Microwave back reduction processing system and method for hard and brittle semiconductor wafer
Through high frequency and low power microwave alternating electromagnetic energy, grinding fluid and metal bonding agent diamond grinding wheel that does not absorb microwaves, the wear and thermal cracks in hard and brittle semiconductor wafer processing is solved, and high-efficiency and low-temperature plastic domain grinding is achieved The process accuracy and efficiency are improved.
Patent Information
- Application Number
- CN202411153293.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The prior art is difficult to efficiently and at low cost for hard and brittle semiconductor wafers, especially while maintaining high quality and accuracy, traditional mechanical grinding and laser-assisted processing have problems of wear, thermal cracks and precise control difficulties.
Using high frequency and low power microwave alternating electromagnetic energy directly acts on hard and brittle semiconductor materials, improves plasticity by inducing internal atomic collision and friction, and uses grinding fluid and metal bonding agent diamond grinding wheel that does not absorb microwaves to achieve low-temperature plastic domain grinding Sharpen, avoid heat damage and precise control.
It realizes high efficiency, high quality, low-temperature plastic domain grinding processing of hard and brittle semiconductor wafers, extends the life of the grinding wheel, improves processing accuracy and efficiency, and reduces the risk of thermal damage.
Smart Images

Figure CN118905775A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ultra-precision machining, and in particular to a microwave high-efficiency ultra-precision plastic domain back-reduction machining system and method for hard and brittle semiconductor wafers. Background Art
[0002] The demand for high-performance semiconductor power devices in the modern industrial field is increasing. Single-crystal silicon carbide (SiC) and gallium nitride (GaN) are typical representatives of the third-generation wide bandgap semiconductor materials. They have excellent physical properties such as high breakdown electric field, high saturated electron velocity, high thermal conductivity and strong radiation resistance, which can meet the needs of modern industry for high-power, high-voltage and high-frequency semiconductor devices. Therefore, they are widely used in modern industrial fields such as aerospace, new energy vehicles, photovoltaic power generation, rail transportation, smart grids, etc., and have a far-reaching impact on the development of "new infrastructure" in various fields in my country.
[0003] Wafer back reduction processing is a crucial link in the manufacture of chips for high-performance semiconductor power devices. On the one hand, the back reduction process can reduce the overall thickness of the chip, which is beneficial to the heat dissipation and integration of the device; on the other hand, it can reduce the thickness of the damaged layer on the wafer surface and the surface roughness, release the residual internal stress of the previous processing step, and reduce the degree of collapse of a single chip during the subsequent dicing process. However, highly hard and brittle SiC and GaN crystals are typical difficult-to-process materials, which leads to rapid wear and failure of ultra-fine diamond abrasive grinding wheels during the single mechanical removal of materials and forming process. It is difficult to achieve high-efficiency and low-cost back reduction processing of high-quality SiC and GaN wafers, and cannot meet the needs of the high-end application market.
[0004] Therefore, in the research and development of back-reduction processing technology for hard and brittle semiconductor wafers, various external energy fields have been used to assist processing to improve the plastic removal of materials and reduce wafer surface damage and surface roughness. For example, patent CN117381568A proposes a processing device and method for wafer laser modification and synchronous thinning. The laser processing system etches and modifies the wafer surface according to the outer edge profile and rotation speed of the grinding wheel, which improves the thinning efficiency and reduces the processing surface roughness, grinding damage, and sub-surface damage depth. This patent mainly uses the high-power and rapid heating effect of the laser to heat the material. As the temperature increases sharply, the material softens, the plastic deformation ability is improved, and plastic domain processing is performed to obtain improved processing quality. However, softened materials are also more likely to clog the grinding wheel, which in turn deteriorates the grinding process and reduces the service life of the grinding wheel. At the same time, the laser is sensitive to the surrounding transmission medium, and the grinding fluid will cause the laser to refract and scatter, and then it is impossible to achieve precise heating and modification of a specific area. During dry grinding, the extremely high temperature in the grinding area will accelerate the thermal damage and wear failure of the abrasive tool, and high-quality and efficient processing cannot be achieved. In addition, during laser heating, the heat is always "from the outside to the inside", and the material will inevitably have a temperature gradient, resulting in thermal cracks. In view of this, patent CN207282468U proposes a plasma thinning device, which realizes damage-free processing through chemical reactions between the strongly oxidizing free radicals in the plasma and the atoms on the surface of the workpiece. Based on its unique processing method, the workpiece will not have crystal defects caused by plastic deformation or brittle fracture, and the original physical properties of the workpiece are maintained, but the surface modification layer formed is very thin, only a few nanometers, so the processing efficiency is extremely low (atomic scale removal rate). Patent CN110625205A proposes a wafer thinning process and device based on the principle of EDM. The wafer is used as the electrode material, and the material is removed by the energy generated by the discharge. It is not limited by the hardness of the material, which solves the problem of traditional mechanical grinding of superhard materials. EDM is a non-contact type of processing, which does not generate contact force or residual stress, and no environmental pollutants are generated during the entire process. However, the discharge erosion position of EDM is not easy to control accurately, and wafer cracking is prone to occur.
