Authigenic fiber reinforced single-crystal high-temperature alloy and preparation method thereof

By using the temperature gradient to form the carbide fiber and γ′ in a single crystal high-temperature alloy, the problem of mismatch between the interface between the carbon fiber and the matrix is ​​solved, and the high-temperature mechanical properties of the single crystal high-temperature alloy are improved, and suitable for high-temperature components.

CN118905195APending Publication Date: 2024-11-08INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410989556.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the interface mismatch between carbon fiber and single crystal high-temperature alloy matrix leads to interface reaction and dissolution, reducing the high-temperature mechanical properties of single crystal high-temperature alloy.

Method used

By performing the first directional solidification treatment on the master alloy ingot, a single crystal piece containing carbide is formed, and then a second directional solidification treatment is carried out to form a composite of carbide fibers with γ', and the carbide fibers are used to make the carbide fibers in the heat flow direction using a temperature gradient. Epitaxial directional growth forms a semi-convergent structure to avoid interface mismatch and reaction dissolution.

Benefits of technology

It improves the high-temperature mechanical properties of single crystal high-temperature alloys, including tensile strength and long-lasting life, and is suitable for high-temperature bearing components such as aircraft engines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905195A_ABST
    Figure CN118905195A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of authigenic fiber reinforced single-crystal high-temperature alloy, and relates to the technical field of material preparation, and the preparation method comprises the following steps: carrying out first directional solidification treatment on a master alloy ingot to obtain a single-crystal piece, and the microstructure of the single-crystal piece contains carbide; the carbide is of a face-centered cubic structure; second directional solidification treatment is carried out on the single crystal piece, so that carbide in the single crystal piece forms carbide fibers, and the authigenic fiber reinforced single crystal high-temperature alloy is obtained after cooling; the holding temperature of the second directional solidification treatment is higher than that of the first directional solidification treatment. Wherein the high-temperature mechanical property (temperature bearing capacity) of the single-crystal high-temperature alloy can be improved through composite reinforcement of the carbon fibers and the gamma'phase; the carbide fibers and the high-temperature alloy matrix form a semi-coherent structure, so that the problems that the interface structures of the fibers and the matrix are not matched and the interface reaction is corroded can be effectively avoided, and meanwhile, the strengthening effect of the carbide fibers in the fiber growth direction is kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and in particular relates to a self-generated fiber reinforced single crystal high temperature alloy and a preparation method thereof. Background Art

[0002] With the continuous development of aero-engine and gas turbine technology, the performance requirements for blades are gradually increasing, and single-crystal high-temperature alloy blades have become the first choice for engine hot end components. Single-crystal high-temperature alloys are mainly based on γ phase and strengthened with high volume fraction of γ′ phase to achieve good high-temperature mechanical properties.

[0003] In order to ensure the high temperature mechanical properties of single crystal high temperature alloys, more refractory elements are usually added to the single crystal high temperature alloys. However, as the content of refractory elements gradually increases, the structural stability of the single crystal high temperature alloys decreases. Therefore, the existing technology improves the high temperature mechanical properties of single crystal high temperature alloys by adding carbon fibers.

[0004] Carbon fiber is a high-performance fiber reinforcement phase with the advantages of high specific strength, high specific modulus, high temperature oxidation resistance, excellent ablation resistance and thermal shock resistance, and its mechanical properties can be maintained above 1200°C. Generally, SiC and other filamentary carbon fibers are prefabricated in high-temperature alloys, and then hot pressed or hot isostatic pressed. However, due to the mismatch between the interface structure of carbon fiber and the single crystal high-temperature alloy matrix, the problem of interface reaction dissolution occurs, resulting in a decrease in the high-temperature mechanical properties of the final prepared single crystal high-temperature alloy. Summary of the invention

[0005] Therefore, the present invention provides a self-generated fiber-reinforced single crystal high-temperature alloy and a preparation method thereof, which can solve the technical problem in the prior art that the mechanical properties of the single crystal high-temperature alloy decrease due to the mismatch between the carbon fiber and the matrix interface.

[0006] In order to solve the above problems, the present invention provides a method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy, comprising the following steps:

[0007] Preparing a single crystal part: performing a first directional solidification treatment on a master alloy ingot to obtain a single crystal part, wherein the microstructure of the single crystal part contains carbides; wherein the carbides are a face-centered cubic structure;

[0008] Preparing a single crystal high temperature alloy: performing a second directional solidification treatment on the single crystal piece so that carbides in the single crystal piece form carbide fibers, and obtaining a self-generated fiber-reinforced single crystal high temperature alloy after cooling;

[0009] The holding temperature of the second directional solidification process is higher than the holding temperature of the first directional solidification process, so that the second directional solidification process forms a higher temperature gradient than the first directional solidification process.

