A method for preparing a monolithic catalyst with a high molecular weight polymer as a carrier suitable for ultra-low temperature SCR reaction

By using a monolithic catalyst with polymer as a support, the problems of poor effect and high cost of low-temperature SCR catalysts in the prior art are solved, and high-efficiency nitrogen oxide removal in the range of 100 to 200°C are achieved, thus reducing the Disposal costs of waste incineration power plants.

CN115445660BActive Publication Date: 2024-12-06ZHEJIANG ZHENENG TECHN RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211227166.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-09
Publication Date
2024-12-06
Estimated Expiration
2042-10-09

AI Technical Summary

Technical Problem

The existing SCR denitrification catalysts have poor effect under low temperature conditions, resulting in high nitrogen oxide treatment costs in the flue gas of waste incineration power plants, and the traditional monolithic catalyst materials are dense and costly.

Method used

The metal oxide pellets are prepared by impregnation method by using polymer polymer as a support, and fixed on the polymer polymer plate to form a monolithic catalyst, which is suitable for low-temperature SCR reactions of 100 to 200°C.

Benefits of technology

It reduces the cost and installation cost of the SCR reaction device, improves the efficiency of catalyst utilization, and achieves efficient denitrification activity and selectivity under low temperature conditions. It is suitable for exhaust gas treatment in waste incineration power plants and other industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115445660B_ABST
    Figure CN115445660B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing an integral catalyst suitable for ultra-low temperature SCR reaction with a high molecular polymer as a carrier, comprising the steps of: dissolving a metal salt to impregnate a metal oxide pellet, drying the metal oxide pellet; placing the metal oxide pellet in an environment filled with ammonia and water vapor for fumigation; roasting to obtain a catalyst pellet; dispersing the catalyst pellet on the surface of a high molecular polymer plate; heating the high molecular polymer plate to allow the catalyst pellet to sink into it; cooling the high molecular polymer plate to harden it, and assembling to obtain an integral catalyst. The beneficial effects of the present invention are: using a high molecular polymer plate as a carrier of an integral catalyst can greatly reduce the cost and installation cost of an SCR reaction device; utilizing the property of the high molecular polymer to soften at the glass transition temperature to allow the catalyst pellet to sink into the surface of the polymer plate and be automatically fixed; the prepared low temperature SCR catalyst has good denitration activity and selectivity, and is suitable for a low temperature range of 100 to 200°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of catalyst preparation technology and nitrogen oxide control technology in environmental protection, and specifically relates to a novel method for preparing a monolithic catalyst with a high molecular polymer as a carrier suitable for ultra-low temperature SCR reaction. The catalyst of the present invention is suitable for removing nitrogen oxides from industrial flue gas, especially the denitrification process of flue gas from waste incineration power plants. Background Art

[0002] In recent years, my country's waste incineration power generation industry has developed rapidly, making great contributions to reducing urban solid waste and landfill land. However, waste incineration flue gas contains a large number of harmful substances that need to be treated. Among them, nitrogen oxides are one of the main air pollutants, which not only harms human health, but also causes photochemical pollution, acid rain and other pollution. At present, the treatment technology of nitrogen oxides is mainly based on the selective catalytic reduction (SCR) of nitrogen oxides, but the denitration temperature range of commercial SCR denitration catalyst V2O5-MoO3(WO3) / TiO2 is 300-350℃, while the tail gas temperature at the denitration device of the waste incineration power plant is between 150 and 200℃. If a commercial SCR denitration catalyst is used, the tail gas needs to be heated to increase its temperature, but this process is not conducive to the economic benefits of the plant, so it is urgent to develop a low-temperature SCR catalyst.

[0003] The integral catalyst is divided into three parts: active ingredients, matrix and carrier. The carrier is mainly some materials that can form an integral structure, generally cordierite or metal. However, cordierite and metal have a large density, and the SCR steel bracket and installation costs will inevitably increase. The catalyst cost in the SCR reactor device accounts for about 50%, and the SCR steel bracket and installation fee account for about 50%. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing an integral catalyst with a high molecular weight polymer as a carrier and suitable for an ultra-low temperature SCR reaction.