[0005] At present, there are four commonly used auxiliary heating cutting methods for hard and brittle materials: plasma arc, oxyacetylene, laser and microwave. Plasma arc, oxyacetylene and laser use the Boltzmann thermal effect to quickly heat the processed materials "from the outside to the inside", which inevitably leads to the existence of temperature gradients in the materials. Hard and brittle materials are very sensitive to heat, so thermal cracks are very likely to occur, reducing the processing quality. Traditional microwave-assisted heating cutting uses the microwave dielectric heating effect to "heat the inside and outside of the processed materials at the same time" through an ultra-high power microwave generator, which greatly shortens the heating time and has high heating efficiency. The ceramic block material can be quickly heated to 1000℃ or even higher to soften the material. However, the thickness of semiconductor wafers is usually only 300 to 500 microns. Excessive heating temperature (over 500℃) will cause the wafer to deform and serious thermal stress inside, resulting in the size accuracy of the processed wafer failing to meet the requirements. At the same time, natural cracking is very likely to occur, reducing the qualified rate of finished products. At the same time, it is still difficult to achieve precise control of the heating energy and heating area at this stage, and excessively high temperatures will cause carbonization and graphitization of diamond abrasives, significantly reducing their strength and shortening the service life of the grinding wheel.
[0006] In addition, unlike the microwave dielectric heating effect, patent CN117532089A proposes a method and equipment for microwave-assisted processing of hard and brittle insulating materials, which uses microwave energy to induce a strong electric field at the processing end of the processing tool to form a discharge. Subsequently, the electrolyte at the discharge position is affected by the high temperature of the discharge to form a corrosive electrolyte to chemically etch the workpiece. However, this patent is essentially a method of micro-processing the surface of insulating ceramic materials based on the principle of electrochemical processing (i.e., using the corrosiveness of the electrolyte), such as micropores, fine grooves, and microstructures, and cannot achieve rapid prototyping of large-scale, high-quality surfaces. In particular, this patent is only suitable for micro-processing of insulating ceramic materials. When the workpiece to be processed has conductor or semiconductor characteristics, the strong electric field generated by the microwave at the processing end will directly discharge and erode the conductive workpiece material (the principle of electrical discharge machining), resulting in the inability to achieve precise control of the entire process and micro-processing of the workpiece surface, and wafer cracking is prone to occur when processing large-size semiconductor wafers. Summary of the invention
[0007] In view of the prominent contradiction between the processing efficiency and processing quality of hard and brittle semiconductor wafers that are difficult to process, the purpose of the present invention is to provide a microwave high-efficiency ultra-precision plastic domain back-reduction processing system and method for hard and brittle semiconductor wafers. The system includes a microwave module and a grinding module. Unlike the existing microwave-assisted processing that uses high-frequency, high-power microwaves to ultra-high temperature heating (1000°C) of materials to improve plasticity, this system mainly uses high-frequency, low-power microwave alternating electromagnetic energy to directly act on hard and brittle semiconductor materials. The high-frequency alternating electromagnetic energy induces violent collisions and frictions between internal atoms, thereby generating dislocations. The microwave-reflecting diamond grinding wheel can be used to prevent the tool material from being directly heated by microwaves, thereby maintaining the high bonding strength and dimensional accuracy of the grinding wheel. Finally, the "low-temperature (workpiece temperature below 200°C)" plastic domain grinding of hard and brittle semiconductor wafers can be achieved.
[0008] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0009] In the first aspect, the present invention discloses a microwave back-reduction processing system for hard and brittle semiconductor wafers, comprising a CNC grinder and a microwave irradiation unit, the CNC grinder is equipped with a first air-floating spindle and a second air-floating spindle, wherein the first air-floating spindle is installed on a Z-axis moving platform, and the first air-floating spindle is driven by a linear motor to realize feeding, and the first air-floating spindle is connected to the grinding wheel processing unit through a grinding wheel clamp to realize the self-rotation movement of the grinding wheel processing unit; the second air-floating spindle is connected to a workbench, and the workbench is used to place the hard and brittle semiconductor wafer to be processed to realize the follow-rotation movement of the hard and brittle semiconductor wafer to be processed, and the microwave irradiation unit is arranged above the hard and brittle semiconductor wafer to be processed, and uses microwave electromagnetic energy to promote the activity of atoms inside the hard and brittle semiconductor wafer material to be processed to produce slip to improve plasticity.
[0010] When microwave back-reduction processing is performed, the microwave irradiation head of the microwave generating assembly of the microwave irradiation unit is connected to the microwave generator through an antenna; when microwave-grinding side-axis back-reduction processing is performed, the microwave irradiation head and the liquid spray device are located on one side of the vacuum self-rotating grinding table, the back-reduction grinding wheel processing unit is fixed to the Z-axis movable platform, and the liquid spray device is used to provide grinding fluid;
[0011] When microwave-grinding coaxial back-reduction processing is performed, the liquid spray device is located on one side of the workbench, and the microwave irradiation head of the microwave irradiation unit is installed at the center of the diamond grinding wheel to process the hard and brittle semiconductor wafer coaxially with the diamond grinding wheel.
[0012] The working principle of this system is based on the microwave dielectric thermal effect. High-frequency, low-power microwaves directly irradiate the surface of hard and brittle semiconductor materials. The high-frequency alternating electromagnetic energy induces collision and friction between atoms inside the crystal material, resulting in dislocation proliferation and slip, and then improving the plasticity of the material. The output low-power alternating electromagnetic energy can avoid the generation of a large amount of heat inside the material. At the same time, the grinding fluid that does not absorb microwaves is used to cool and lubricate the abrasive-workpiece contact interface, reducing the thermal damage and wear of the grinding wheel caused by heat conduction. The metal bond diamond grinding wheel that does not absorb microwaves is used to avoid direct heating of the tool material by microwaves, maintain the high bonding strength and dimensional accuracy of the grinding wheel, and finally realize the "low-temperature" plastic domain grinding of hard and brittle semiconductor wafers.