[0010] Further, in terms of mass percentage, the chemical composition of the master alloy ingot is as follows:

[0011] C: 0.2-1.2wt%, Cr: 3.0-7.5wt%, Co: 8.0-11.0wt%, Al: 4.5-7.0wt%, W: 9.0-13. 0wt%, Mo: 0.8-2.0wt%, Nb: 1.0-5.0wt%, V: 0.3-1.5wt%, Ta: 3.0-6.0wt%, Ni balance.

[0012] Furthermore, before the step of preparing the single crystal piece, the method further includes: preparing a master alloy ingot;

[0013] Preferably, the step of preparing the master alloy ingot comprises: smelting the alloy raw material, refining after melting, and then casting to obtain the master alloy ingot.

[0014] Furthermore, the smelting is performed by vacuum induction smelting.

[0015] Furthermore, in the step of preparing the single crystal part: the holding temperature of the first directional solidification treatment is 1450-1600° C.; and / or

[0016] The pouring temperature during the first directional solidification treatment is 1450-1600°C; and / or

[0017] The pulling rate of the first directional solidification process is 1-10 mm / min.

[0018] Furthermore, the single crystal piece is in the shape of a plate or a rod; and / or

[0019] The single crystal piece is a

[001] oriented single crystal piece; and / or

[0020] The carbides in the single crystal piece are in a skeleton or block shape.

[0021] Furthermore, in the step of preparing the single crystal high temperature alloy, performing a second directional solidification treatment on the single crystal piece comprises:

[0022] The single crystal piece is processed into a blank, and then the blank is loaded into an Al2O3 ceramic cavity to obtain an alloy ceramic body; the ceramic alloy body is placed in a heating element of a directional solidification furnace, and then the heating element is heated to 1500-1650°C, and after insulation, secondary directional pulling and solidification is performed, and after cooling, the ceramic cavity is removed to obtain the self-generated fiber-reinforced single crystal high-temperature alloy.

[0023] Furthermore, the pulling rate of the second directional solidification process is 0.5-20 μm / min; and / or

[0024] The holding temperature of the second directional solidification treatment is 50-150° C. higher than the holding temperature of the first directional solidification treatment.

[0025] On the other hand, the present invention also provides a self-generated fiber-reinforced single crystal high-temperature alloy, the microstructure of which includes a γ′ phase and carbide fibers; the carbide fibers are in the shape of long strips, the average diameter of the carbide fibers is 0.7-1 μm, the spacing between the carbide fibers is 3-10 μm, and the γ phase and the carbide fibers form a semi-coherent structure.

[0026] Further, the carbide fiber includes at least one of NbC fiber and TaC fiber;

[0027] Preferably, the single crystal high temperature alloy is obtained by any of the preparation methods described above.

[0028] The present invention provides a single crystal high temperature alloy and a preparation method thereof, which has the following beneficial effects:

[0029] 1. The present invention performs a first directional solidification treatment on the master alloy ingot to obtain a single crystal containing block or skeleton carbides, and then performs a second directional solidification treatment on the single crystal. The temperature of the second directional solidification treatment is higher than that of the first directional solidification treatment, that is, the temperature of the second directional solidification treatment forms a temperature gradient with the temperature of the first directional solidification treatment. Under the high temperature gradient, the face-centered cubic structure of niobium carbide or tantalum carbide grows preferentially along the

[001] direction like the matrix, so that the carbides in the single crystal can be epitaxially and directionally grown in situ along the heat flow direction to form carbon fibers, thereby obtaining a single crystal high-temperature alloy with carbon fibers and γ′ phase composite reinforcement; wherein, the composite reinforcement of carbon fibers and γ′ phase can improve the high-temperature mechanical properties (temperature bearing capacity) of the single crystal high-temperature alloy. The face-centered cubic structure of the carbide fiber and the face-centered cubic structure of the high-temperature alloy matrix (γ phase) form a semi-coherent structure, which can effectively avoid the problem of interface structure mismatch and interface reaction dissolution between the fiber and the matrix, while maintaining the strengthening effect of the carbide fiber in the fiber growth direction.

