achieves a significant improvement in the performance of the denitrification catalyst by precisely controlling each step of the material synthesis. From the preparation of the hyper-crosslinked asphalt to the formation of the porous carbon carrier, to the effective loading of the active components, each step is aimed at optimizing the structure and function of the catalyst, so that it has excellent denitrification efficiency and low SO at low temperatures. 2 The oxidation rate is high while maintaining long-term stability and durability. This preparation method is not only simple in process and cost-effective, but also very suitable for industrial production, providing an efficient and economical solution for the field of low-temperature flue gas denitrification.
[0007] Preferably, in step S1, the mass ratio of the coal tar pitch, p-xylene dimethyl ether, concentrated sulfuric acid with a mass concentration of 98% and dichloromethane is 1:(1.6-2.4):(2-3):6.
[0008] By adopting the above technical scheme, coal tar pitch: as a carbon source, coal tar pitch is converted into a super cross-linked pitch with a rich pore structure in the cross-linking reaction. Its high carbon content provides a good electron conduction path and a stable skeleton structure for the final catalyst. Dimethyl ether: as a cross-linking agent, it reacts with coal tar pitch to promote the formation of a three-dimensional network structure, increase the specific surface area and porosity of the super cross-linked pitch, and provide a location for the formation of catalytic active centers. Concentrated sulfuric acid (98%): as a catalyst, it accelerates the cross-linking reaction, promotes the chemical reaction between coal tar pitch and dimethyl ether, and improves the yield and quality of super cross-linked asphalt. Dichloromethane: as a solvent, it can evenly disperse the reactants to ensure the full progress of the reaction. At the same time, the volatility of dichloromethane is conducive to the subsequent drying and purification process. By precisely controlling the ratio of coal tar pitch to dimethyl ether, the cross-linking degree and pore structure of the super cross-linked asphalt can be adjusted, thereby affecting the performance of the final catalyst. Sufficient cross-linking agent can ensure the formation of a highly developed pore structure, while an appropriate amount of coal tar pitch provides sufficient carbon source to maintain the stability of the structure. Concentrated sulfuric acid not only promotes the cross-linking reaction, but may also affect the surface functional groups of the super-cross-linked asphalt, which have a direct impact on the distribution and strength of the catalytic active centers. In general, the mass fraction ratio of the raw materials in step S1 is obtained through optimization experiments, aiming to achieve the best performance of the super-cross-linked asphalt. The adjustment of this proportional relationship takes into account the reaction efficiency, product performance and convenience of subsequent processing, and reflects the precise control of reaction conditions and meticulous requirements for product performance during the material preparation process. These factors work together to ensure that the denitrification catalyst has good activity, selectivity and stability at low temperatures, while reducing the oxidation rate of sulfur dioxide.
[0009] Preferably, in step S2, the process conditions of the carbonization treatment are: heating to 1300-1400°C at a heating rate of 5-8°C / min and keeping the temperature for 3-4h.
[0010] By adopting the above technical scheme, the heating rate has a direct impact on the pore structure and performance of the final porous carbon carrier. A slower heating rate contributes to a more uniform and sufficient carbonization reaction, avoiding structural inhomogeneity or pore collapse caused by too fast temperature increase. : The high temperature range of 1300-1400℃ can ensure that the super-crosslinked asphalt is fully carbonized and converted into a porous carbon carrier with high specific surface area and excellent chemical stability. This temperature range is optimized. Too low may not achieve the ideal carbonization effect, and too high may cause structural damage. Keeping at this temperature for 3-4 hours can ensure that the inside and outside of the super-crosslinked asphalt are completely carbonized to form a stable porous structure. At the same time, a long enough time is conducive to the optimization and reconstruction of the pore structure, and improves the uniformity and availability of the pores. By precisely controlling the heating rate and target temperature, as well as sufficient insulation time, the pore size, distribution and volume of the porous carbon carrier can be optimized. This is extremely critical for the effective loading of subsequent active components, providing more active sites and promoting the catalytic reaction. High carbonization not only increases the specific surface area of the material, but also significantly improves its chemical corrosion resistance and thermal stability, which is crucial for maintaining the performance stability of the catalyst in harsh environments (such as high temperature, high pressure, and the presence of corrosive gases). Excellent pore structure is conducive to improving the adsorption capacity of the catalyst for reactants, especially for NO x and NH 3 , thereby improving the efficiency of the catalytic reaction. At the same time, a good pore structure is also conducive to the desorption of the reaction products, slowing down the deactivation of the catalyst due to product deposition. In summary, the carbonization treatment process conditions in step S2 are finely controlled to achieve the optimization of the structure and performance of the porous carbon carrier, laying a solid foundation for the efficient performance of the subsequent denitration catalyst. This step demonstrates the attention to detail and the pursuit of the ultimate performance goals in the material preparation process, and reflects the scientificity and practicality of the preparation method.