[0013] As a further technical solution, the microwave irradiation unit is coaxially arranged with the grinding wheel processing unit, the microwave irradiation head of the microwave irradiation unit is connected to the microwave generator through a microwave antenna, and the microwave irradiation head is placed at the center of the ultra-fine diamond abrasive grinding wheel. The liquid spraying device is offset to the ultra-fine diamond abrasive grinding wheel, and the microwave-grinding coaxial back-reduction processing is performed on the hard and brittle semiconductor wafer through the mutual cooperation of microwaves and grinding wheels, combined with the cooling, lubrication and flushing effects of the grinding fluid.
[0014] As a further technical solution, the microwave irradiation head and liquid spray device of the microwave irradiation unit are offset to the ultra-fine diamond abrasive grinding wheel; through the mutual cooperation of microwaves and grinding wheels, combined with the cooling, lubrication and flushing effects of the grinding fluid, microwave-grinding off-axis back-reduction processing is performed on hard and brittle semiconductor wafers.
[0015] As a further technical solution, the grinding fluid does not contain polar molecules and is a type of lubricating fluid that does not absorb microwaves (ie, it will not be heated by microwaves and can maintain excellent cooling performance).
[0016] As a further technical solution, the grinding wheel processing unit is an ultrafine diamond abrasive grinding wheel, which is a metal bonded diamond abrasive grinding wheel, so it will not absorb microwaves (that is, it will not be heated by microwaves and can maintain high bonding strength), and its abrasive particle size is 0.5 to 5 microns.
[0017] The microwave back-reduction processing in the present invention mainly utilizes microwave electromagnetic energy to promote the propagation and slip of internal dislocations of brittle crystal materials, improve plastic deformation capacity, and achieve high-efficiency and high-quality processing.
[0018] In the second aspect, the present invention is based on the above-mentioned microwave irradiation unit and the grinding wheel processing unit are coaxially arranged, and the corresponding processing method is as follows:
[0019] Fixing the processed hard and brittle semiconductor wafer to be processed onto the workbench;
[0020] The grinding fluid spray device is moved to one side of the hard and brittle semiconductor wafer to be processed;
[0021] The grinding fluid that does not absorb microwaves is evenly sprayed onto the surface of the hard and brittle semiconductor wafer to be processed through a liquid spraying device;
[0022] The worktable drives the hard and brittle semiconductor wafer to be processed to rotate;
[0023] The microwave irradiation head is connected to the microwave generator through the microwave antenna and placed in the center of the grinding wheel processing unit and fixed in parallel, and then installed on the Z-axis movable platform, and the Z-axis is moved for tool setting;
[0024] The microwave generator adjusts the microwave transmission power to perform microwave radiation; the grinding wheel processing unit performs grinding processing;
[0025] After the processing is completed, turn off the microwave generator, turn off the vacuum self-rotating grinding table and retract it to a safe position.
[0026] As a further technical solution, the critical cutting depth d of hard and brittle semiconductor wafers c =λ(H / E) 1 / 2 (K c / H) 2 , where λ is about 8.7, is the brittle-to-plastic transition factor of the hard and brittle semiconductor wafer material, H is the hardness of the hard and brittle semiconductor wafer material after microwave radiation, E is the elastic modulus of the hard and brittle semiconductor wafer material after microwave radiation, and K c It is the fracture toughness of hard and brittle semiconductor wafer material after microwave radiation.
[0027] In the second aspect, the present invention is based on the aforementioned microwave irradiation unit being located on one side of the grinding wheel processing unit and being arranged on different axes, and the corresponding processing method is as follows:
[0028] Mounting the processed hard and brittle semiconductor wafer to be processed on a workbench;
[0029] Placing a microwave irradiation head on one side of the hard and brittle semiconductor wafer to be processed, and determining the relative position between the microwave irradiation head and the surface of the hard and brittle semiconductor wafer;
[0030] The spray head of the grinding fluid spray device is moved to one side of the hard and brittle semiconductor wafer to be processed;
[0031] The grinding fluid that does not absorb microwaves is evenly sprayed onto the surface of the hard and brittle semiconductor wafer to be processed through a micro-lubricating liquid spray device;
[0032] The microwave generator radiates microwaves to perform "low temperature" plastic modification on the surface material of the hard and brittle semiconductor wafer to be processed, and adjusts the microwave heating position and the size of the microwave irradiation area;
[0033] The worktable drives the hard and brittle semiconductor wafer to rotate;
[0034] Install the grinding wheel processing unit to the Z-axis movable platform of the machine tool, move the Z-axis to calibrate the tool, and perform grinding processing;
[0035] After the processing is completed, turn off the microwave generator, turn off the vacuum self-rotating grinding table, retract the tool to a safe position, and withdraw the microwave generator to a safe position.
[0036] As a further technical solution, the critical cutting depth d of hard and brittle semiconductor wafers c =λ(H / E) 1 / 2 (K c / H) 2 , where λ is about 8.7, is the brittle-to-plastic transition factor of the hard and brittle semiconductor wafer material, H is the hardness of the hard and brittle semiconductor wafer material after microwave radiation, E is the elastic modulus of the hard and brittle semiconductor wafer material after microwave radiation, and K c It is the fracture toughness of hard and brittle semiconductor wafer material after microwave radiation.