[0030] 2. Furthermore, by forming carbide fibers through an in-situ self-generation method, problems such as interface stability of prefabricated fibers are avoided, and a composite reinforced single crystal high-temperature alloy with stable interface can be obtained; the tensile strength of the above-mentioned single crystal high-temperature alloy at 980°C can reach more than 790MPa; the tensile strength at 1100°C can reach more than 440MPa; the endurance life at 1120°C / 137MPa can reach more than 100h, and it is expected to be applied to high temperature-bearing components such as aircraft engine turbines. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0032] Figure 1 is a microstructure diagram of a single crystal high temperature alloy according to Example 1 of the present invention;

[0033] Figure 2 is a microstructure diagram of a single crystal high temperature alloy according to Example 2 of the present invention;

[0034] Figure 3 is a microstructure diagram of a single crystal high temperature alloy according to Example 3 of the present invention;

[0035] Figure 4 is a microstructure diagram of a single crystal test rod of Comparative Example 1 of the present invention;

[0036] Figure 5 is a microstructure diagram of a single crystal high temperature alloy of Comparative Example 2 of the present invention;

[0037] Figure 6 It is the microstructure diagram of the single crystal high temperature alloy of comparative example 3 of the present invention. DETAILED DESCRIPTION

[0038] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0039] According to an embodiment of the present invention, a method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy is provided, comprising the following steps:

[0040] Preparing a single crystal part: performing a first directional solidification treatment on a master alloy ingot to obtain a single crystal part, wherein the microstructure of the single crystal part contains carbides; wherein the carbides are a face-centered cubic structure;

[0041] Preparation of single crystal high temperature alloy: performing a second directional solidification treatment on the single crystal part so that carbides in the single crystal part form carbide fibers, and obtaining a self-generated fiber-reinforced single crystal high temperature alloy after cooling;

[0042] Among them, the insulation temperature of the second directional solidification treatment is higher than the insulation temperature of the first directional solidification treatment, that is, the temperature of the heat insulation heating element of the mold shell during the second directional solidification treatment is higher than the temperature of the heat insulation heating element of the mold shell during the first directional solidification treatment, so that the temperature difference between the heating zone and the cooling zone during the second directional solidification treatment is greater, that is, the temperature gradient of the second directional solidification treatment is higher than the temperature gradient of the first directional solidification treatment; under high temperature gradient, the carbides of face-centered cubic structure, like the matrix, preferentially <001> direction to form fibers.

[0043] Based on the above method, in the process of preparing single crystal parts, elements such as C and Nb or Ta in the raw materials form carbides; then the single crystal parts are subjected to directional solidification with a high temperature gradient, so that the carbides can form carbon fibers in situ by epitaxial directional growth along the heat flow direction, and a single crystal high-temperature alloy reinforced with carbon fibers and γ′ phase is obtained; wherein, the composite reinforcement of carbon fibers and γ′ phase can improve the high-temperature mechanical properties (temperature bearing capacity) of the single crystal high-temperature alloy. Among them, the semi-coherent structure is formed by using the face-centered cubic structure of the carbide fiber and the face-centered cubic structure of the high-temperature alloy matrix, which can effectively avoid the problem of interface structure mismatch between the fiber and the matrix and interface reaction dissolution, while maintaining the strengthening effect of the carbide fiber in the direction of fiber growth.

[0044] In some embodiments, the chemical composition of the master alloy ingot is as follows, measured by mass percentage:

[0045] C: 0.2-1.2wt%, Cr: 3.0-7.5wt%, Co: 8.0-11.0wt%, Al: 4.5-7.0wt%, W: 9.0-13.0wt%, Mo: 0.8-2.0wt%, Nb: 1.0-5.0wt%, V: 0.3-1.5wt%, Ta: 3.0-6.0wt%, Ni balance. Among them, the elements Nb and Ta can form NbC fibers and TaC fibers respectively with C during the preparation process to enhance the mechanical properties of the single crystal high temperature alloy.

[0046] In some embodiments, before the step of preparing the single crystal piece, the method further includes: preparing a master alloy ingot;

[0047] Preferably, the steps of preparing the master alloy ingot include: smelting the alloy raw materials, refining after melting, and then casting to obtain the master alloy ingot.

[0048] In some embodiments, the smelting is performed by vacuum induction melting.

