Flexible riser outermost tensile armor layer defect preparation method
By preparing the defects of the tensile armor layer on the flexible riser, the corrosion and fracture of the tensile armor layer in the offshore flexible riser is solved, and a method of simulated defects is provided, which supports the verification of non-destructive testing, ensuring the flexible riser safety and mechanical properties.
Patent Information
- Application Number
- CN202410969956.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
During the operation and maintenance of the offshore flexible riser, corrosion and fatigue fracture of the tensile armor layer due to the penetration of oil and gas medium, lacking effective defect preparation methods, which affects its mechanical properties and safety.
By intercepting the flexible riser, fixing both ends, cutting the outer protective layer, processing defects of the outermost tensile armor layer (such as holes, grooves, and fracture defects), and restoring the outer protective layer, simulating corrosion and fracture defects.
It provides the ability to prepare samples containing defects in the flexible riser section, solves the problem of prefabricated defects of the outermost tensile armor layer, simulates the corrosion and fracture of the armor layer, and supports the verification of the non-destructive detection method.
Smart Images

Figure CN118905563A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of flexible riser defect preparation, and in particular to a method for preparing defects in the outermost tensile armor layer of a flexible riser. Background Art
[0002] During the operation and maintenance of offshore flexible risers, the oil and gas medium will penetrate into the annulus of the flexible riser to form a corrosive environment, which will cause corrosion of the tensile armor layer; and the movement of the flexible riser between the layers in the internal structure of the flexible riser will cause friction and fatigue stress in the tensile armor layer, which will cause the metal armor layer (the outermost tensile armor layer) to be prone to corrosion thinning, fatigue fracture and other problems. These problems destroy the integrity of the flexible riser and reduce its mechanical properties, which may cause the flexible riser to be damaged or fractured and fail, causing major production accidents, thus seriously damaging the environment and endangering personal and property safety. Therefore, in order to prevent accidents, it is necessary to find defects in the metal armor layer through non-destructive testing methods so that flexible riser repair measures can be taken in time. However, in order to verify the effectiveness of the non-destructive testing method, it is necessary to prepare a flexible riser with defects such as corrosion and fracture in the armor layer. At present, there is still a lack of effective defect preparation methods for offshore flexible risers. Summary of the invention
[0003] In view of this, the present invention aims to propose a method for preparing defects in the outermost tensile armor layer of a flexible riser. Through this method, the defects in the outermost tensile armor layer can be prepared in the existing flexible riser section, which can solve the current problem of lack of prefabricated defects in the outermost tensile armor layer of the flexible riser.
[0004] To achieve the above object, the technical solution of the present invention is implemented as follows: a method for preparing defects in the outermost tensile armor layer of a flexible riser, comprising the following steps:
[0005] Step 1, cutting a flexible riser of a preset length as an experimental steel pipe matrix;
[0006] Step 2, fixing both ends of the flexible riser;
[0007] Step 3, cutting the outer protective layer of the flexible riser;
[0008] Step 4, machining defects on the outermost tensile armor layer;
[0009] Step 5, restore the outer protective layer of the flexible riser.
[0010] Furthermore, step 2 specifically includes fixing or welding the metal layers at two end surfaces of the flexible riser together using a flexible riser clamping device or a welding method.
[0011] Furthermore, step 3 includes, first, cutting along the outer protective layer of the flexible riser and not exceeding the thickness of the outer protective layer to cut into a closed shape; then, removing the cut outer protective layer to expose the outermost tensile armor layer; if the outer protective layer in the cut area cannot be removed, soften the outer protective layer by local heating and then remove it.
[0012] Further, in step 4, when processing defects on the outermost tensile armor layer, one or more flat steel processing defects of the outermost tensile armor layer are selected, and the defects include hole defects, groove defects and fracture defects;
[0013] The hole defects are selected with different diameters and arranged at the same spacing; the groove defects are selected with different lengths, widths and depths and arranged at the same spacing; the fracture defects are selected and set at different fracture positions of the outermost tensile armor layer flat steel.
[0014] Furthermore, step 5 includes, first, putting the outer protective layer removed in step 3 back to its original position; then, heating the outer protective layer at the notch to fuse the removed outer protective layer and the outer protective layer of the flexible riser together; finally, polishing the connection position of the outer protective layer to make it smooth.