[0037] As a further technical solution, the microwave radiation area is the action area of the grinding wheel processing unit.
[0038] The beneficial effects of the present invention are as follows:
[0039] The processing system of the present invention is a detachable microwave back-reducing processing system, which is easy to integrate. The microwave irradiation unit can be combined with the back-reducing grinding wheel processing unit to form a microwave-grinding paraxial back-reducing processing system and a microwave-grinding coaxial back-reducing processing system. At the same time, when the present invention performs microwave back-reducing on semiconductor wafers, high-frequency alternating electromagnetic energy is used to induce atoms inside the crystal to collide and rub against each other, promote the propagation and slip of dislocations, and then improve the plastic deformation ability. The output low-power alternating electromagnetic energy can avoid the material from generating a large amount of heat. At the same time, a grinding fluid that does not absorb microwaves is used to cool and lubricate the abrasive-workpiece contact interface, reduce thermal damage and wear of the grinding wheel caused by heat conduction, and use a metal bond diamond grinding wheel that does not absorb microwaves to avoid direct heating of the tool material by microwaves, maintain the high bonding strength and dimensional accuracy of the grinding wheel, and achieve high-efficiency, high-quality, "low-temperature" plastic domain grinding. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0041] Figure 1 , Figure 2 They are respectively schematic diagrams of a microwave-grinding side-axis back-reduction processing system and a microwave-grinding side-axis back-reduction processing system of the present invention;
[0042] FIG3(a), FIG3(b), and FIG3(c) are schematic diagrams of a microwave irradiation unit, a liquid spraying device, and a grinding wheel processing unit, respectively, according to the present invention;
[0043] FIG4( a ) is a simplified schematic diagram of a microwave-grinding side-axis back-reduction processing system;
[0044] FIG4( b ) is a simplified schematic diagram of a microwave-grinding coaxial back-reduction processing system;
[0045] Among them, 1-CNC machine tool, 2-high-speed air-floating spindle, 3-vacuum self-rotating grinding table, 4-hard and brittle semiconductor wafer, 5-multi-freedom magnetic fixture, 6-Z-axis moving platform, 7-microwave irradiation unit, 8-liquid spray device, 9-grinding wheel processing unit, 10-microwave-grinding side-axis back-reduction processing system, 11-microwave-grinding coaxial back-reduction processing system; DETAILED DESCRIPTION
[0046] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0047] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present invention. As used herein, unless otherwise explicitly stated in the present invention, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "include" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof;
[0048] With the rapid development of the power electronics industry, the performance requirements of semiconductor devices are gradually increasing, and the wafer thinning process plays an important role in the semiconductor material chip manufacturing process. On the one hand, the thinning process can reduce the overall thickness of the chip, which is conducive to heat dissipation and integration; on the other hand, it can reduce the thickness of the wafer surface damage layer and surface roughness, release the internal stress accumulated inside the wafer caused by the various processes before thinning, and reduce the degree of collapse of a single chip during the dicing process. The current wafer thinning research and development is in the research and development stage and it is difficult to meet high-end use requirements. Therefore, this embodiment provides a microwave high-efficiency ultra-precision plastic domain back-thinning processing system and method for hard and brittle semiconductor wafers.
[0049] Generally speaking, the main way to improve the plasticity of materials is heating. Heating the material promotes the molecular movement inside the material to produce slip and thus improve the plasticity. Laser-assisted processing is a commonly used auxiliary means in processing. Although it can obtain good surface quality, its shortcomings cannot be ignored. Due to the lack of lubrication and cooling of grinding fluid or cutting fluid, the tool or mold cannot reduce the temperature, resulting in a reduction in the life of the tool or mold. Laser is based on the Boltzmann thermal effect to heat the material to improve the plasticity. Heat is always transferred from the surface to the inside. The material inevitably has a temperature gradient and is prone to thermal cracks. Microwave electromagnetic energy directly acts on the polar molecules or ions inside the material to produce slip to improve plasticity. Heat is only a by-product of the action of microwave energy and materials. Therefore, compared with laser, microwave back reduction processing can perform plastic processing on materials at "low temperature". In addition, the grinding fluid in the present invention is a type of cooling lubricant that does not absorb microwaves. It will not be heated by microwaves to generate high temperatures. Therefore, during the processing of hard and brittle semiconductor wafers, the abrasive-workpiece contact interface can be cooled and lubricated, reducing the thermal damage and wear of the grinding wheel caused by heat conduction; and the grinding fluid that does not absorb microwaves will not affect the radiation path of microwaves, so it can achieve precise irradiation of specific areas, and then achieve fine regulation of the plastic deformation of hard and brittle semiconductor wafers. By adjusting the power and processing time of microwaves, the degree of plastic deformation of the material and the amount of plastic removal of the material can be accurately controlled. At the same time, the use of metal-bonded diamond grinding wheels that do not absorb microwaves avoids direct heating of the tool material by microwaves, maintains the high bonding strength and dimensional accuracy of the grinding wheel, and achieves high-efficiency, high-quality, "low-temperature" plastic domain grinding.