[0049] In some embodiments, in the step of preparing a single crystal member: the holding temperature of the first directional solidification treatment is 1450-1600° C.; and / or

[0050] The pouring temperature during the first directional solidification treatment is 1450-1600°C; and / or

[0051] The pulling rate of the first directional solidification process is 1-10 mm / min.

[0052] In some embodiments, the single crystal piece is in the shape of a plate or a rod; and / or

[0053] The single crystal piece is a

[001] oriented single crystal piece; and / or

[0054] The carbides in single crystal parts are skeletal or blocky.

[0055] In some embodiments, in the step of preparing a single crystal high temperature alloy, performing a second directional solidification treatment on the single crystal member includes:

[0056] The single crystal part is processed into a blank, and then the blank is loaded into a high-temperature resistant Al2O3 ceramic cavity to obtain an alloy ceramic body; the ceramic alloy body is placed in a heating element of a directional solidification furnace, and then the heating element is heated to 1500-1650°C, and after insulation, a secondary directional pulling solidification is performed, and after cooling, the ceramic cavity is removed to obtain a self-generated fiber reinforced single crystal high-temperature alloy.

[0057] In some embodiments, the pulling rate of the second directional solidification process is 0.5-20 μm / min; and / or

[0058] The insulation temperature of the second directional solidification treatment is 50-150°C higher than that of the first directional solidification treatment. Compared with the first directional solidification treatment, the insulation temperature of the second directional solidification treatment (the temperature of the heating element used for shell insulation) is higher, and the temperature difference between the heating zone and the cooling zone is greater (the overheating temperature of the alloy is higher), that is, the temperature gradient of the second directional solidification treatment is higher. The high temperature gradient of the second directional solidification is conducive to the formation of carbide fibers; during the first directional solidification treatment, only the matrix single crystal structure needs to be formed, and a too high temperature gradient is not required. Among them, during the second directional solidification treatment, if the temperature gradient is too low, carbide fibers cannot be formed, and if the temperature gradient is too high, the qualitative solidification furnace cannot be achieved.

[0059] When the sample is subjected to directional solidification treatment, the heat preservation means that after the heating element is heated to the heat preservation temperature, the drawing begins until the desired sample is obtained by drawing. That is, the heat preservation is completed after the sample is drawn.

[0060] The pulling in the first directional solidification process is recorded as a primary directional pulling.

[0061] On the other hand, the present invention also provides a self-generated fiber-reinforced single crystal high-temperature alloy, the microstructure of the single crystal high-temperature alloy includes a γ′ phase and carbide fibers; the carbide fibers are in the shape of long strips, the average diameter of the carbide fibers is 0.7-1μm, the spacing between the carbide fibers is 3-10μm, and the γ phase and the carbide fibers form a semi-coherent structure.

[0062] In some embodiments, the carbide fiber includes at least one of NbC fiber and TaC fiber;

[0063] Preferably, the single crystal high temperature alloy is obtained by any of the above-mentioned preparation methods.

[0064] The present invention is further described below with reference to specific embodiments and comparative examples.

[0065] Example 1

[0066] This embodiment provides a method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy, comprising the following steps:

[0067] Preparation of a master alloy ingot: mixing the raw materials according to the alloy raw material ratio, and then putting the raw materials except Al into a crucible for vacuum induction melting, the refining temperature is 1550°C, adding Al after refining, and pouring into a master alloy ingot with a diameter of 80 mm after stirring; wherein, the chemical composition of the alloy raw materials is C: 0.6wt%, Cr: 5wt%, Co: 10wt%, Al: 6wt%, W: 10wt%, Mo: 1wt%, Nb: 4wt%, V: 1wt%, Ta: 3.5wt%, and Ni balance, in terms of mass percentage;

[0068] Preparation of single crystal parts: After the surface of the master alloy ingot is polished to remove the oxide scale, it is placed in a crucible, and the single crystal mold shell is added to the heater, and the temperature of the lower zone of the heater is heated to 1550°C to perform the first directional solidification treatment on the master alloy ingot, and then cast into a single crystal test rod with a diameter of 12 mm; wherein the pouring temperature is 1550°C and the pulling rate is 6 mm / min;

[0069] Preparation of single crystal high-temperature alloy: cut the single crystal test rod and then finish it into a blank, put the blank into a ceramic tube with an inner diameter of 12 mm, and then put the ceramic tube with the blank into a high gradient directional solidification furnace for a second directional solidification treatment, heat the heating element to 1600°C, keep it warm for 5 minutes, and then carry out directional pulling solidification at a pulling rate of 0.5μm / min, and then pull it down to the cooling chamber, remove the surface ceramic after cooling to room temperature, and you can get a single crystal high-temperature alloy with in-situ self-generated fibers and γ′ phase composite reinforcement.