[0015] Furthermore, step 5 includes, first, putting the outer protective layer removed in step 3 back in place; then, heating a glue stick made of the same material as the outer protective layer to melt the heated end of the glue stick, and dripping glue drops into the gap to fuse the removed outer protective layer and the outer protective layer of the flexible riser together; finally, polishing the connection position of the outer protective layer to make it smooth.
[0016] Compared with the prior art, the method for preparing defects in the outermost tensile armor layer of a flexible riser described in the present invention has the following advantages: the present invention is a preparation method that can provide a sample pipe containing defects for a flexible riser, and can realize the preparation of defects in the outermost tensile armor layer in the existing flexible riser pipe section, solving the current problem of lack of prefabricated defects in the outermost tensile armor layer of the flexible riser; the prepared defects can simulate the corrosion and fracture of the outermost tensile armor layer of the flexible riser. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0018] Figure 1 It is a flow chart of the method for preparing defects of the outermost tensile armor layer of the flexible riser;
[0019] Figure 2 This is a schematic diagram of cutting the outer protective layer of the flexible riser;
[0020] Figure 3 Schematic diagram of processing defects on the outermost tensile armor layer.
[0021] Description of reference numerals:
[0022] 1. Flexible riser; 2. Outermost tensile armor layer; 3. Groove defect; 4. Fracture defect; 5. Hole defect. DETAILED DESCRIPTION
[0023] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0024] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.
[0025] like Figure 1 As shown, the present invention is a method for preparing defects in the outermost tensile armor layer of a flexible riser, comprising the following steps:
[0026] Step 1, cutting a flexible riser 1 of a preset length as an experimental steel pipe substrate;
[0027] Step 2, fixing the two ends of the flexible riser 1; specifically, using a flexible riser clamping device (or a pipeline fixing clamping device) or a welding method to fix or weld the metal layers at the two end faces of the flexible riser 1 together, so as to prevent the armor layer from spreading and causing the pipeline structure to be damaged during the cutting process of the outer protective layer of the flexible riser 1.
[0028] Step 3, cutting the outer protective layer of the flexible riser 1;
[0029] First, cut along the outer protective layer of the flexible riser 1 without exceeding the thickness of the outer protective layer to form a closed shape; then, remove the cut outer protective layer to expose the outermost tensile armor layer 2 so that defects can be better processed on the outermost tensile armor layer 2; if the outer protective layer in the cut area cannot be removed, soften the outer protective layer by local heating and then remove it.
[0030] Step 4, processing defects on the outermost tensile armor layer 2; specifically, when processing defects on the outermost tensile armor layer 2, one or more flat steel processing defects of the outermost tensile armor layer 2 are selected, and the defects include hole defects 5, groove defects 3 and fracture defects 4; the hole defects 5 are selected with different diameters and arranged at the same spacing. The hole defects 5 of various diameters are set, which can be better used for subsequent verification of the detection accuracy of non-destructive testing means; the groove defects 3 are selected with different lengths, widths and depths, respectively, and arranged at the same spacing. The groove defects 3 of various sizes are set, which can be better used for subsequent verification of the detection accuracy of non-destructive testing means; in order to prevent the fracture defect 4 from affecting the hole defect 5 or the groove defect 3 during the subsequent non-destructive testing test, the fracture defect 4 is selected to be set at different fracture positions of the flat steel of the outermost tensile armor layer 2, that is, the flat steel with the fracture defect 4 is not the same flat steel as the flat steel with the hole defect 5 or the flat steel with the groove defect 3.
[0031] Step 5, restoring the outer protective layer of the flexible riser 1.
[0032] First, put the outer protective layer removed in step 3 back in place;
[0033] Then, the removed outer protective layer is fused with the outer protective layer of the flexible riser 1. Specifically, there are two ways: one is to heat the outer protective layer at the notch to fuse the removed outer protective layer with the outer protective layer of the flexible riser 1; the other is to heat a glue stick made of the same material as the outer protective layer to melt the heated end of the glue stick, and drip glue drops into the notch to fuse the removed outer protective layer with the outer protective layer of the flexible riser 1;
[0034] Finally, polish the connection position of the outer protective layer to make it smooth.
[0035] The method of the present invention solves the problem that the outermost tensile armor layer of the flexible riser is difficult to prefabricate due to the lack of defects. The outermost tensile armor layer defects of the flexible riser produced by the present invention can effectively simulate the corrosion and fracture defects of the armor layer.