[0011] Preferably, in step S3, the mass ratio of tetraethyl titanate, ethanol, mixed solution and porous carbon carrier is 2:(20-25):(12-15):(6-8).
[0012] By adopting the above technical scheme, by controlling the ratio of tetraethyl titanate to the porous carbon carrier, the coverage and particle size of nano-titanium dioxide on the carrier surface can be accurately controlled to achieve the maximum distribution of active sites, while avoiding excessive titanium coverage leading to pore blockage. As a solvent, the ratio of ethanol to tetraethyl titanate directly affects the rate and degree of hydrolysis and condensation reaction of tetraethyl titanate, and then affects the nucleation and growth process of titanium dioxide particles. Optimizing this ratio can achieve the regulation of particle size. The water and nitric acid in the mixed solution not only affect the hydrolysis reaction of tetraethyl titanate, but also control the surface properties of titanium dioxide particles by adjusting the acidity and alkalinity of the solution, and enhance the adsorption and activation ability of the catalyst to the reactants. The ratio of the entire system is carefully designed to achieve the optimal loading effect of nano-titanium dioxide particles, ensure their uniform dispersion on the porous carbon carrier, and maintain the porosity and specific surface area of the carrier to facilitate the efficient catalytic reaction. In summary, in step S3, by precisely controlling the mass ratio of tetraethyl titanate, ethanol, mixed solution and porous carbon support, the microstructure and performance of the denitrification catalyst were effectively regulated, thereby obtaining a catalyst with excellent low-temperature activity and low SO 2 The optimization of this ratio relationship reflects a deep understanding of the details of material synthesis and provides a strong guarantee for achieving efficient and stable flue gas denitrification.
[0013] Preferably, in step S3, the mass ratio of ethanol, deionized water and nitric acid in the mixed solution is 10:(4-6):(5-7).
[0014] Preferably, in step S4, the mass ratio of the iron source, manganese source, cerium source, vanadium source and denitration catalyst carrier is 5:(15-20):(3-6):(6-8):100.