[0005] The method for preparing the monolithic catalyst with a high molecular weight polymer as a carrier and suitable for ultra-low temperature SCR reaction comprises the following steps:

[0006] S1. Dissolve the iron salt and the manganese salt in deionized water, impregnate the metal oxide pellets by an equal volume impregnation method, and then dry them in an oven until the outer surface of the metal oxide pellets is dry;

[0007] S2, placing the dried metal oxide pellets in a sealed container filled with ammonia and water vapor, and heating and fumigating;

[0008] S3, calcining the fumigated metal oxide pellets to obtain catalyst pellets;

[0009] S4, dispersing the catalyst beads on the surface of the polymer plate;

[0010] S5, heating the polymer plate to the glass transition temperature, so that the catalyst balls sink into the softened polymer plate surface;

[0011] S6. Lowering the temperature to harden the polymer plates, and assembling the polymer plates to obtain an integral catalyst.

[0012] Preferably, in step S1: the iron salt is one or more of ferric nitrate, ferric chloride, ferric sulfate and ferric acetate; the manganese salt is one or more of manganese acetate, manganese nitrate, manganese sulfate and manganese chloride; and a cerium salt may be selectively added to the deionized water for dissolution, and the cerium salt is one or more of cerium nitrate, ammonium cerium nitrate, cerium sulfate and cerium chloride.

[0013] Preferably, the diameter of the metal oxide spheres is 4 to 10 mm; the metal oxide spheres are composed of one or more of aluminum oxide, silicon dioxide and titanium dioxide.

[0014] Preferably, in step S4: the average density of the catalyst beads dispersed on the surface of the polymer plate is 0.4-0.8 g / m 2 .

[0015] Preferably, in step S1, the drying temperature is 60-80° C., and the drying time is 10-60 minutes.

[0016] Preferably, in step S2: the ammonia concentration in the closed container is 0.001-1%, the water vapor concentration is 1-15%, the fumigation temperature is 50-95° C., and the fumigation time is 1-5 hours.

[0017] Preferably, in step S3: the calcination temperature is 300-600° C., and the calcination time is 1-3 hours.

[0018] Preferably, in step S4, the polymer plate is composed of one or more of polyacrylamide, polyvinyl carbazole, polycarbonate, polysulfone, polyphenylene ether sulfone, polyimide, polyamide-imide and polyetherimide.

[0019] Preferably, in step S4: the shape of the polymer plate is one or more of a plate shape, a corrugated plate shape, a honeycomb shape, and a plate with holes.

[0020] Preferably, the amount of Fe source in the catalyst pellets, calculated as Fe2O3, is 5 to 20 wt.% of the total mass of the catalyst pellets; the amount of Ce source, calculated as CeO2, is 0 to 20 wt.% of the total mass of the catalyst pellets; the amount of Mn source, calculated as MnO2, is 20 to 50 wt.% of the total mass of the catalyst pellets; the amount of Al source, calculated as Al2O3, is 0 to 70 wt.% of the total mass of the catalyst pellets; the amount of Si source, calculated as SiO2, is 0 to 70 wt.% of the total mass of the catalyst pellets; the amount of Ti source, calculated as TiO2, is 0 to 70 wt.% of the total mass of the catalyst pellets.

[0021] The beneficial effects of the present invention are:

[0022] 1) The present invention uses a polymer plate as a carrier of the monolithic catalyst. Compared with cordierite and metal used in traditional monolithic catalysts, the polymer has low density, low price and simple processing. Therefore, the preparation method of the present invention can greatly reduce the cost and installation cost of the SCR reaction device; and the working conditions of the flue gas terminal of the waste incineration power plant are low dust and low temperature, and the polymer can meet the working operation requirements.

[0023] 2) The present invention utilizes the property of high molecular polymer to soften at the glass transition temperature, so that the catalyst beads are sunk into the surface of the polymer plate and automatically fixed, without the need for additives such as adhesives, surfactants, and modifiers, which can improve the utilization efficiency of catalytic active centers and reduce the amount of catalyst used.

[0024] 3) The low-temperature SCR catalyst prepared by the present invention has good denitration activity and selectivity, and is suitable for the low temperature range of 100 to 200°C. It can be directly used for the denitration treatment of tail gas in industries such as waste incineration power plants, steel sintering and non-ferrous smelting, without the need for preheating, thereby reducing the cost of denitration treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of the denitration efficiency of the integral catalyst obtained in an embodiment of the present invention. DETAILED DESCRIPTION

[0026] The present invention is further described below in conjunction with embodiments. The description of the following embodiments is only used to help understand the present invention. It should be noted that for ordinary persons in the art, without departing from the principle of the present invention, the present invention can also be modified in some ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0027] Embodiment 1

