A polishing pad with uniform pores and its preparation method

By using p-toluenesulfonamide to replace the high-temperature expansion balls, and combining a specific mixing process and mold preheating, the problem of uneven pore size in traditional polyurethane polishing pads was solved, thus improving the quality uniformity and polishing performance of the polishing pads.

CN118905914BActive Publication Date: 2026-11-17SHANGHAI XINQIAN INTEGRATED CIRCUIT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411172356.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2026-11-17
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Traditional polyurethane polishing pads cannot meet the requirements of precision polishing in terms of dynamic polishing uniformity, concave deformation and mechanical properties, resulting in unstable polishing quality. Furthermore, uneven dispersion of high-temperature expansion balls leads to inconsistent micropores, which may cause wafer scratches or electrostatic breakdown.

Method used

p-Toluenesulfonamide is used instead of high-temperature expansion balls. Through a specific mixing process with polyurethane prepolymer and chain extender, closed, fine and uniform pores are formed. Combined with anhydrous ethanol dissolution and nitrogen gas filling and mixing, the raw materials are ensured to be evenly distributed. The mold is preheated to control the uniformity of curing temperature.

Benefits of technology

This design achieves a uniform distribution of pores within the polishing pad, avoids metal particle residue, improves the quality uniformity and polishing performance of the polishing pad, reduces the density of the polishing pad, and ensures the stability of the polishing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905914B_ABST
    Figure CN118905914B_ABST
Patent Text Reader

Abstract

This invention relates to a polishing pad with uniform pores and its preparation method. The preparation method includes the following steps: (a) weighing the following raw materials by weight: 70-80 parts of polyurethane prepolymer, 3-5 parts of foaming agent, and 15-24 parts of chain extender, wherein the foaming agent is p-toluenesulfonamide; (b) softening the polyurethane prepolymer and the chain extender respectively; (c) dissolving the foaming agent; (d) uniformly mixing the polyurethane prepolymer and the foaming agent to obtain a first mixture; (e) uniformly mixing the chain extender with the first mixture to obtain a second mixture; and (f) subjecting the second mixture to mold curing treatment. Compared with the prior art, this invention uses p-toluenesulfonamide (TSH) instead of high-temperature expansion balls. P-toluenesulfonamide decomposes nitrogen gas upon heating, forming closed, fine, and uniform pores inside the polishing pad to achieve internal pore creation, thereby reducing the density of the polishing pad and effectively avoiding metal particle residue caused by high-temperature expansion balls.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polishing pad preparation, and more particularly to a polishing pad with uniform pores and its preparation method. Background Technology

[0002] In chemical mechanical polishing (CMP), the polishing pad plays a crucial role in storing and transporting polishing fluid, removing waste, transferring processing loads, and ensuring a stable polishing process. The quality of the polishing pad directly affects the polishing effect, and improving the quality of the polishing pad is essential for improving the quality of wafer manufacturing. Common CMP polishing pads include polyurethane polishing pads, non-woven fabric polishing pads, and synthetic leather polishing pads. Among them, polyurethane has the highest polishing removal rate and is currently the most commonly used polishing pad material.

[0003] However, as precision electronic devices place increasingly higher demands on the polishing precision of integrated circuits and wafer surfaces, traditional polyurethane polishing pads cannot fully meet the requirements of precision polishing in terms of dynamic polishing uniformity, concave deformation, and mechanical properties. This results in a high frequency of polishing pad replacement, affecting polishing quality and efficiency.

[0004] To obtain polyurethane polishing pads with more uniform porosity, existing polyurethane polishing pads are made by premixing PET high-temperature expansion balls with liquid polyurethane material, adding a certain amount of chain extender, and then curing in a mold. The cured sample undergoes multiple subsequent processing steps such as slicing, engraving, and lamination to form the final polishing pad. However, polyurethane polishing pads obtained using high-temperature expansion balls are prone to electrostatic agglomeration during the raw material mixing process, resulting in uneven dispersion of the high-temperature expansion balls. This ultimately forms micropores of varying sizes inside the polishing pad, leading to unstable quality. At the same time, metal particles from the high-temperature expansion balls can remain inside the polishing pad and be released during the polishing process, causing irreversible damage to the wafer, such as scratches or electrostatic breakdown. Summary of the Invention

[0005] The purpose of this invention is to overcome the defects of the prior art by providing a polishing pad with uniform pores and its preparation method, so as to improve the uniformity of pore distribution in the polishing pad.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] A method for preparing a polishing pad with uniform pores includes the following steps:

[0008] (a) Weigh the following raw materials by weight: 70-80 parts of polyurethane prepolymer, 3-5 parts of foaming agent and 15-24 parts of chain extender, wherein the foaming agent is p-toluenesulfonamide;

[0009] (b) Soften the polyurethane prepolymer and the chain extender respectively;

[0010] (c) Dissolve the foaming agent;

[0011] (d) The polyurethane prepolymer and the foaming agent are uniformly mixed to obtain a first mixture;

[0012] (e) The chain extender is uniformly mixed with the first mixture to obtain a second mixture;

[0013] (f) The second mixture is subjected to mold curing treatment.