[0070] The microstructure of the single crystal high temperature alloy prepared in this embodiment is shown in Figure 1It can be seen that the single crystal high temperature alloy of this embodiment not only forms the γ′ phase, but also forms long strips of carbide fibers, the average diameter of the carbide fibers is 1 μm, and the spacing between the carbide fibers is 10 μm. Its tensile and endurance properties are shown in Tables 1 and 2, where θ is the test temperature, σ b is the tensile strength, σ P0.2 is the yield strength, δ5 is the elongation, ψ / % is the cross-sectional shrinkage, σ is the endurance stress, and τ is the endurance life.

[0071] Table 1 Tensile properties of single crystal high temperature alloy of Example 1 at different temperatures

[0072] θ / ℃ <![CDATA[σ b / MPa]]> <![CDATA[σ P0.2 / MPa]]> <![CDATA[δ5 / %]]> ψ / % 25 917 853 12.3 10.5 980 812 688 25.9 41.2 1050 562 479 36.4 42.7 1100 476 434 30.7 56.2

[0073] Table 2: Durability properties of single crystal high temperature alloy of Example 1

[0074] θ / ℃ σ / MPa t / h 760 810 89.3 1120 137 156.5

[0075] Example 2

[0076] This embodiment provides a method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy, comprising the following steps:

[0077] Preparation of a master alloy ingot: mixing the raw materials according to the alloy raw material ratio, and then putting the raw materials except Al into a crucible for vacuum induction melting, the refining temperature is 1550°C, adding Al after refining, and pouring into a master alloy ingot with a diameter of 80 mm after stirring; wherein, the chemical composition of the alloy raw materials is C: 0.8wt%, Cr: 5wt%, Co: 10wt%, Al: 6wt%, W: 9wt%, Mo: 1wt%, Nb: 4wt%, V: 1wt%, Ta: 3.5wt%, and Ni balance, in terms of mass percentage;

[0078] Preparation of single crystal parts: After the surface of the master alloy ingot is polished to remove the oxide scale, it is placed in a crucible, and the single crystal mold shell is added to the heater, and the temperature of the lower zone of the heater is heated to 1500°C to perform the first directional solidification treatment on the master alloy ingot, and then cast into a single crystal test rod with a diameter of 5 mm; wherein the pouring temperature is 1500°C and the pulling rate is 10 mm / min;

[0079] Preparation of single crystal high-temperature alloy: cut the single crystal test rod and then finish it into a blank, put the blank into a ceramic tube with an inner diameter of 5 mm, and then put the ceramic tube with the blank into a high gradient directional solidification furnace for a second directional solidification treatment, heat the heating element to 1600°C, keep it warm for 5 minutes, and then carry out directional pulling solidification at a pulling rate of 7μm / min, and then pull it down to the cooling chamber, remove the surface ceramic after cooling to room temperature, and you can get a single crystal high-temperature alloy with in-situ self-generated fibers and γ′ phase composite reinforcement.

[0080] The microstructure of the single crystal high temperature alloy prepared in this embodiment is shown in Figure 2 It can be seen that the single crystal high temperature alloy of this embodiment not only forms the γ′ phase, but also forms long strips of carbide fibers, the average diameter of the carbide fibers is 0.95 μm, and the distance between the carbide fibers is 8.9 μm. Its tensile and endurance properties are shown in Tables 3 and 4.

[0081] Table 3 Tensile properties of single crystal high temperature alloy of Example 2 at different alloy temperatures

[0082] θ / ℃ <![CDATA[σ b / MPa]]> <![CDATA[σ P0.2 / MPa]]> <![CDATA[δ5 / %]]> ψ / % 25 896 841 12.6 10.8 980 804 671 21.4 36.3 1100 453 418 29.6 52.8

[0083] Table 4: Durability properties of single crystal high temperature alloy of Example 2

[0084] θ / ℃ σ / MPa t / h 760 810 85.1 1120 137 134.0

[0085] Example 3

[0086] This embodiment provides a method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy, comprising the following steps:

[0087] Preparation of a master alloy ingot: mixing the raw materials according to the alloy raw material ratio, and then putting the raw materials except Al into a crucible for vacuum induction melting, the refining temperature is 1550°C, adding Al after refining, and pouring into a master alloy ingot with a diameter of 80 mm after stirring; wherein, the chemical composition of the alloy raw materials is C: 1wt%, Cr: 3wt%, Co: 8wt%, Al: 4.6wt%, W: 12wt%, Mo: 1wt%, Nb: 2wt%, V: 0.4wt%, Ta: 5.5wt%, and Ni balance, in terms of mass percentage;

[0088] Preparation of single crystal parts: After the surface of the master alloy ingot is polished to remove the oxide scale, it is placed in a crucible, and the single crystal mold shell is added to the heater, and the temperature of the lower zone of the heater is heated to 1450°C to perform the first directional solidification treatment on the master alloy ingot, and then cast into a single crystal test rod with a diameter of 8 mm; wherein the pouring temperature is 1450°C and the pulling rate is 2 mm / min;

[0089] Preparation of single crystal high-temperature alloy: cut the single crystal test rod and then finish it into a blank, put the blank into a ceramic tube with an inner diameter of 8 mm, and then put the ceramic tube with the blank into a high gradient directional solidification furnace for a second directional solidification treatment, heat the heating element to 1500°C, keep it warm for 5 minutes, and then carry out directional pulling solidification at a pulling rate of 2μm / min, and then pull it down to the cooling chamber, remove the surface ceramic after cooling to room temperature, and you can get a single crystal high-temperature alloy with in-situ self-generated fibers and γ′ phase composite reinforcement.

[0090] The microstructure of the single crystal high temperature alloy prepared in this embodiment is shown in Figure 3It can be seen that carbide fibers are formed, the average diameter of the carbide fibers is 0.85 μm, and the spacing between the carbide fibers is 4.5 μm. The tensile and endurance properties are shown in Tables 5 and 6.

[0091] Table 5 Tensile properties of single crystal high temperature alloy of Example 3 at different temperatures

[0092] θ / ℃ <![CDATA[σ b / MPa]]> <![CDATA[σ P0.2 / MPa]]> <![CDATA[δ5 / %]]> ψ / % 25 879 826 11.4 10.2 980 795 659 19.6 32.6 1100 445 403 28.1 43.2

[0093] Table 6 Stress resistance of single crystal high temperature alloy of Example 3

[0094] θ / ℃ σ / MPa t / h 760 810 76.1 1120 137 103.2

[0095] Comparative Example 1

[0096] This comparative example provides a method for preparing a single crystal test rod, comprising the following steps:

[0097] Preparation of a master alloy ingot: mixing the raw materials according to the alloy raw material ratio, placing the raw materials except Al into a crucible for vacuum induction melting, adding Al after refining, and casting into a master alloy ingot with a diameter of 80 mm after stirring; wherein, the chemical composition of the alloy raw materials is C: 0.6wt%, Cr: 5wt%, Co: 10wt%, Al: 6wt%, W: 10wt%, Mo: 1wt%, Nb: 4wt%, V: 1wt%, Ta: 3.5wt%, and Ni balance, in terms of mass percentage;

[0098] Preparation of single crystal parts: After the surface of the mother alloy ingot is polished to remove the oxide scale, it is placed in a crucible and the single crystal mold shell is added to the heater. The temperature of the lower zone of the heater is heated to 1550°C to remelt the mother alloy ingot, and then cast into a single crystal test rod with a diameter of 16 mm; wherein the pouring temperature is 1550°C and the pulling rate is 5 mm / min.

[0099] The microstructure of the single crystal test rod prepared in this comparative example is shown in Figure 4 It can be seen that a γ′ strengthening phase is formed in the single crystal test rod of this comparative example. However, since the single crystal test rod is not subjected to the second directional solidification treatment, the skeleton-like carbide cannot be oriented into a fibrous state. The existence of the skeleton-like carbide interface causes the alloy to have many lateral interfaces when loaded along the matrix growth direction. These areas become weak areas, making it difficult for the alloy to fully exert its performance.