[0036] Example 1
[0037] A method for preparing defects in the outermost tensile armor layer of a flexible riser comprises the following steps:
[0038] Step 1, cutting a 2-meter-long flexible riser 1 as an experimental steel pipe substrate, and the cross-sectional size of the outermost tensile armor layer 2 is 5mm×10mm;
[0039] Step 2, using a pipe fixing clamping device to fix both ends of the flexible riser 1;
[0040] Step 3, cutting a 1 meter × 0.5 meter outer protective layer of the flexible riser 1 along the axial direction of the flexible riser 1, and removing the outer protective layer to see the outermost tensile armor layer 2;
[0041] Step 4, select a flat steel of the outermost tensile armor layer 2, and drill hole defects 5 of 1mm, 2mm, 3mm, and 4mm respectively; select another flat steel of the outermost tensile armor layer 2, and cut groove defects 3 of 1mm×1mm×1mm, 1mm×2mm×1mm, 1mm×3mm×1mm, 1mm×4mm×1mm or 1mm×1mm×1mm, 2mm×1mm×1mm, 3mm×1mm×1mm, 4mm×1mm×1mm or 1mm×3mm×1mm, 1mm×3mm×2mm, 1mm×3mm×3mm, 1mm×3mm×4mm respectively; select another flat steel of the outermost tensile armor layer and cut it off to form a fracture defect 4;
[0042] Step 5. Put the removed outer protective layer back in place, use a hot air blower to heat the cut to fuse the cuts together, and grind the cut connections smooth after cooling.
[0043] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing defects in the outermost tensile armor layer of a flexible riser, characterized in that: The following steps are involved: Step 1, cutting a flexible riser (1) of a preset length as a test steel pipe substrate; Step 2, fixing both ends of the flexible riser (1); Step 3, cutting the outer protective layer of the flexible riser (1); Step 4, machining defects on the outermost tensile armor layer (2); Step 5, restoring the outer protective layer of the flexible riser (1).
2. The method for preparing defects in the outermost tensile armor layer of a flexible riser according to claim 1, characterized in that: Step 2 specifically includes using a flexible riser clamping device or a welding method to fix or weld the metal layers at the two end surfaces of the flexible riser (1) together.
3. The method for preparing defects in the outermost tensile armor layer of a flexible riser according to claim 1, characterized in that: Step 3 includes, first, cutting along the outer protective layer of the flexible riser (1) without exceeding the thickness of the outer protective layer, cutting into a closed shape; then, removing the cut outer protective layer to expose the outermost tensile armor layer (2); if the outer protective layer in the cut area cannot be removed, soften the outer protective layer by local heating and then remove it.
4. The method for preparing defects in the outermost tensile armor layer of a flexible riser according to claim 3, characterized in that: In step 4, when processing defects on the outermost tensile armor layer (2), one or more flat steel processing defects of the outermost tensile armor layer (2) are selected, and the defects include hole defects (5), groove defects (3) and fracture defects (4); The hole defects (5) are selected with different diameters and arranged at the same spacing; the groove defects (3) are selected with different lengths, widths and depths and arranged at the same spacing; the fracture defects (4) are selected to be arranged at different fracture positions of the flat steel of the outermost tensile armor layer (2).
5. The method for preparing defects in the outermost tensile armor layer of a flexible riser according to claim 3, characterized in that: Step 5 includes, first, putting the outer protective layer removed in step 3 back to its original position; then, heating the outer protective layer at the notch to fuse the removed outer protective layer and the outer protective layer of the flexible riser (1); and finally, polishing the connection position of the outer protective layer to make it smooth.
6. The method for preparing defects in the outermost tensile armor layer of a flexible riser according to claim 3, characterized in that: Step 5 includes, first, putting the outer protective layer removed in step 3 back to its original position; then, heating a glue stick made of the same material as the outer protective layer to melt the heated end of the glue stick, dripping glue drops into the gap to fuse the removed outer protective layer and the outer protective layer of the flexible riser (1); finally, polishing the connection position of the outer protective layer to make it smooth.
Citation Information
Patent Citations
Manufacturing method of air gap defect intermediate head of cross-linked polyethylene cable
CN104332939A
Test method and device for simulating interlayer wearing of flexible standpipe armors
CN106855482A
Lead seal defect eddy current detection simulation testing block and preparation method and application thereof
CN110231398A
Armored optical cable stripping device and armored optical cable stripping method
CN111487721A
Method for manufacturing defect simulation test block for polyethylene pipe hot-melt welded joint
CN113125229A