[0015] By adopting the above technical solution, iron as one of the active components can improve the low temperature activity of the catalyst and reduce SO 2Oxidation rate. The mass fraction of iron source is less than that of other elements, which helps to ensure its uniform distribution in the catalyst and avoid the coverage of active sites caused by excessive aggregation. Manganese mainly provides redox performance in the catalyst, which is beneficial to the conversion of NOx. Its mass fraction is large because manganese can promote the adsorption and conversion of NOx at a lower temperature and improve the overall activity of the catalyst. The addition of cerium can enhance the oxygen storage capacity and stability of the catalyst, which helps to improve the efficiency of the catalyst in the use of oxygen during the reaction. An appropriate amount of cerium source can be effectively dispersed in the catalyst to provide the necessary oxygen vacancies. Vanadium is a commonly used active component in SCR (selective catalytic reduction) catalysts, which can effectively promote the reduction reaction of NOx. The proportion of vanadium source is adjusted to achieve efficient catalytic activity while controlling the toxicity risk of vanadium. DeNOx catalyst carrier: As a support for the active component, it ensures sufficient specific surface area and pore structure, provides a good dispersion medium for the active component, and maintains the mechanical strength and chemical stability of the catalyst. The reasonable ratio of the four metal elements of iron, manganese, cerium and vanadium enables them to promote each other in the catalytic reaction, forming more active centers, improving the low-temperature activity of the catalyst and reducing SO 2 The carrier not only provides physical support, but its surface properties may also react chemically with the active components to form new active sites or promote electron transfer, further enhancing the catalytic activity. By precisely controlling the mass fraction of each active component, the overlap of active sites and pore blockage caused by excessive loading is avoided, ensuring the high activity and stability of the catalyst. While ensuring high-efficiency and low-temperature denitrification performance, SO is reduced by optimizing the component ratio. 2 In summary, by using the specific mass fraction ratio of the iron source, manganese source, cerium source, vanadium source and denitration catalyst carrier in step S4, effective synergy between multiple components is achieved, thereby obtaining a catalyst with excellent low temperature activity, low SO 2 The oxidation rate and wide adaptability of the denitrification catalyst. The careful adjustment of this proportional relationship reflects the in-depth understanding of material design and performance regulation, and provides important support for the advancement of low-temperature flue gas denitrification technology.
[0016] Preferably, in step S4, the mass ratio of the denitration catalyst carrier to the urea is 100:13-16.
[0017] By adopting the above technical solution, urea: During the calcination process, urea not only acts as a nitrogen source to introduce nitrogen into the catalyst, but also acts as a mild reducing agent to a certain extent, which helps the metal active components to better disperse and form active phases at a lower temperature. By mixing with urea and calcining, nitrogen is introduced into the catalyst to form nitrogen-containing functional groups. These functional groups can enhance the catalyst's resistance to NO and NH 3The decomposition reaction of urea during the calcination process helps to increase the specific surface area of the catalyst and provide more active sites for the catalytic reaction. Calcination in a nitrogen-containing atmosphere promotes the interaction between active components such as iron, manganese, cerium and vanadium and the carrier, which helps to form a more stable active phase. These active phases have a highly efficient catalytic effect on low-temperature denitrification reactions. The addition of urea may also affect the surface acid-base properties of the catalyst. By changing the Bronster acid or basic sites on the surface, the adsorption-desorption performance of the catalyst for reactants can be further optimized. The introduction of nitrogen not only improves the denitrification activity of the catalyst, but also helps to reduce SO 2 Oxidation rate, because nitrogen functional groups can react with SO 2 Compete for adsorption sites, reduce the generation of sulfate species, and thus reduce the oxidation rate of sulfur dioxide. By precisely controlling the ratio of the denitrification catalyst carrier to urea, the effective introduction of nitrogen is ensured without excess, avoiding excessive nitridation of the catalyst surface or pore blockage due to excessive urea, and maintaining the mechanical strength and chemical stability of the catalyst. In summary, the precise control of the mass fraction ratio of the denitrification catalyst carrier to urea in step S4 not only optimizes the surface chemical properties and physical structure of the catalyst, but also improves the low-temperature denitrification activity of the catalyst and reduces SO through the introduction of nitrogen. 2 The oxidation rate shows the scientificity and practicality of the preparation method. The careful adjustment of this proportional relationship reflects the in-depth understanding of material design and performance regulation, and provides important support for the advancement of low-temperature flue gas denitrification technology.
[0018] Preferably, in step S4, the manganese source is at least one of manganese chloride, manganese sulfate, manganese nitrate, and manganese acetate, the cerium source is at least one of cerium nitrate, ammonium cerium nitrate, and cerium sulfate, the cerium source is at least one of ammonium metavanadate, vanadyl sulfate, and vanadyl acetylacetonate, and the iron source is at least one of ferric chloride, ferric sulfate, and ferric nitrate.