[0014] In one embodiment, step (c) includes the following step: dissolving the foaming agent in anhydrous ethanol, wherein the ratio of the anhydrous ethanol to the foaming agent is 5:1 to 10:1.

[0015] Step (d) includes the following steps: thoroughly mixing the polyurethane prepolymer and the foaming agent; subjecting the mixed polyurethane prepolymer and the foaming agent to constant temperature baking treatment at a temperature of 70-80°C for 15-20 minutes to obtain the first mixture.

[0016] In one embodiment, between step (d) and step (e), the following step is further included: aeration mixing of the first mixture by introducing nitrogen gas above the first mixture at a pressure of 5 to 8 bar, the aeration mixing temperature being 50 to 80°C, and the aeration mixing time being 3 to 4 hours.

[0017] In one embodiment, in step (b), the softening temperature of the polyurethane prepolymer is 50–70°C, and the softening time of the polyurethane prepolymer is 3–5 hours.

[0018] In one embodiment, in step (b), the chain extender is 4,4'-methylenedi(2-chloroaniline), the softening temperature of the chain extender is 100-120°C, and the softening time of the chain extender is 4 hours.

[0019] In one embodiment, in step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 50-80°C, and the softening time of the chain extender is 4 hours.

[0020] In one embodiment, in step (a), the density of the polyurethane prepolymer is 1100–1190 kg / m³. 3The polyurethane prepolymer has a Brookfield viscosity (30°C) of 70–150 poise, the polyurethane prepolymer has an isocyanate group (NCO) mass percentage of 6.5%–11.8%, and the polyurethane prepolymer has a moisture content of less than or equal to 500 ppm.

[0021] In one embodiment, in step (a), the weight components of each raw material are: 73-75 parts of polyurethane prepolymer, 3-5 parts of foaming agent, and 20-24 parts of chain extender.

[0022] In one embodiment, step (f) includes the following steps:

[0023] The mold is preheated at a temperature ≥110℃ for a time ≥5 hours.

[0024] The second mixture is poured into a preheated mold;

[0025] The mold is placed in a constant temperature oven for curing, the curing temperature is 110-120℃, and the curing time is ≥15h.

[0026] A polishing pad with uniform pores is prepared using the above-described preparation method.

[0027] Compared with the prior art, the present invention has the following advantages:

[0028] 1. The above preparation method uses p-toluenesulfonamide (TSH) instead of high-temperature expansion balls. P-toluenesulfonamide decomposes nitrogen gas upon heating, forming closed, fine, and uniform pores inside the polishing pad to achieve pore creation inside the polishing pad, thereby reducing the density of the polishing pad and effectively avoiding metal particle residue caused by high-temperature expansion balls. In the preparation process, the polyurethane prepolymer and the foaming agent are mixed first, and then the chain extender is mixed. This is beneficial for the foaming agent to be fully and uniformly distributed in the mixture, so as to form pores with uniform density and pore size in all parts of the polishing pad. At the same time, the polyurethane prepolymer and chain extender are softened before mixing, and the foaming agent is dissolved before mixing, thereby further improving the uniformity of raw material mixing, thereby improving the uniformity of polishing pad product quality.

[0029] 2. Anhydrous ethanol, as an organic solvent, can effectively dissolve p-toluenesulfonamide, promoting its uniform mixing into the polyurethane prepolymer. Furthermore, it can be removed from the raw material mixture by heating after uniform mixing, thus avoiding the impact of the solvent on the quality of the polishing pad and improving the production quality of the polishing pad.

[0030] 3,4'-methylenebis(2-chloroaniline) (MOCA) and dimethylthiotoluenediamine (DMTDA) are both good and commonly used chain extenders. Therefore, selecting different softening temperatures and softening times according to different chain extenders is beneficial to improving the softening effect of the chain extender, thereby improving the uniformity of raw material mixing.