[0050] Glossary: "Low temperature" in the present invention means that the temperature of the workpiece is lower than 200°C;
[0051] Example 1
[0052] This embodiment provides a microwave high-efficiency ultra-precision plastic domain back-reduction processing system and method for hard and brittle semiconductor wafers, such as Figure 1 As shown. The microwave high-efficiency ultra-precision plastic domain back-reduction processing system for hard and brittle semiconductor wafers includes a high-precision CNC back-reduction grinding machine 1, a microwave irradiation unit 7 and a liquid spray device 8. The CNC back-reduction grinding machine 1 is equipped with two high-precision air-floating spindles 2. The two high-speed air-floating spindles are respectively connected to the back-reduction grinding wheel and the vacuum self-rotating grinding table 3 through the grinding wheel clamp and the workpiece clamp, so as to realize the self-rotation movement of the grinding wheel and the vacuum self-rotating grinding table 3 outputting the movement of rotation around its own axis. The vacuum self-rotating grinding table 3 adopts the existing vacuum adsorption hard and brittle semiconductor wafers, and its specific structure is not described in detail here. A high-precision linear motor is installed on the bed of the CNC back-reduction grinding machine, and the linear motor is connected to the high-speed air-floating spindle connected to the grinding wheel to realize high-precision feeding; a Z-axis moving platform 6 is also installed on the bed of the CNC machine tool 1, and the Z-axis moving platform 6 can output vertical movement (according to Figure 1The orientation shown is the horizontal movement direction), and the output movement direction is parallel to the axial direction of the high-speed air-floating spindle 2; the Z-axis moving platform 6 is detachably connected to the liquid spraying device 8 and the grinding wheel processing unit 9.
[0053] The microwave irradiation unit 7 is clamped by a multi-degree-of-freedom magnetic clamp and placed on the left side of the hard and brittle semiconductor wafer to be processed. The microwave irradiation unit 7 is non-coaxially arranged with the grinding wheel processing unit 9, that is, the microwave irradiation unit 7 can be combined with the grinding wheel processing unit 9 to form a microwave-grinding side-axis back-reduction processing system; the microwave irradiation head in the microwave irradiation unit 7 is connected to the microwave generator, and the microwave energy generated by the microwave generator can be emitted to the hard and brittle semiconductor wafer to be processed through the microwave irradiation head; the liquid spraying device 8 can evenly spray the grinding fluid that does not absorb microwaves required in the processing process. Sprinkled onto the surface of the hard and brittle semiconductor wafer to be processed; the grinding wheel processing unit 9 includes a grinding power system, a high-speed air floating spindle, a grinding wheel fixture, etc. The grinding power system can output rotational motion, the grinding power system is connected to the high-speed air floating spindle, and a grinding wheel fixture is provided on the high-speed air floating spindle. The grinding wheel fixture is connected to a grinding wheel, and the grinding wheel adopts a diamond grinding wheel. The abrasive particle size of the diamond grinding wheel is 0.5-5μm, and the selection range of the distance between the diamond grinding wheel and the offset microwave irradiation head is 1.0-10.0cm, and the diameter of the microwave radiation effective area is 50mm.
[0054] In this embodiment, the microwave irradiation head power of the microwave generator in the microwave irradiation unit 7 is 100W, the output power is 0W-100W, and the frequency is 2450MHz.
[0055] During processing, the present invention utilizes the microwave dielectric thermal effect, and high-frequency, low-power microwaves are directly irradiated to act on the surface of hard and brittle semiconductor materials. The high-frequency alternating electromagnetic energy induces collision and friction of atoms inside the crystal material, resulting in dislocation proliferation and slip, thereby improving the plasticity of the material. The output low-power alternating electromagnetic energy can avoid generating a large amount of heat inside the material. At the same time, a grinding fluid that does not absorb microwaves is used to cool and lubricate the abrasive-workpiece contact interface, thereby reducing thermal damage and wear of the grinding wheel caused by heat conduction. A metal-bonded diamond grinding wheel that does not absorb microwaves is used to avoid direct heating of the tool material by microwaves, thereby maintaining the high bonding strength and dimensional accuracy of the grinding wheel, and ultimately achieving "low-temperature" plastic grinding of hard and brittle semiconductor wafers and economical, efficient, and nearly damage-free ultra-precision processing.
[0056] As a further technical solution, the hard and brittle semiconductor wafer to be processed is vacuum adsorbed in front of a vacuum self-selectable grinding table, and the hard and brittle semiconductor wafer to be processed is placed in anhydrous ethanol for ultrasonic cleaning for a set time to remove dirt on the surface of the hard and brittle semiconductor wafer.
[0057] As a further technical solution, the distance between the diamond grinding wheel and the offset microwave irradiation head is selected in the range of 1.0 to 10.0 cm, and the microwave radiation area is the action area of the diamond grinding wheel.
[0058] As a further technical solution, the device is provided with a protective cover against microwave interference, which enables it to operate normally during microwave back-reduction processing.
[0059] It should be particularly noted that the microwave action of this system avoids generating a large amount of heat, and mainly utilizes the microwave energy to interact with the atoms inside the hard and brittle semiconductor wafer to promote dislocation proliferation and slip to improve plasticity.