[0019] Preferably, in step S4, the calcination temperature is 400-480° C., and the calcination time is 3-5 hours.
[0020] In the second aspect, the present application provides a denitration catalyst with a low sulfur dioxide oxidation rate, adopting the following technical scheme: As a general technical concept, the present application also provides the above-mentioned denitration catalyst with a low sulfur dioxide oxidation rate, which is prepared by the preparation method of the above-mentioned denitration catalyst with a low sulfur dioxide oxidation rate.
[0021] In summary, the beneficial technical effects of this application are: 1. Low-temperature denitration activity: Through a specific preparation process, the obtained denitration catalyst exhibits good denitration activity in the temperature range of 120-200°C. This feature makes the catalyst very suitable for flue gas treatment in low-temperature environments, and can effectively remove nitrogen oxides in flue gas, meeting modern environmental protection requirements.
[0022] 2. Low SO 2 Oxidation rate: The catalyst not only has excellent low-temperature denitrification performance, but also has excellent low SO 2 This means that in a sulfur-containing environment, the catalyst can still maintain a stable denitrification efficiency, thereby extending the service life of the catalyst and reducing corrosion and clogging problems of the equipment.
[0023] 3. Stability and durability: The preparation of hyper-crosslinked asphalt and subsequent precise carbonization treatment endow the catalyst with highly stable physical and chemical properties. This stability ensures that the catalyst maintains high performance during long-term operation, reduces replacement frequency, and reduces operation and maintenance costs.
[0024] 4. Improvement of catalytic efficiency: The uniform dispersion of nano-titanium dioxide on the surface of the porous carbon carrier provides abundant active sites for the catalyst, which can effectively promote the reaction of reactants (such as NO and NH 3 ) adsorption and conversion, thereby improving the overall catalytic efficiency.
[0025] 5. Synergistic effect: The reasonable ratio of active components such as iron, manganese, cerium, vanadium and nitrogen doping with urea produces a significant synergistic effect. This synergistic effect not only enhances the low-temperature activity of the catalyst, but also improves its anti-toxicity, so that the catalyst can still maintain efficient denitrification performance in complex flue gas components.
[0026] 6. Advantages of production process: The preparation method of the present application is simple and easy to operate, and the raw materials are readily available, which is conducive to reducing production costs and facilitating large-scale industrial production. This is not only conducive to the promotion and application of environmental protection technology, but also helps to reduce the environmental protection investment costs of enterprises.
[0027] 7. Wide application prospects: Given its low temperature, high activity and low SO 2 With the characteristics of high oxidation rate, this denitrification catalyst has great application potential in the field of low-temperature flue gas denitrification. It provides an effective means of controlling nitrogen oxides for emission sources such as industrial boilers and kilns, which is of great significance for promoting industry emission reduction upgrades and improving air quality. DETAILED DESCRIPTION
[0028] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0029] Example 1 A method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate comprises the following steps: S1. According to the mass fractions, 10 kg coal tar pitch, 16 kg p-phenylenedimethyl ether and 20 kg concentrated sulfuric acid with a mass concentration of 98% were added to 60 kg dichloromethane, and then the temperature was raised to 80 ° C. The cross-linking reaction was kept warm for 14 hours. The product obtained by the reaction was first washed with anhydrous ethanol for 3 times, then extracted with tetrahydrofuran for 4 hours, and then dried at 75 ° C for 16 hours to obtain super cross-linked asphalt; S2. In a high-temperature tube furnace, a certain amount of super-crosslinked asphalt is added, and the temperature is raised to 1300°C at a heating rate of 5°C / min under an argon atmosphere and kept at this temperature for 4 hours. After the high-temperature tube furnace is completely cooled, a porous carbon support is obtained; S3, dissolving 4 kg of tetraethyl titanate in 40 kg of ethanol, adding 24 kg of a mixed solution containing ethanol, deionized water and nitric acid thereto, mixing evenly, adding 12 kg of a porous carbon carrier thereto, stirring and mixing evenly, drying after aging, and then calcining in an air atmosphere at 350 ° C for 3 h to obtain a denitration catalyst carrier; wherein the mass ratio of ethanol, deionized water and nitric acid in the mixed solution is 10:4:5; S4. Dissolve 0.5 kg of ferric chloride, 1.5 kg of manganese chloride, 0.3 kg of cerium nitrate and 0.6 kg of ammonium metavanadate in 40 L of deionized water, then add 10 kg of the denitration catalyst carrier thereto, disperse it evenly by ultrasonication, wash and dry it, mix it with 1.3 kg of urea, place it in a tubular furnace, and roast it at 400 ° C in a nitrogen atmosphere for 5 hours, then grind it and pass it through a 80-mesh sieve to obtain a denitration catalyst with a low sulfur dioxide oxidation rate.