[0031] 4. When pouring and curing the raw material mixture, preheat the mold first to ensure that the temperature of the mold is close to the curing temperature and that the temperature is uniform throughout the mold. This will prevent the raw material mixture from being heated unevenly after being poured into the mold, and from localized rapid cooling and curing, which would lead to unstable quality of the polishing pad. Attached Figure Description

[0032] Figure 1 This is a process flow diagram of the polishing pad preparation method in this invention.

[0033] Figure 2 The image shown is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 1.

[0034] Figure 3 The image shown is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 2.

[0035] Figure 4 The image shown is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 3.

[0036] Figure 5 The image shown is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 4.

[0037] Figure 6 The image shown is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 5.

[0038] Figure 7 The image shown is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 6.

[0039] Figure 8 The image shown is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 7. Detailed Implementation

[0040] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0041] The following describes in detail, with reference to the accompanying drawings, a polishing pad with uniform pores and its preparation method.

[0042] like Figure 1As shown, in one embodiment, a method for preparing a polishing pad with uniform pores is provided, comprising the following steps:

[0043] (a) Weigh the following raw materials by weight: 70-80 parts of polyurethane prepolymer, 3-5 parts of foaming agent and 15-24 parts of chain extender, wherein the foaming agent is p-toluenesulfonamide;

[0044] (b) Soften the polyurethane prepolymer and the chain extender respectively;

[0045] (c) Dissolve the foaming agent;

[0046] (d) The polyurethane prepolymer and the foaming agent are uniformly mixed to obtain a first mixture;

[0047] (e) The chain extender is uniformly mixed with the first mixture to obtain a second mixture;

[0048] (f) The second mixture is subjected to mold curing treatment.

[0049] The above preparation method uses p-toluenesulfonamide (TSH) instead of high-temperature expansion balls. P-toluenesulfonamide decomposes nitrogen gas upon heating, forming closed, fine, and uniform pores inside the polishing pad to achieve pore creation within the polishing pad, thereby reducing the density of the polishing pad and effectively avoiding metal particle residue caused by high-temperature expansion balls. In the preparation process, the polyurethane prepolymer and the foaming agent are mixed first, and then the chain extender is mixed. This facilitates the full and uniform distribution of the foaming agent in the mixture, so as to form pores with uniform density and pore size in all parts of the polishing pad. At the same time, the polyurethane prepolymer and chain extender are softened before mixing, and the foaming agent is dissolved before mixing, thereby further improving the uniformity of the raw material mixing, and thus improving the uniformity of the polishing pad product quality.

[0050] Specifically, in one embodiment, step (c) includes the following step: dissolving the foaming agent in anhydrous ethanol, wherein the ratio of the anhydrous ethanol to the foaming agent is 5:1 to 10:1.

[0051] Step (d) includes the following steps: thoroughly mixing the polyurethane prepolymer and the foaming agent; subjecting the mixed polyurethane prepolymer and the foaming agent to constant temperature baking treatment at a temperature of 70-80°C for 15-20 minutes to obtain the first mixture.

[0052] Further, in one embodiment, the ratio of anhydrous ethanol to the foaming agent is 8:1; the baking temperature is 75°C and the baking time is 20 minutes to obtain the first mixture.

[0053] Anhydrous ethanol, as an organic solvent, can effectively dissolve p-toluenesulfonamide, promoting its uniform mixing into the polyurethane prepolymer. Furthermore, it can be removed from the raw material mixture by heating after uniform mixing, thus avoiding the impact of the solvent on the quality of the polishing pad and improving the production quality of the polishing pad.

[0054] Specifically, in one embodiment, between step (d) and step (e), the following step is further included: aeration mixing of the first mixture, wherein nitrogen gas is introduced above the first mixture at a pressure of 5 to 8 bar, the aeration mixing temperature is 50 to 80°C, and the aeration mixing time is 3 to 4 hours.

[0055] Further, the first mixture is subjected to aeration mixing, in which nitrogen gas is introduced above the first mixture at a pressure of 5 bar, the aeration mixing temperature is 50°C, and the aeration mixing time is 4 hours.

[0056] Further, the first mixture is subjected to aeration mixing by introducing nitrogen gas above the first mixture at a pressure of 8 bar, the aeration mixing temperature being 80°C, and the aeration mixing time being 3 hours.

[0057] Specifically, in one embodiment, in step (b), the softening temperature of the polyurethane prepolymer is 50–70°C, and the softening time of the polyurethane prepolymer is 3–5 hours.

[0058] Further, in step (b), the softening temperature of the polyurethane prepolymer is 50°C, and the softening time of the polyurethane prepolymer is 5 hours.