[0060] Using this system, when microwave-grinding side-axis back-reduction processing is performed on hard and brittle semiconductor wafers, the specific steps are as follows:
[0061] S1: vacuum adsorbing the hard and brittle semiconductor wafer after ultrasonic cleaning onto a vacuum self-rotating grinding table;
[0062] S2: Clamp the microwave irradiation head with a multi-degree-of-freedom magnetic fixture and place it on the left side of the hard and brittle semiconductor wafer to be processed, determine the relative position between the microwave irradiation head and the surface of the hard and brittle semiconductor wafer, install the liquid spraying device on the Z-axis movable platform, and move the spraying head to the left side of the hard and brittle semiconductor wafer to be processed;
[0063] S3: Spraying the grinding fluid that does not absorb microwaves evenly onto the surface of the hard and brittle semiconductor wafer through a liquid spraying device;
[0064] S4: Turn on the microwave generator to radiate microwaves, perform "low temperature" plastic modification on the surface material of the hard and brittle semiconductor wafer, and adjust the microwave irradiation position and area size through a multi-degree-of-freedom magnetic fixture;
[0065] S5: Turn on the vacuum self-rotating grinding table to drive the hard and brittle semiconductor wafer to rotate;
[0066] S6: Install the back-reducing grinding wheel processing unit to the Z-axis movable platform of the machine tool, and move the Z-axis to perform tool setting;
[0067] S7: Start the CNC machine tool to perform microwave-grinding side-axis back reduction processing on the hard and brittle semiconductor wafer. After the processing is completed, turn off the microwave generator, turn off the vacuum self-rotating grinding table, retract the tool to a safe position, and withdraw the microwave generator to a safe position;
[0068] Using the system and method, the method for processing a gallium nitride wafer is as follows:
[0069] S1: Place the GaN wafer in anhydrous ethanol and perform ultrasonic cleaning for 10 minutes to obtain a clean and uncontaminated GaN wafer;
[0070] S2: Use a digital display heater to fix the hard and brittle semiconductor wafer to be processed on the aluminum alloy sample table through paraffin, start the silent oil-free vacuum pump, vacuum adsorb the aluminum alloy sample table onto the vacuum self-rotating grinding table of the machine tool, and adjust the spindle rotation accuracy to less than 1μm through a high-precision micrometer;
[0071] S3: Install the microwave irradiation head on the multi-degree-of-freedom magnetic fixture, adsorb the multi-degree-of-freedom magnetic fixture on the left side of the vacuum self-rotating grinding table, adjust the multi-degree-of-freedom magnetic fixture to move the microwave irradiation head to the left side of the GaN wafer to be processed, and determine its relative position with the surface of the GaN wafer;
[0072] S4: starting the high-precision CNC machine tool 1, turning on the control system, controlling the moving mechanism to move the diamond grinding wheel to the top of the GaN wafer, adjusting the relative position between the grinding wheel and the surface of the GaN wafer by controlling the moving mechanism and the air-floating spindle, and reading the coordinate value of the tool machine coordinate system Z;
[0073] S5: Set the microwave processing parameters, turn on the microwave generator to radiate the processing position of the GaN wafer, and spray the grinding fluid that does not absorb microwaves onto the surface of the GaN wafer at a flow rate of 50L / h through the liquid spray device. Use the grinding fluid for cooling and lubrication, and use microwave energy to perform "low-temperature" plastic modification on the GaN wafer. Adjust the size of the microwave radiation area through a multi-degree-of-freedom magnetic fixture;
[0074] S6: Start the high-speed air-floating spindle 2 to make the vacuum self-rotating grinding table rotate with the gallium nitride wafer;
[0075] S7: Start the high-speed air-floating spindle and the air-floating spindle assembly, control the Z axis to feed 0.5 μm at a time for trial grinding, until the center of the ground sample is flat and has no micro-convexities, and the tool setting is completed;
[0076] S8: Turn on the microwave generator, irradiate the specific position of the gallium nitride wafer with microwaves, use the infrared thermal imager to observe the surface of the gallium nitride wafer immediately after microwave radiation, select the position of the microwave irradiation head corresponding to the hot spot with good roundness and uniform energy, and finally determine the microwave working position;
[0077] S9: Use a multi-degree-of-freedom magnetic fixture to adjust the microwave irradiation head and the diamond grinding wheel to tilt by 30 degrees, and the center of the microwave irradiated hot spot on the surface of the GaN wafer is concentric with the center of the diamond grinding wheel. Set the grinding parameters: GaN wafer speed 1000rpm, grinding wheel speed 3000rpm, grinding depth DOC 0.5μm, feed speed 1μm / min. Set the microwave parameters: microwave action area diameter 50mm, power 50W, time 30min;
[0078] S10: Start the high-precision CNC machine tool and start microwave paraxial assisted wafer thinning on the GaN wafer. After the processing is completed, withdraw the tool to a safe position;
[0079] S11: Withdraw the microwave irradiation head to a safe position, turn off the microwave generator, high-speed air-floating spindle and air-floating spindle assembly, control system and cooling and lubrication system.