[0030] Example 2 A method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate comprises the following steps: S1. According to the mass fractions, 10 kg coal tar pitch, 24 kg p-phenylenedimethyl ether and 30 kg concentrated sulfuric acid with a mass concentration of 98% are added to 60 kg dichloromethane, and then the temperature is raised to 85 ° C. The cross-linking reaction is kept for 10 hours. The product obtained by the reaction is first washed with anhydrous ethanol for 3 times, then extracted with tetrahydrofuran for 6 hours, and then dried at 85 ° C for 10 hours to obtain super cross-linked asphalt; S2. In a high-temperature tube furnace, a certain amount of super-crosslinked asphalt is added, and the temperature is raised to 1400°C at a heating rate of 8°C / min under an argon atmosphere and kept at this temperature for 3 hours. After the high-temperature tube furnace is completely cooled, a porous carbon support is obtained; S3, dissolving 4 kg of tetraethyl titanate in 50 kg of ethanol, adding 30 kg of a mixed solution containing ethanol, deionized water and nitric acid thereto, mixing evenly, adding 16 kg of a porous carbon carrier thereto, stirring and mixing evenly, drying after aging, and then calcining in an air atmosphere at 400 ° C for 2 h to obtain a denitration catalyst carrier; wherein the mass ratio of ethanol, deionized water and nitric acid in the mixed solution is 10:6:7; S4. Dissolve 0.5 kg of ferric sulfate, 2 kg of manganese sulfate, 0.6 kg of cerium sulfate and 0.8 kg of vanadyl sulfate in 40 L of deionized water, then add 10 kg of the denitration catalyst carrier thereto, disperse it evenly by ultrasonication, wash and dry it, mix it with 1.6 kg of urea, place it in a tubular furnace, roast it at 480 ° C in a nitrogen atmosphere for 3 hours, then grind it and pass it through a 80-mesh sieve to obtain a denitration catalyst with a low sulfur dioxide oxidation rate.
[0031] Example 3 A method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate comprises the following steps: S1. According to the mass fractions, 10 kg coal tar pitch, 20 kg p-phenylenedimethyl ether and 25 kg concentrated sulfuric acid with a mass concentration of 98% were added to 60 kg dichloromethane, and then the temperature was raised to 83 ° C. The cross-linking reaction was kept warm for 12 hours. The product obtained by the reaction was first washed with anhydrous ethanol for 3 times, then extracted with tetrahydrofuran for 5 hours, and then dried at 80 ° C for 13 hours to obtain super cross-linked asphalt; S2. In a high-temperature tube furnace, a certain amount of super-crosslinked asphalt is added, and the temperature is raised to 1360°C at a heating rate of 6°C / min under an argon atmosphere and kept at this temperature for 3.5 hours. After the high-temperature tube furnace is completely cooled, a porous carbon support is obtained; S3, dissolving 4 kg of tetraethyl titanate in 45 kg of ethanol, adding 27 kg of a mixed solution containing ethanol, deionized water and nitric acid thereto, mixing evenly, adding 14 kg of a porous carbon carrier thereto, stirring and mixing evenly, drying after aging, and then calcining in an air atmosphere at 380 ° C for 2.5 h to obtain a denitration catalyst carrier; wherein the mass ratio of ethanol, deionized water and nitric acid in the mixed solution is 10:5:6; S4. Dissolve 0.5 kg of ferric nitrate, 1.8 kg of manganese nitrate, 0.5 kg of ammonium cerium nitrate and 0.7 kg of acetylacetonato vanadyl in 40 L of deionized water, then add 10 kg of the denitration catalyst carrier thereto, disperse it evenly by ultrasonication, wash and dry it, mix it with 1.45 kg of urea, place it in a tubular furnace, and roast it at 450 ° C in a nitrogen atmosphere for 4 hours, then grind it and pass it through a 80-mesh sieve to obtain a denitration catalyst with a low sulfur dioxide oxidation rate.