[0059] Further, in step (b), the softening temperature of the polyurethane prepolymer is 70°C, and the softening time of the polyurethane prepolymer is 3 hours.

[0060] Further, in step (b), the softening temperature of the polyurethane prepolymer is 60°C, and the softening time of the polyurethane prepolymer is 4 hours.

[0061] Specifically, in one embodiment, in step (b), the chain extender is 4,4'-methylenedi(2-chloroaniline), the softening temperature of the chain extender is 100-120°C, and the softening time of the chain extender is 4 hours.

[0062] Further, in one embodiment, in step (b), the chain extender is 4,4'-methylenedi(2-chloroaniline), the softening temperature of the chain extender is 100°C, and the softening time of the chain extender is 4 hours.

[0063] Further, in one embodiment, in step (b), the chain extender is 4,4'-methylenedi(2-chloroaniline), the softening temperature of the chain extender is 110°C, and the softening time of the chain extender is 4 hours.

[0064] Further, in one embodiment, in step (b), the chain extender is 4,4'-methylenebis(2-chloroaniline), the softening temperature of the chain extender is 120°C, and the softening time of the chain extender is 4 hours.

[0065] Specifically, in one embodiment, in step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 50-80°C, and the softening time of the chain extender is 4 hours.

[0066] Furthermore, in one embodiment, in step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 70°C, and the softening time of the chain extender is 4 hours.

[0067] Furthermore, in one embodiment, in step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 50°C, and the softening time of the chain extender is 4 hours.

[0068] Furthermore, in one embodiment, in step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 80°C, and the softening time of the chain extender is 4 hours.

[0069] 4,4'-methylenebis(2-chloroaniline) (MOCA) and dimethylthiotoluenediamine (DMTDA) are both good and commonly used chain extenders. Therefore, selecting different softening temperatures and softening times according to different chain extenders is beneficial to improving the softening effect of the chain extender, thereby improving the uniformity of raw material mixing.

[0070] Specifically, in one embodiment, in step (a), the density of the polyurethane prepolymer is 1100–1190 kg / m³. 3 The polyurethane prepolymer has a Brookfield viscosity (30°C) of 70–150 poise, the polyurethane prepolymer has an isocyanate group (NCO) mass percentage of 6.5%–11.8%, and the polyurethane prepolymer has a moisture content of less than or equal to 500 ppm.

[0071] Furthermore, in one embodiment, in step (a), the density of the polyurethane prepolymer is 1100 kg / m³. 3The polyurethane prepolymer has a Brookfield viscosity (30°C) of 100 poise, the polyurethane prepolymer contains 7.5% isocyanate groups (NCO) by mass, and the polyurethane prepolymer contains 400 ppm of moisture.

[0072] Specifically, in one embodiment, in step (a), the weight components of each raw material are: 73-75 parts of polyurethane prepolymer, 3-5 parts of foaming agent and 20-24 parts of chain extender.

[0073] Further, in one embodiment, in step (a), the weight components of each raw material are: 75 parts of polyurethane prepolymer, 4 parts of foaming agent and 22 parts of chain extender.

[0074] Further, in one embodiment, in step (a), the weight components of each raw material are: 73 parts of polyurethane prepolymer, 3 parts of foaming agent and 20 parts of chain extender.

[0075] Further, in one embodiment, in step (a), the weight components of each raw material are: 74 parts of polyurethane prepolymer, 5 parts of foaming agent and 24 parts of chain extender.

[0076] Specifically, in one embodiment, step (f) includes the following steps:

[0077] The mold is preheated at a temperature ≥110℃ for a time ≥5 hours.

[0078] The second mixture is poured into a preheated mold;

[0079] The mold is placed in a constant temperature oven for curing, the curing temperature is 110-120℃, and the curing time is ≥15h.

[0080] Furthermore, in one embodiment, in step (f), the mold preheating temperature is ≥115°C, the mold preheating time is 6h, the curing temperature is 115°C, and the curing time is 17h.

[0081] When pouring and curing the raw material mixture, the mold is preheated to ensure that the temperature of the mold is close to the curing temperature and that the temperature is uniform throughout the mold. This prevents the raw material mixture from being heated unevenly after being poured into the mold, and avoids localized rapid cooling and curing, which would lead to unstable quality of the polishing pad.

[0082] In one embodiment, a polishing pad with uniform pores is provided, which is prepared by the above-described preparation method.