[0080] Example 2
[0081] This embodiment provides another microwave back-reduction processing system, which is different from the first embodiment in that: the microwave irradiation unit 7 can be coaxially arranged with the grinding wheel processing unit 9, that is, a microwave-grinding coaxial back-reduction processing system is formed; specifically, in this embodiment, the diamond grinding wheel and the grinding wheel fixture are hollow, the microwave irradiation head of the microwave irradiation unit 7 is placed at the center of the diamond grinding wheel and is fixed inside the grinding wheel fixture, the microwave generator is arranged on the Z-axis moving platform, the microwave antenna connected to the microwave generator passes through the grinding wheel high-speed air floating spindle, the grinding wheel fixture is connected to the microwave irradiation head, the grinding power system can output rotational motion, the grinding power system is connected to the high-speed air floating spindle, the high-speed air floating spindle is provided with a grinding wheel fixture, the grinding wheel fixture is connected to the grinding wheel and the microwave irradiation head, and the remaining structure is the same as that of the first embodiment, and will not be repeated here;
[0082] Using this system, the method of microwave-grinding coaxial back-reduction processing on hard and brittle semiconductor wafers is as follows:
[0083] S1: vacuum adsorbing the hard and brittle semiconductor wafer after ultrasonic cleaning onto a vacuum self-rotating grinding table;
[0084] S2: Install the liquid spraying device on the Z-axis movable platform, and move the spray head to the left side of the hard and brittle semiconductor wafer to be processed;
[0085] S3: Spraying the grinding fluid that does not absorb microwaves evenly onto the surface of the hard and brittle semiconductor wafer through a liquid spraying device;
[0086] S4: Turn on the vacuum self-rotating grinding table to drive the hard and brittle semiconductor wafer to rotate;
[0087] S5: Connect the microwave irradiation head to the microwave generator through the microwave antenna and place it at the center of the diamond grinding wheel. Fix it with a grinding wheel fixture and install it on the Z-axis movable platform of the machine tool. Move the Z-axis to perform tool alignment.
[0088] S6: Turn on the microwave generator, adjust the microwave transmission power to perform microwave radiation, start the CNC machine tool, perform microwave-grinding coaxial back-reduction processing on the hard and brittle semiconductor wafer, and after the processing is completed, turn off the microwave generator, turn off the vacuum self-rotating grinding table, and retract the tool to a safe position;
[0089] As a further technical solution, during microwave-grinding coaxial back-reduction processing, the diamond grinding wheel and the grinding wheel fixture are hollow, the microwave irradiation head is placed in the center of the diamond grinding wheel and fixed inside the grinding wheel fixture, the microwave irradiation head is 1 cm away from the processing surface of the hard and brittle semiconductor wafer, and the microwave radiation area is the action area of the diamond grinding wheel.
[0090] The method for processing gallium nitride wafers by microwave back-reduction specifically comprises the following steps:
[0091] S1: Place the GaN wafer in anhydrous ethanol and perform ultrasonic cleaning for 10 minutes to obtain a clean and uncontaminated GaN wafer;
[0092] S2: Use a digital display heater to fix the hard and brittle semiconductor wafer to be processed on the aluminum alloy sample table through paraffin, start the silent oil-free vacuum pump, vacuum adsorb the aluminum alloy sample table onto the vacuum self-rotating grinding table of the machine tool, and adjust the spindle rotation accuracy to less than 1μm through a high-precision micrometer;
[0093] S3: Connect the microwave irradiation head to the microwave generator through the microwave antenna, place it at the center of the diamond grinding wheel and fix it with a grinding wheel fixture, and then install the grinding wheel processing unit and the microwave generator to the Z-axis movable platform of the machine tool;
[0094] S4: starting the high-precision CNC machine tool 1, turning on the control system, controlling the moving mechanism to move the diamond grinding wheel to the top of the GaN wafer, adjusting the relative position between the grinding wheel and the surface of the GaN wafer by controlling the moving mechanism and the air-floating spindle, and reading the coordinate value of the tool machine coordinate system Z;
[0095] S5: Set the microwave processing parameters, turn on the microwave generator to radiate the processing position of the GaN wafer, and spray the grinding fluid that does not absorb microwaves evenly onto the surface of the GaN wafer at a flow rate of 50L / h through the liquid spray device. Use the grinding fluid for cooling and lubrication, and use microwave energy to perform "low-temperature" plastic modification on the GaN wafer.
[0096] S6: Start the high-speed air-floating spindle 2 to make the vacuum self-rotating grinding table rotate with the gallium nitride wafer;
[0097] S7: Start the high-speed air-floating spindle and the air-floating spindle assembly, and control the Z-axis to feed 0.5 μm at a time until the center of the ground sample is flat and has no micro-convexities, and the tool setting is completed;
[0098] S8: Turn on the microwave generator to irradiate the gallium nitride wafer with microwaves, and use an infrared thermal imager to observe the surface of the gallium nitride wafer immediately after microwave radiation;
[0099] S9: The center of the hot spot on the surface of the GaN wafer is concentric with the center of the diamond grinding wheel. The grinding parameters are set as follows: GaN wafer speed 1000rpm, grinding wheel speed 3000rpm, grinding depth DOC 0.5μm, feed speed 1μm / min. The microwave parameters are set as follows: microwave action area diameter 50mm, power 50W, time 30min;
[0100] S10: Start the high-precision CNC machine tool and start microwave coaxial assisted wafer thinning on the GaN wafer. After the processing is completed, withdraw the tool to a safe position;
[0101] S11: Turn off the microwave generator, high-speed air-floating spindle and air-floating spindle assembly, control system and cooling and lubrication system.
[0102] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A microwave back-reduction processing system for hard and brittle semiconductor wafers, characterized in that: The invention comprises a numerically controlled grinding machine, a microwave irradiation unit, a grinding fluid spraying device and a grinding wheel processing unit. The numerically controlled grinding machine is equipped with a first air-floating spindle and a second air-floating spindle, wherein the first air-floating spindle is installed on a Z-direction moving platform and driven by a linear motor to realize feeding, and the first air-floating spindle is connected to the grinding wheel processing unit through a grinding wheel clamp to realize the self-rotation movement of the grinding wheel processing unit; the second air-floating spindle is connected to a workbench, and the workbench is used to place a hard and brittle semiconductor wafer to be processed to realize the follow-rotation movement of the hard and brittle semiconductor wafer to be processed; the microwave irradiation unit is arranged above the hard and brittle semiconductor wafer to be processed, and microwave electromagnetic energy is used to promote the collision and friction of atoms inside the hard and brittle semiconductor wafer material to be processed to generate the propagation and slip of dislocations to improve the plasticity; the grinding fluid spraying device is offset obliquely above the hard and brittle semiconductor wafer to be processed.