[0028] A novel method for preparing a monolithic catalyst with a high molecular weight polymer as a carrier suitable for ultra-low temperature SCR reaction comprises the following steps:

[0029] Step 1: Dissolve 61.7 g of manganese nitrate, 15.12 g of iron nitrate and 15.9 g of cerium ammonium nitrate in deionized water, impregnate 60 g of alumina balls with a diameter of 5 mm by equal volume impregnation method, and dry in an oven at 60°C for 15 minutes;

[0030] Step 2: Place the dried alumina balls in a sealed container filled with 0.1% ammonia and 5% water vapor, and heat and fumigate at 80°C for 2 hours;

[0031] Step 3, calcining the dried metal oxide pellets at 500° C. for 3 hours to obtain catalyst pellets;

[0032] Step 4: dispersing the catalyst beads on the surface of the polyetherimide plate;

[0033] Step 5: Heat the polyetherimide plate to 220°C, and fix the catalyst balls in the polymer plate;

[0034] Step 6: Cool down to harden the polyetherimide plates, and assemble the polyetherimide plates to obtain an integral catalyst.

[0035] Embodiment 2

[0036] A novel method for preparing a monolithic catalyst with a high molecular weight polymer as a carrier suitable for ultra-low temperature SCR reaction comprises the following steps:

[0037] Step 1: Take 49.7g of manganese acetate, 20.25g of ferric chloride, and 9.47g of cerium nitrate and dissolve them in deionized water, impregnate 60g of titanium oxide balls with a diameter of 4 mm by equal volume impregnation method, and dry them in an oven at 80°C for 5 minutes;

[0038] Step 2: Place the dried titanium oxide balls in a sealed container filled with 0.5% ammonia and 10% water vapor, and heat and fumigate at 70°C for 3 hours;

[0039] Step 3: calcining the dried metal oxide pellets at 550° C. for 2 hours to obtain catalyst pellets;

[0040] Step 4: dispersing the catalyst beads on the surface of the polyetherimide plate;

[0041] Step 5: Heat the polyetherimide plate to 220°C, and the catalyst pellets are trapped and fixed in the polymer plate;

[0042] Step 6: Cooling down, hardening the polyamide-imide plates, and assembling the polyamide-imide plates to obtain an integral catalyst.

[0043] Embodiment 3

[0044] A novel method for preparing a monolithic catalyst with a high molecular weight polymer as a carrier suitable for ultra-low temperature SCR reaction comprises the following steps:

[0045] Step 1: Dissolve 45.42g of manganese nitrate, 12.76g of ferric chloride and 12.46g of cerium nitrate in deionized water, impregnate 60g of 6mm diameter silica balls by equal volume impregnation method, and dry in a 90°C oven for 5 minutes;

[0046] Step 2: Place the dried silica balls in a sealed container filled with 0.8% ammonia and 12% water vapor, and heat and fumigate at 90°C for 2 hours;

[0047] Step 3: calcining the dried metal oxide pellets at 500° C. for 3 hours to obtain catalyst pellets;

[0048] Step 4: dispersing the catalyst beads on the surface of the polyetherimide plate;

[0049] Step 5: Heat the polyamide plate to 200°C, and the catalyst pellets are trapped and fixed in the polymer plate;

[0050] Step 6: Cooling down, hardening the polyamide plates, and assembling the polyamide plates to obtain an integral catalyst.

[0051] The three groups of monolithic catalysts with high molecular weight polymer as carrier suitable for ultra-low temperature SCR reaction prepared in Examples 1 to 3 were heated at normal pressure and a space velocity of 40000 h -1 , NO concentration 500ppm, NH3 concentration 510ppm, O2 concentration 5vol.%, temperature 120 ~ 200 ℃ conditions for denitration treatment, the conversion efficiency with temperature change relationship as shown in Figure 1 As shown:

[0052] The catalytic effect of the integral catalyst obtained in Example 1 is manifested in that as the reaction temperature increases from 120°C to 200°C, the conversion rate shows an increasing trend, and when the temperature reaches 180°C, the increase in the conversion rate is significantly weakened; when the temperature is 160°C, the conversion rate of the integral catalyst obtained in Example 1 is 86.6%.

[0053] The catalytic effect of the integral catalyst obtained in Example 2 is manifested in that as the reaction temperature increases from 120°C to 200°C, the conversion rate shows an increasing trend, and when the temperature approaches 180°C, the increase in the conversion rate is significantly weakened, and this change trend is similar to that of the integral catalyst obtained in Example 1; when the temperature is 200°C, the catalytic effects of the integral catalysts obtained in Examples 1 and 2 are almost the same; when the temperature is 160°C, the conversion rate of the integral catalyst obtained in Example 2 is 77.3%.