[0083] The above preparation method uses p-toluenesulfonamide (TSH) instead of high-temperature expansion balls. P-toluenesulfonamide decomposes nitrogen gas upon heating, forming closed, fine, and uniform pores inside the polishing pad to achieve pore creation within the polishing pad, thereby reducing the density of the polishing pad and effectively avoiding metal particle residue caused by high-temperature expansion balls. In the preparation process, the polyurethane prepolymer and the foaming agent are mixed first, and then the chain extender is mixed. This facilitates the full and uniform distribution of the foaming agent in the mixture, so as to form pores with uniform density and pore size in all parts of the polishing pad. At the same time, the polyurethane prepolymer and chain extender are softened before mixing, and the foaming agent is dissolved before mixing, thereby further improving the uniformity of the raw material mixing, and thus improving the uniformity of the polishing pad product quality.

[0084] Example 1

[0085] The polishing pad obtained by the preparation method in Example 1 is as follows: Figure 2 As shown, the specific steps are as follows:

[0086] Weigh the following raw materials by weight: 75 parts polyurethane prepolymer, 4 parts high-temperature expansion balls, and 20 parts chain extender. The density of the polyurethane prepolymer is 1100 kg / m³. 3 The polyurethane prepolymer has a Brookfield viscosity (30°C) of 150 poise, the polyurethane prepolymer has an isocyanate group (NCO) mass percentage of 10.8%, and the polyurethane prepolymer has a moisture content of less than or equal to 500 ppm.

[0087] The polyurethane prepolymer and the chain extender are softened separately. The softening temperature of the polyurethane prepolymer is 60°C and the softening time of the polyurethane prepolymer is 4h. The chain extender is 4,4'-methylenedi-(2-chloroaniline) (MOCA), the softening temperature of the chain extender is 110°C, and the softening time of the chain extender is 4h.

[0088] The polyurethane prepolymer and high-temperature expansion balls are thoroughly mixed; the mixed polyurethane prepolymer and high-temperature expansion balls are then subjected to constant temperature baking treatment at 75°C for 20 minutes to obtain the first mixture.

[0089] The first mixture is subjected to aeration mixing, in which nitrogen gas is introduced above the first mixture at a pressure of 5 bar, the aeration mixing temperature is 70°C, and the aeration mixing time is 3 hours.

[0090] The mold is preheated at a temperature of 115°C for 6 hours.

[0091] The second mixture is poured into a preheated mold;

[0092] The mold is placed in a constant temperature oven for curing at a temperature of 120°C for 16 hours.

[0093] Example 2

[0094] Compared with Example 1, Example 2 uses p-toluenesulfonamide foaming agent instead of high-temperature expansion balls to prepare the polishing pad, while keeping other components and process conditions unchanged. The polishing pad obtained by the preparation method of Example 2 is as follows: Figure 3 As shown, the specific steps are as follows:

[0095] Weigh the following raw materials by weight: 75 parts polyurethane prepolymer, 4 parts blowing agent, and 20 parts chain extender, wherein the blowing agent is p-toluenesulfonamide, and the density of the polyurethane prepolymer is 1100 kg / m³. 3 The polyurethane prepolymer has a Brookfield viscosity (30°C) of 150 poise, the polyurethane prepolymer has an isocyanate group (NCO) mass percentage of 10.8%, and the polyurethane prepolymer has a moisture content of less than or equal to 500 ppm.

[0096] The polyurethane prepolymer and the chain extender are softened separately. The softening temperature of the polyurethane prepolymer is 60°C and the softening time of the polyurethane prepolymer is 4h. The chain extender is 4,4'-methylenedi-(2-chloroaniline) (MOCA), the softening temperature of the chain extender is 110°C, and the softening time of the chain extender is 4h.

[0097] The foaming agent is dissolved in anhydrous ethanol, wherein the ratio of anhydrous ethanol to the foaming agent is 8:1.

[0098] The polyurethane prepolymer and the foaming agent are thoroughly mixed; the mixed polyurethane prepolymer and the foaming agent are then subjected to a constant temperature baking treatment at 75°C for 20 minutes to obtain the first mixture.

[0099] The first mixture is subjected to aeration mixing, in which nitrogen gas is introduced above the first mixture at a pressure of 5 bar, the aeration mixing temperature is 70°C, and the aeration mixing time is 3 hours.

[0100] The mold is preheated at a temperature of 115°C for 6 hours.

[0101] The second mixture is poured into a preheated mold;

[0102] The mold is placed in a constant temperature oven for curing at a temperature of 120°C for 16 hours.