2. The microwave back-reduction processing system for hard and brittle semiconductor wafers according to claim 1, characterized in that: The microwave irradiation unit is coaxially arranged with the grinding wheel processing unit. The microwave irradiation head of the microwave irradiation unit is connected with the microwave generator through a microwave antenna, and the microwave irradiation head is placed at the center of the grinding wheel processing unit.
3. The microwave back-reduction processing system for hard and brittle semiconductor wafers according to claim 1, characterized in that: The microwave irradiation head and the liquid spraying device of the microwave irradiation unit are offset to the ultrafine diamond abrasive grinding wheel.
4. The microwave back-reduction processing system for hard and brittle semiconductor wafers according to claim 1, characterized in that: Grinding fluid does not contain polar molecules and is a type of lubricating fluid that does not absorb microwaves.
5. The microwave back-reduction processing system for hard and brittle semiconductor wafers according to any one of claims 1 to 4, characterized in that: The grinding wheel processing unit is an ultra-fine diamond abrasive grinding wheel, which is a metal-bonded diamond abrasive grinding wheel that does not absorb microwaves and has an abrasive particle size of 0.5 to 5 microns.
6. The processing method of the microwave back-reduction processing system for hard and brittle semiconductor wafers according to any one of claims 2-3, characterized in that: Fixing the processed hard and brittle semiconductor wafer to be processed onto the workbench; The grinding fluid that does not absorb microwaves is evenly sprayed onto the surface of the hard and brittle semiconductor wafer to be processed through a liquid spraying device; The worktable drives the hard and brittle semiconductor wafer to be processed to rotate; The microwave irradiation head is connected to the microwave generator through the microwave antenna and placed in the center of the grinding wheel processing unit and fixed, and then installed on the Z-axis movable platform, and the Z-axis is moved for tool setting; The microwave generator adjusts the microwave transmission power to perform microwave radiation; the grinding wheel processing unit performs grinding processing; After the processing is completed, turn off the microwave generator, turn off the vacuum self-rotating grinding table and retract it to a safe position.
7. The method for processing hard and brittle semiconductor wafers by using a microwave back-reduction processing system as claimed in claim 6, characterized in that: Critical cutting depth d for hard and brittle semiconductor wafers c =λ(H / E) 1 / 2 (K c / H) 2 , where λ is about 8.7, is the brittle-to-plastic transition factor of the hard and brittle semiconductor wafer material, H is the hardness of the hard and brittle semiconductor wafer material after microwave radiation, E is the elastic modulus of the hard and brittle semiconductor wafer material after microwave radiation, and K c It is the fracture toughness of hard and brittle semiconductor wafer material after microwave radiation.
8. The method for processing hard and brittle semiconductor wafers by using a microwave back-reduction processing system as claimed in claim 4, characterized in that: Mounting the processed hard and brittle semiconductor wafer to be processed on a workbench; Placing a microwave irradiation head on one side of the hard and brittle semiconductor wafer to be processed, and determining the relative position between the microwave irradiation head and the surface of the hard and brittle semiconductor wafer; The grinding fluid that does not absorb microwaves is evenly sprayed onto the surface of the hard and brittle semiconductor wafer to be processed through a liquid spraying device; The microwave generator radiates microwaves to perform "low temperature" plastic modification on the surface material of the hard and brittle semiconductor wafer to be processed, and adjusts the microwave heating position and the size of the microwave irradiation area; The worktable drives the hard and brittle semiconductor wafer to rotate; Install the grinding wheel processing unit to the Z-axis movable platform of the machine tool, move the Z-axis to calibrate the tool, and perform grinding processing; After the processing is completed, turn off the microwave generator, turn off the vacuum self-rotating grinding table, retract the tool to a safe position, and withdraw the microwave generator to a safe position.
9. The method for processing hard and brittle semiconductor wafers by a microwave back-reduction processing system as claimed in claim 8, characterized in that: Critical cutting depth d for hard and brittle semiconductor wafers c =λ(H / E) 1 / 2 (K c / H) 2 , where λ is about 8.7, is the brittle-to-plastic transition factor of the hard and brittle semiconductor wafer material, H is the hardness of the hard and brittle semiconductor wafer material after microwave radiation, E is the elastic modulus of the hard and brittle semiconductor wafer material after microwave radiation, and K c It is the fracture toughness of hard and brittle semiconductor wafer material after microwave radiation.
10. The processing method of the microwave back-reduction processing system for hard and brittle semiconductor wafers according to claim 9, characterized in that: The microwave radiation area is the action area of the grinding wheel machining unit.
Citation Information
Patent Citations
Chemical mechanical polishing device based on microwave assistance and method for polishing CaF2 wafer by using chemical mechanical polishing device
CN116810619A
Multi-energy-field combined machining system and method for fragile materials
CN117066904A
Oil-based thermosensitive active grinding fluid and microwave-assisted fixed abrasive grinding method
CN117551424A
Apparatus and method for machining hard and brittle material
JP2010110799A
Cutting method and cutting device of semiconductor substrate
JP2012109357A