[0032] Comparative Example 1 The same as Example 3, except that: there is no step S1 and step S2, and in step S3, an equal amount of activated carbon (specific surface area of 953.5m 2 / g, and the total pore volume is 1.137cm 3 / g) to replace the porous carbon support.
[0033] Comparative Example 2 The method is the same as Example 3, except that: there is no step S3, and in step S4, an equal amount of porous carbon carrier is used to replace the denitration catalyst carrier.
[0034] Comparative Example 3 The present invention is the same as Example 3, except that: in step S4, 0.5 kg of ferric nitrate, 1.8 kg of manganese nitrate, 0.5 kg of ammonium cerium nitrate and 0.7 kg of acetylacetonato vanadium are dissolved in 40 L of deionized water, and then 10 kg of the denitration catalyst carrier is added thereto, ultrasonically dispersed evenly, washed and dried, placed in a tubular furnace, and calcined at 450° C. under a nitrogen atmosphere for 4 hours, and then ground and passed through a 80-mesh sieve to obtain a denitration catalyst with a low sulfur dioxide oxidation rate.
[0035] Comparative Example 4 The present invention is the same as Example 3, except that: in step S4, 2.8 kg of ferric nitrate and 0.7 kg of vanadium acetylacetonate are dissolved in 40 L of deionized water, and then 10 kg of the denitration catalyst carrier is added thereto, ultrasonically dispersed evenly, washed and dried, and then mixed with 1.45 kg of urea, placed in a tubular furnace, and calcined at 450° C. for 4 hours under a nitrogen atmosphere, and then ground and passed through a 80-mesh sieve to obtain a denitration catalyst with a low sulfur dioxide oxidation rate.
[0036] Comparative Example 5 The present invention is the same as Example 3, except that: in step S4, 2.8 kg of manganese nitrate and 0.7 kg of vanadium acetylacetonate are dissolved in 40 L of deionized water, and then 10 kg of the denitration catalyst carrier is added thereto, ultrasonically dispersed evenly, washed and dried, and then mixed with 1.45 kg of urea, placed in a tubular furnace, and calcined at 450° C. for 4 h in a nitrogen atmosphere, and then ground and passed through a 80-mesh sieve to obtain a denitration catalyst with a low sulfur dioxide oxidation rate.
[0037] Comparative Example 6 The present invention is the same as Example 3, except that: in step S4, 2.8 kg of ammonium cerium nitrate and 0.7 kg of vanadium acetylacetonate are dissolved in 40 L of deionized water, and then 10 kg of the denitration catalyst carrier is added thereto, ultrasonically dispersed evenly, washed and dried, and then mixed with 1.45 kg of urea, placed in a tubular furnace, and calcined at 450° C. for 4 h in a nitrogen atmosphere, and then ground and passed through a 80-mesh sieve to obtain a denitration catalyst with a low sulfur dioxide oxidation rate.