[0103] Example 3

[0104] Compared with Example 2, Example 3 changed the raw material ratio, while keeping other components and process conditions unchanged. The polishing pad obtained by the preparation method of Example 3 is as follows: Figure 4 As shown, the specific steps are as follows:

[0105] Weigh the following raw materials by weight: 100 parts polyurethane prepolymer, 2 parts blowing agent, and 22 parts chain extender, wherein the blowing agent is p-toluenesulfonamide, and the density of the polyurethane prepolymer is 1100 kg / m³. 3 The polyurethane prepolymer has a Brookfield viscosity (30°C) of 150 poise, the polyurethane prepolymer contains 8.5% isocyanate groups (NCO) by mass, and the polyurethane prepolymer contains less than or equal to 500 ppm of moisture.

[0106] The polyurethane prepolymer and the chain extender are softened separately. The softening temperature of the polyurethane prepolymer is 60°C and the softening time of the polyurethane prepolymer is 4h. The chain extender is 4,4'-methylenedi-(2-chloroaniline) (MOCA), the softening temperature of the chain extender is 110°C, and the softening time of the chain extender is 4h.

[0107] The foaming agent is dissolved in anhydrous ethanol, wherein the ratio of anhydrous ethanol to the foaming agent is 8:1.

[0108] The polyurethane prepolymer and the foaming agent are thoroughly mixed; the mixed polyurethane prepolymer and the foaming agent are then subjected to a constant temperature baking treatment at 75°C for 20 minutes to obtain the first mixture.

[0109] The first mixture is subjected to aeration mixing, in which nitrogen gas is introduced above the first mixture at a pressure of 5 bar, the aeration mixing temperature is 70°C, and the aeration mixing time is 3 hours.

[0110] The mold is preheated at a temperature of 115°C for 6 hours.

[0111] The second mixture is poured into a preheated mold;

[0112] The mold is placed in a constant temperature oven for curing at a temperature of 120°C for 16 hours.

[0113] Example 4

[0114] Compared with Example 2, Example 4 changed the raw material ratio, while keeping other components and process conditions unchanged. The polishing pad obtained by the preparation method of Example 4 is as follows: Figure 5 As shown, the specific steps are as follows:

[0115] Weigh the following raw materials by weight: 100 parts polyurethane prepolymer, 0.5 parts blowing agent, and 24 parts chain extender, wherein the blowing agent is p-toluenesulfonamide, and the density of the polyurethane prepolymer is 1100 kg / m³. 3 The polyurethane prepolymer has a Brookfield viscosity (30°C) of 150 poise, the polyurethane prepolymer has an isocyanate group (NCO) mass percentage of 9.8%, and the polyurethane prepolymer has a moisture content of less than or equal to 500 ppm.

[0116] The polyurethane prepolymer and the chain extender are softened separately. The softening temperature of the polyurethane prepolymer is 60°C and the softening time of the polyurethane prepolymer is 4h. The chain extender is 4,4'-methylenedi-(2-chloroaniline) (MOCA), the softening temperature of the chain extender is 110°C, and the softening time of the chain extender is 4h.

[0117] The foaming agent is dissolved in anhydrous ethanol, wherein the ratio of anhydrous ethanol to the foaming agent is 8:1.

[0118] The polyurethane prepolymer and the foaming agent are thoroughly mixed; the mixed polyurethane prepolymer and the foaming agent are then subjected to a constant temperature baking treatment at 75°C for 20 minutes to obtain the first mixture.

[0119] The first mixture is subjected to aeration mixing, in which nitrogen gas is introduced above the first mixture at a pressure of 5 bar, the aeration mixing temperature is 70°C, and the aeration mixing time is 3 hours.

[0120] The mold is preheated at a temperature of 115°C for 6 hours.

[0121] The second mixture is poured into a preheated mold;

[0122] The mold is placed in a constant temperature oven for curing at a temperature of 120°C for 16 hours.

[0123] Example 5

[0124] Compared with Example 2, Example 5 uses DMTDA (dimethylthiotoluene diamine) as a chain extender, and changes the raw material ratio, curing temperature, and time, while keeping other components and process conditions unchanged. The polishing pad obtained by the preparation method of Example 5 is as follows: Figure 6 As shown, the specific steps are as follows:

[0125] Weigh the following raw materials by weight: 100 parts polyurethane prepolymer, 4 parts blowing agent, and 20 parts chain extender, wherein the blowing agent is p-toluenesulfonamide, and the density of the polyurethane prepolymer is 1100 kg / m³. 3 The polyurethane prepolymer has a Brookfield viscosity (30°C) of 150 poise, the polyurethane prepolymer has an isocyanate group (NCO) mass percentage of 10.8%, and the polyurethane prepolymer has a moisture content of less than or equal to 500 ppm.