[0054] The catalytic effect of the integral catalyst obtained in Example 3 is manifested in that as the reaction temperature increases from 120°C to 200°C, the conversion rate shows an increasing trend, and when the temperature approaches 180°C, the increase in the conversion rate is significantly weakened. This change trend is similar to that of the integral catalysts obtained in Examples 1 and 2, but the catalytic effect of the integral catalyst obtained in Example 3 is significantly weaker than that of Examples 1 and 2 at all test temperatures, especially when the temperature is 120°C; when the temperature is 160°C, the conversion rate of the integral catalyst obtained in Example 3 is 70.0%.

Claims

1. A method for preparing a monolithic catalyst with a high molecular weight polymer as a carrier suitable for ultra-low temperature SCR reaction, characterized in that: The following steps are involved: S1. Dissolve an iron salt and a manganese salt in deionized water, impregnate the metal oxide pellets by an equal volume impregnation method, and then dry in an oven until the outer surface of the metal oxide pellets is dry; the iron salt is one or more of ferric nitrate, ferric chloride, ferric sulfate and ferric acetate; the manganese salt is one or more of manganese acetate, manganese nitrate, manganese sulfate and manganese chloride; optionally add a cerium salt to the deionized water to dissolve, the cerium salt is one or more of cerium nitrate, ammonium cerium nitrate, cerium sulfate and cerium chloride; the diameter of the metal oxide pellets is 4 to 10 mm; the composition of the metal oxide pellets is one or more of aluminum oxide, silicon dioxide and titanium dioxide; S2, placing the dried metal oxide pellets in a sealed container filled with ammonia and water vapor, and heating and fumigating; the ammonia concentration in the sealed container is 0.001-1%, the water vapor concentration is 1-15%, the fumigation temperature is 50-95°C, and the fumigation time is 1-5 hours; S3, calcining the fumigated metal oxide pellets to obtain catalyst pellets; the amount of Fe source in the catalyst pellets is calculated as Fe2O3, which is 5-20wt.% of the total mass of the catalyst pellets; the amount of Ce source is calculated as CeO2, which is 0-20wt.% of the total mass of the catalyst pellets; the amount of Mn source is calculated as MnO2, which is 20-50wt.% of the total mass of the catalyst pellets; the amount of aluminum oxide is 0-70wt.% of the total mass of the catalyst pellets; the amount of silicon dioxide is 0-70wt.% of the total mass of the catalyst pellets; the amount of titanium dioxide is 0-70wt.% of the total mass of the catalyst pellets; S4, dispersing the catalyst beads on the surface of the polymer plate; the polymer plate is composed of one or more of polyacrylamide, polyvinyl carbazole, polycarbonate, polysulfone, polyphenylene ether sulfone, polyimide, polyamide-imide and polyetherimide; S5, heating the polymer plate to the glass transition temperature, so that the catalyst balls sink into the softened polymer plate surface; S6. Lowering the temperature to harden the polymer plates, and assembling the polymer plates to obtain an integral catalyst.

2. The method for preparing a monolithic catalyst suitable for ultra-low temperature SCR reaction with a high molecular weight polymer as a carrier according to claim 1, characterized in that: In step S4: the average density of the catalyst beads dispersed on the surface of the polymer plate is 0.4-0.8 g / m 2 .

3. The method for preparing a monolithic catalyst suitable for ultra-low temperature SCR reaction with a high molecular weight polymer as a carrier according to claim 1, characterized in that: In step S1: the drying temperature is 60-80° C., and the drying time is 10-60 minutes.

4. The method for preparing a monolithic catalyst suitable for ultra-low temperature SCR reaction with a high molecular weight polymer as a carrier according to claim 1, characterized in that: In step S3: the calcination temperature is 300-600° C., and the calcination time is 1-3 hours.

5. The method for preparing a monolithic catalyst suitable for ultra-low temperature SCR reaction with a high molecular polymer as a carrier according to claim 1, characterized in that: In step S4: the shape of the polymer plate is one or more of a corrugated plate, a honeycomb plate, and a plate with holes.

6. The method for preparing a monolithic catalyst suitable for ultra-low temperature SCR reaction with a high molecular weight polymer as a carrier according to claim 1, characterized in that: In step S4: the high molecular polymer plate is in a plate shape.