[0038] Performance Testing 1. Catalyst activity evaluation: Take 0.5g of the denitration catalyst with low sulfur dioxide oxidation rate prepared in Examples 1 to 3 and Comparative Examples 1 to 6 respectively, and carry out SCR reaction. Raise the reactor program to the required temperature and keep it stable, and record the NO x The concentration changes and calculation of NO x The catalytic performance of the catalyst was evaluated using a fixed reaction bed with a diameter of 15 mm. The simulated gas composition is as follows: NO x The flow rate was set to 40 mL / min, and NH 3 The flow rate was set to 40 mL / min, with a volume ratio of 3% O 2 , N 2 As the balance gas; the total gas flow rate is 1000mL / min. Under the conditions of 120℃, 140℃, 160℃, 180℃ and 200℃, the concentration of NOx at the inlet and outlet was tested using a Testo flue gas analyzer to obtain the denitration efficiency of the catalyst for NOx at different temperatures. The test results are shown in Table 1.
[0039] 2. SO 2 / SO 3 Oxidation rate test test conditions: test temperature 150℃, NH 3 Concentration 500ppm, NH 3 / NO=1,SO 2 Concentration 500ppm, H 2 O concentration 8%, GHSV = 120000h -1 , 0.5g of denitrification catalyst with low sulfur dioxide oxidation rate, the results are shown in Table 2.
[0040] Table 1 Catalyst activity results Table 2SO 2 / SO 3 Oxidation rate project <![CDATA[SO 2 / SO 3 Oxidation rate (%)]]> Example 1 0.15 Example 2 0.11 Example 3 0.12 Comparative Example 1 0.85 Comparative Example 2 0.97 Comparative Example 3 0.98 Comparative Example 4 1.85 Comparative Example 5 1.67 Comparative Example 6 1.98 Analyzing the data in Tables 1 and 2, we can see that: 1) The denitration catalyst with low sulfur dioxide oxidation rate prepared in Examples 1 to 3 has excellent catalytic activity and low SO 2 The oxidation rate shows excellent low-temperature denitrification performance, prolongs the service life of the catalyst, reduces equipment clogging and corrosion, and solves the problems of easy poisoning and deactivation, SO 2 The problem of high oxidation rate.
[0041] 2) The performance comparison analysis of the denitration catalyst with low sulfur dioxide oxidation rate prepared in combination with Example 3 and Comparative Example 1 shows that the porous carbon carrier of the present application prepares a super-crosslinked asphalt with large specific surface area, excellent performance and good stability through a crosslinking reaction, and then the pore structure of the porous carbon carrier can be well adjusted by accurately controlling the carbonization temperature and heating rate of the super-crosslinked asphalt to obtain an ideal carrier for denitration catalysis. It ensures that the denitration catalyst has good activity, selectivity and stability at low temperatures, while reducing the oxidation rate of sulfur dioxide.
[0042] 3) The performance comparison analysis of the denitration catalyst with low sulfur dioxide oxidation rate prepared in combination with Example 3 and Comparative Example 2 shows that the precursors such as tetraethyl titanate are combined with the porous carbon support and calcined to form a carbon support modified with nano-titanium dioxide. This step not only increases the active points of the catalyst, but also improves the anti-poisoning ability and low-temperature activity of the catalyst. The combination of nano-titanium dioxide and the carbon support produces new active centers, which are crucial for the reduction reaction of NOx, while improving the catalytic activity of the catalyst and reducing SO 2 Oxidation rate.
[0043] 4) The performance comparison analysis of the denitration catalyst with low sulfur dioxide oxidation rate prepared in combination with Example 3 and Comparative Example 3 shows that the denitration catalyst carrier loaded with iron, manganese, vanadium and cerium is mixed with urea, has a part of nitrogen element after nitrogen doping, has a very large specific surface area after calcination, and contains oxygen and nitrogen groups and a very large specific surface area, which is more conducive to NO and NH 3 The adsorption of the reaction gas is beneficial to the adsorption of the reaction gas and improves the catalytic effect.