[0126] The polyurethane prepolymer and the chain extender are softened separately. The softening temperature of the polyurethane prepolymer is 60°C and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is DMTDA (dimethylthiotoluene diamine), and the softening temperature of the chain extender is 110°C and the softening time of the chain extender is 4 hours.

[0127] The foaming agent is dissolved in anhydrous ethanol, wherein the ratio of anhydrous ethanol to the foaming agent is 8:1.

[0128] The polyurethane prepolymer and the foaming agent are thoroughly mixed; the mixed polyurethane prepolymer and the foaming agent are then subjected to a constant temperature baking treatment at 75°C for 20 minutes to obtain the first mixture.

[0129] The first mixture is subjected to aeration mixing, in which nitrogen gas is introduced above the first mixture at a pressure of 5 bar, the aeration mixing temperature is 70°C, and the aeration mixing time is 3 hours.

[0130] The mold is preheated at a temperature of 115°C for 6 hours.

[0131] The second mixture is poured into a preheated mold;

[0132] The mold is placed in a constant temperature oven for curing at a temperature of 110°C for 20 hours.

[0133] Example 6

[0134] Compared to Example 2, Example 6 used DMTDA (dimethylthiotoluene diamine) as a chain extender, and changed the raw material ratio, curing temperature, and time, while keeping other components and process conditions unchanged. The polishing pad obtained by the preparation method of Example 6 is as follows: Figure 7 As shown, the specific steps are as follows:

[0135] Weigh the following raw materials by weight: 100 parts polyurethane prepolymer, 2 parts blowing agent, and 22 parts chain extender, wherein the blowing agent is p-toluenesulfonamide, and the density of the polyurethane prepolymer is 1100 kg / m³. 3The polyurethane prepolymer has a Brookfield viscosity (30°C) of 150 poise, the polyurethane prepolymer has an isocyanate group (NCO) mass percentage of 10.8%, and the polyurethane prepolymer has a moisture content of less than or equal to 500 ppm.

[0136] The polyurethane prepolymer and the chain extender are softened separately. The softening temperature of the polyurethane prepolymer is 60°C and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is DMTDA (dimethylthiotoluene diamine), and the softening temperature of the chain extender is 110°C and the softening time of the chain extender is 4 hours.

[0137] The foaming agent is dissolved in anhydrous ethanol, wherein the ratio of anhydrous ethanol to the foaming agent is 8:1.

[0138] The polyurethane prepolymer and the foaming agent are thoroughly mixed; the mixed polyurethane prepolymer and the foaming agent are then subjected to a constant temperature baking treatment at 75°C for 20 minutes to obtain the first mixture.

[0139] The first mixture is subjected to aeration mixing, in which nitrogen gas is introduced above the first mixture at a pressure of 5 bar, the aeration mixing temperature is 70°C, and the aeration mixing time is 3 hours.

[0140] The mold is preheated at a temperature of 115°C for 6 hours.

[0141] The second mixture is poured into a preheated mold;

[0142] The mold is placed in a constant temperature oven for curing at a temperature of 110°C for 20 hours.

[0143] Example 7

[0144] Compared with Example 2, Example 7 used DMTDA (dimethylthiotoluene diamine) as a chain extender, and changed the raw material ratio, curing temperature and time, while keeping other components and process conditions unchanged. The polishing pad obtained by the preparation method of Example 7 is as follows: Figure 8 As shown, the specific steps are as follows:

[0145] Weigh the following raw materials by weight: 100 parts polyurethane prepolymer, 4 parts blowing agent, and 24 parts chain extender, wherein the blowing agent is p-toluenesulfonamide, and the density of the polyurethane prepolymer is 1100 kg / m³. 3The polyurethane prepolymer has a Brookfield viscosity (30°C) of 150 poise, the polyurethane prepolymer has an isocyanate group (NCO) mass percentage of 10.8%, and the polyurethane prepolymer has a moisture content of less than or equal to 500 ppm.

[0146] The polyurethane prepolymer and the chain extender are softened separately. The softening temperature of the polyurethane prepolymer is 60°C and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is DMTDA (dimethylthiotoluene diamine), and the softening temperature of the chain extender is 110°C and the softening time of the chain extender is 4 hours.

[0147] The foaming agent is dissolved in anhydrous ethanol, wherein the ratio of anhydrous ethanol to the foaming agent is 8:1.