[0100] Comparative Example 2

[0101] This comparative example provides a method for preparing a high-temperature alloy, comprising the following steps:

[0102] Preparation of a master alloy ingot: mixing the raw materials according to the alloy raw material ratio, placing the raw materials except Al into a crucible for vacuum induction melting, adding Al after refining, and casting into a master alloy ingot with a diameter of 80 mm after stirring; wherein, the chemical composition of the alloy raw materials is C: 0.6wt%, Cr: 5wt%, Co: 10wt%, Al: 6wt%, W: 10wt%, Mo: 1wt%, Nb: 4wt%, V: 1wt%, Ta: 3.5wt%, and Ni balance, in terms of mass percentage;

[0103] Preparation of master alloy test bars: After surface grinding and removing oxide scale from the master alloy ingot, the ingot was processed into a test bar with a diameter of 12 mm;

[0104] Preparation of high-temperature alloy: The above-mentioned test rod is placed in a ceramic tube with an inner diameter of 12 mm, and then the ceramic tube containing the master alloy test rod is placed in a high-gradient directional solidification furnace for directional solidification treatment, the heating element is heated to 1600°C, and after keeping warm for 5 minutes, directional pulling solidification is carried out at a pulling rate of 0.5 μm / min, and then pulled down to the cooling chamber, and after cooling to room temperature, the surface ceramic is removed to obtain a high-temperature alloy.

[0105] The tensile and rupture properties of the high temperature alloy prepared in this comparative example are shown in Table 7 and Table 8. Figure 5 As shown. It can be seen that compared with Example 1, the tensile properties and rupture properties of this comparative example are significantly reduced, and more directional grain boundaries (i.e., directional columnar crystal structures) are formed in the high-temperature alloy. This is because the comparative example directly uses the master alloy test rod for directional solidification treatment, and these directional columnar crystal structures in the alloy will have a certain angle with the loading direction, thereby reducing the performance of the high-temperature alloy. .

[0106] Table 7 Tensile properties of the high temperature alloy of Comparative Example 2 at 980°C

[0107] θ / ℃ <![CDATA[σ b / MPa]]> <![CDATA[σ P0.2 / MPa]]> <![CDATA[δ5 / %]]> ψ / % 980 590 535 25.1 38.5

[0108] Table 8 Durability properties of high temperature alloy of comparative example 2

[0109] θ / ℃ σ / MPa t / h 1120 137 7.8

[0110] Comparative Example 3

[0111] This comparative example provides a method for preparing a single crystal high temperature alloy, comprising the following steps:

[0112] Preparation of a master alloy ingot: mixing the raw materials according to the alloy raw material ratio, placing the raw materials except Al into a crucible for vacuum induction melting, adding Al after refining, and casting into a master alloy ingot with a diameter of 80 mm after stirring; wherein, the chemical composition of the alloy raw materials is C: 0.6wt%, Cr: 5wt%, Co: 10wt%, Al: 6wt%, W: 10wt%, Mo: 1wt%, Nb: 4wt%, V: 1wt%, Ta: 3.5wt%, and Ni balance, in terms of mass percentage;

[0113] Preparation of single crystal parts: After the surface of the master alloy ingot is polished to remove the oxide scale, it is placed in a crucible, and the single crystal mold shell is raised to the heater, and the temperature of the lower zone of the heater is heated to 1550°C to perform the first directional solidification treatment on the master alloy ingot, and then cast into a single crystal test rod with a diameter of 12 mm; wherein the pouring temperature is 1550°C and the pulling rate is 6 mm / min;

[0114] Preparation of single crystal high-temperature alloy: cut the single crystal test rod and then finish it into a blank, put the blank into a ceramic tube with an inner diameter of 12 mm, and then put the ceramic tube with the blank into a high gradient directional solidification furnace for a second directional solidification treatment, heat the heating element to 1600°C, keep it warm for 5 minutes, and then carry out directional pulling solidification at a pulling rate of 25μm / min, and then pull it down to the cooling chamber, remove the surface ceramic after cooling to room temperature, and you can get a single crystal high-temperature alloy with in-situ self-generated fibers and γ′ phase composite reinforcement.

[0115] The microstructure of the single crystal high temperature alloy prepared in this comparative example is shown in Figure 6 It can be seen that the γ′ phase is formed in the single crystal high temperature alloy of this comparative example, but no fibers are formed, but carbides are distributed discontinuously. The tensile and rupture properties of the single crystal high temperature alloy prepared in this comparative example are shown in Tables 9 and 10. Compared with Example 1, the tensile properties and rupture properties of the single crystal high temperature alloy of this comparative example are significantly reduced. This is because the pulling rate during the second directional solidification treatment is relatively high, resulting in the discontinuous distribution of carbides in the form of dots, making it difficult to form a strengthening effect, and the existence of directional grain boundaries affects the performance of the high temperature alloy.