[0044] 5) The performance comparison analysis of the denitration catalyst with low sulfur dioxide oxidation rate prepared in combination with Example 3 and Comparative Examples 4 to 6 shows that the addition of iron, manganese and cerium active components and the synergistic effect between them make the denitration catalyst have low temperature and high efficiency catalytic activity and low SO 2 Oxidation rate.
[0045] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation methods of the present application can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate, characterized in that: The following steps are involved: S1. According to the mass fractions, coal tar pitch, p-phenylenedimethyl ether and concentrated sulfuric acid with a mass concentration of 98% are added to dichloromethane in sequence, and then the temperature is raised to 80-85°C, and the cross-linking reaction is carried out at this temperature for 10-14 hours. The product obtained by the reaction is first washed with anhydrous ethanol for 3 times, and then extracted with tetrahydrofuran for 4-6 hours, and then dried at a temperature of 75-85°C for 10-16 hours to obtain a super cross-linked asphalt; S2. In a high-temperature tube furnace, a certain amount of super-crosslinked asphalt is added and carbonized under an argon atmosphere. After the high-temperature tube furnace is completely cooled, a porous carbon carrier is obtained; S3, dissolving tetraethyl titanate in ethanol, adding a mixed solution containing ethanol, deionized water and nitric acid thereto, mixing evenly, adding a porous carbon carrier thereto, stirring and mixing evenly, drying after aging, and then calcining in an air atmosphere at 350-400° C. for 2-3 hours to obtain a denitration catalyst carrier; S4. Dissolve the iron source, manganese source, cerium source and vanadium source in deionized water, then add the denitration catalyst carrier thereto, disperse it evenly by ultrasonication, wash and dry it, mix it with urea, place it in a tubular furnace, roast it under a nitrogen atmosphere, grind it and pass it through a 80-mesh sieve to obtain a denitration catalyst with a low sulfur dioxide oxidation rate.
2. The method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate according to claim 1, characterized in that: In step S1, the mass ratio of the coal tar pitch, p-xylene dimethyl ether, concentrated sulfuric acid with a mass concentration of 98% and dichloromethane is 1:(1.6-2.4):(2-3):
6.
3. The method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate according to claim 1, characterized in that: In step S2, the process conditions of the carbonization treatment are: heating to 1300-1400°C at a heating rate of 5-8°C / min and keeping the temperature for 3-4h.
4. The method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate according to claim 1, characterized in that: In step S3, the mass ratio of tetraethyl titanate, ethanol, mixed solution and porous carbon carrier is 2:(20-25):(12-15):(6-8).
5. The method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate according to claim 1, characterized in that: In step S3, the mass ratio of ethanol, deionized water and nitric acid in the mixed solution is 10:(4-6):(5-7).
6. The method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate according to claim 1, characterized in that: In step S4, the mass ratio of the iron source, manganese source, cerium source, vanadium source and denitration catalyst carrier is 5:(15-20):(3-6):(6-8):
100.
7. The method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate according to claim 1, characterized in that: In step S4, the mass ratio of the denitration catalyst carrier to the urea is 100:13-16.
8. The method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate according to claim 1, characterized in that: In step S4, the manganese source is at least one of manganese chloride, manganese sulfate, manganese nitrate, and manganese acetate, the cerium source is at least one of cerium nitrate, ammonium cerium nitrate, and cerium sulfate, the cerium source is at least one of ammonium metavanadate, vanadyl sulfate, and vanadyl acetylacetonate, and the iron source is at least one of ferric chloride, ferric sulfate, and ferric nitrate.
9. The method for preparing a denitration catalyst with a low sulfur dioxide oxidation rate according to claim 1, characterized in that: In step S4, the calcination temperature is 400-480°C, and the calcination time is 3-5h.
10. A denitration catalyst with low sulfur dioxide oxidation rate, characterized in that: The denitration catalyst with a low sulfur dioxide oxidation rate is prepared by the preparation method of the denitration catalyst with a low sulfur dioxide oxidation rate according to any one of claims 1-9.