[0148] The polyurethane prepolymer and the foaming agent are thoroughly mixed; the mixed polyurethane prepolymer and the foaming agent are then subjected to a constant temperature baking treatment at 75°C for 20 minutes to obtain the first mixture.

[0149] The first mixture is subjected to aeration mixing, in which nitrogen gas is introduced above the first mixture at a pressure of 5 bar, the aeration mixing temperature is 70°C, and the aeration mixing time is 3 hours.

[0150] The mold is preheated at a temperature of 115°C for 6 hours.

[0151] The second mixture is poured into a preheated mold;

[0152] The mold is placed in a constant temperature oven for curing at a temperature of 110°C for 20 hours.

[0153] The polishing pad prepared in Example 1 is as follows: Figure 2 As shown, the polishing pads prepared in Examples 2-7 are as follows: Figure 3-8 As shown in the scanning electron microscope images of the polishing pads, the polishing pads prepared in Examples 2-7 have a significantly more uniform pore distribution and smaller pore diameter. Therefore, the polishing pads prepared using p-toluenesulfonamide (TSH) have better polishing performance and effectively improve the pore uniformity and quality uniformity of the polishing pads.

[0154] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A method of manufacturing a polishing pad having uniform pores, characterized by, Includes the following steps: (a) Weigh the following raw materials by weight: 70-80 parts of polyurethane prepolymer, 3-5 parts of foaming agent and 15-24 parts of chain extender, wherein the foaming agent is p-toluenesulfonamide; (b) Soften the polyurethane prepolymer and the chain extender respectively; (c) Dissolve the foaming agent; (d) The polyurethane prepolymer and the foaming agent are uniformly mixed to obtain a first mixture; (e) The chain extender is uniformly mixed with the first mixture to obtain a second mixture; (f) The second mixture is subjected to mold curing treatment; In step (c), the following steps are included: dissolving the foaming agent in anhydrous ethanol, wherein the ratio of the anhydrous ethanol to the foaming agent is 5:1 to 10:1; Step (d) includes the following steps: thoroughly mixing the polyurethane prepolymer and the foaming agent; subjecting the mixed polyurethane prepolymer and the foaming agent to constant temperature baking treatment at a temperature of 70~80℃ for 15~20min to obtain the first mixture.

2. The method for preparing a polishing pad with uniform pores according to claim 1, characterized in that, Between steps (d) and (e), the following steps are also included: aeration mixing of the first mixture, nitrogen gas is introduced above the first mixture at a pressure of 5-8 bar, the aeration mixing temperature is 50-80°C, and the aeration mixing time is 3-4 hours.

3. The method for preparing a polishing pad with uniform pores according to claim 1, characterized in that, In step (b), the softening temperature of the polyurethane prepolymer is 50~70℃, and the softening time of the polyurethane prepolymer is 3~5h.

4. The method for preparing a polishing pad with uniform pores according to claim 1, characterized in that, In step (b), the chain extender is 4,4'-methylenedi-(2-chloroaniline), the softening temperature of the chain extender is 100~120℃, and the softening time of the chain extender is 4h.

5. The method for preparing a polishing pad with uniform pores according to claim 1, characterized in that, In step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 50~80℃, and the softening time of the chain extender is 4h.

6. The method for preparing a polishing pad with uniform pores according to claim 1, characterized in that, In step (a), the density of the polyurethane prepolymer is 1100~1190 kg / m³, the Brookfield viscosity (30°C) of the polyurethane prepolymer is 70~150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 6.5%~11.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

7. The method for preparing a polishing pad with uniform pores according to claim 1, characterized in that, In step (a), the weight composition of each raw material is: 73-75 parts of polyurethane prepolymer, 3-5 parts of foaming agent and 20-24 parts of chain extender.

8. The method for preparing a polishing pad with uniform pores according to claim 1, characterized in that, Step (f) includes the following steps: The mold is preheated at a temperature ≥110℃ for a time ≥5 hours. The second mixture is poured into a preheated mold; The mold is placed in a constant temperature oven for curing, the curing temperature is 110~120℃, and the curing time is ≥15h.

9. A polishing pad with uniform pores, characterized in that, It is prepared by the preparation method according to any one of claims 1-8.

Citation Information

Patent Citations

  • Blending modification aromatic polyester microcellular foaming material and preparation method thereof

    CN107057303A

  • Fixed abrasive polishing pad, method of preparing the same, and chemical mechanical polishing apparatus including the same

    US20070128991A1