[0116] Table 9 Tensile properties of single crystal high temperature alloy of comparative example 3 at 980°C

[0117] θ / ℃ <![CDATA[σ b / MPa]]> <![CDATA[σ P0.2 / MPa]]> <![CDATA[δ5 / %]]> ψ / % 980 575 495 27.0 39.5

[0118] Table 10 Durability of single crystal high temperature alloy of comparative example 3

[0119] θ / ℃ σ / MPa t / h 1120 137 6.5

[0120] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.

[0121] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy, characterized in that: The following steps are involved: Preparing a single crystal part: performing a first directional solidification treatment on a master alloy ingot to obtain a single crystal part, wherein the microstructure of the single crystal part contains carbides; wherein the carbides are a face-centered cubic structure; Preparing a single crystal high temperature alloy: performing a second directional solidification treatment on the single crystal piece so that carbides in the single crystal piece form carbide fibers, and obtaining a self-generated fiber-reinforced single crystal high temperature alloy after cooling; Wherein, the insulation temperature of the second directional solidification treatment is higher than the insulation temperature of the first directional solidification treatment.

2. The method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy according to claim 1, characterized in that: According to mass percentage, the chemical composition of the master alloy ingot is as follows: C: 0.2-1.2wt%, Cr: 3.0-7.5wt%, Co: 8.0-11.0wt%, Al: 4.5-7.0wt%, W: 9.0-13. 0wt%, Mo: 0.8-2.0wt%, Nb: 1.0-5.0wt%, V: 0.3-1.5wt%, Ta: 3.0-6.0wt%, Ni balance.

3. The method for preparing the self-generated fiber-reinforced single crystal high-temperature alloy according to claim 2, characterized in that: Before the step of preparing the single crystal piece, the method further includes: preparing a master alloy ingot; Preferably, the step of preparing the master alloy ingot comprises: smelting the alloy raw material, refining after melting, and then casting to obtain the master alloy ingot.

4. The method for preparing the self-generated fiber-reinforced single crystal high-temperature alloy according to claim 3, characterized in that: The smelting is carried out by vacuum induction smelting.

5. The method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy according to claim 1, characterized in that: In the step of preparing the single crystal piece: the holding temperature of the first directional solidification treatment is 1450-1600° C.; and / or The pouring temperature during the first directional solidification treatment is 1450-1600°C; and / or The pulling rate of the first directional solidification process is 1-10 mm / min.

6. The method for preparing the self-generated fiber-reinforced single crystal high-temperature alloy according to claim 5, characterized in that: The single crystal piece is in the shape of a plate or a rod; The single crystal piece is a single crystal piece with a [001] orientation; The carbides in the single crystal piece are in a skeleton or block shape.

7. The method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy according to claim 1, characterized in that: In the step of preparing the single crystal high temperature alloy, performing a second directional solidification treatment on the single crystal piece comprises: The single crystal piece is processed into a blank, and then the blank is loaded into an Al2O3 ceramic cavity to obtain an alloy ceramic body; the ceramic alloy body is placed in a heating element of a directional solidification furnace, and then the heating element is heated to 1500-1650°C, and after insulation, secondary directional pulling and solidification is performed, and after cooling, the ceramic cavity is removed to obtain the self-generated fiber-reinforced single crystal high-temperature alloy.

8. The method for preparing a self-generated fiber-reinforced single crystal high-temperature alloy according to claim 1, characterized in that: The pulling rate of the second directional solidification process is 0.5-20 μm / min; and / or The holding temperature of the second directional solidification treatment is 50-150° C. higher than the holding temperature of the first directional solidification treatment.

9. A self-grown fiber reinforced single crystal high temperature alloy, characterized in that: The microstructure of the self-generated fiber-reinforced single crystal high-temperature alloy includes γ phase, γ′ phase and carbide fibers; the carbide fibers are in the shape of long strips, the average diameter of the carbide fibers is 0.7-1 μm, the spacing between the carbide fibers is 3-10 μm, and the γ phase and the carbide fibers form a semi-coherent structure.

10. The self-grown fiber reinforced single crystal high temperature alloy according to claim 9, characterized in that: The carbide fiber includes at least one of NbC fiber and TaC fiber; Preferably, the self-generated fiber-reinforced single crystal high-temperature alloy is obtained by the preparation method according to any one of claims 1-8.