High-thermal-conductivity graphene structure film and synthesis method thereof

During the processing of graphene structural film, the problem of dust introduction is solved by peeling off the release layer of the double-sided adhesive surface with the combination of guide rods, limiting wheels and small electro-extension rods, and the release layer of the double-sided adhesive surface is used to remove and spiral winding the receiving coil, which ensures that graphite is High thermal conductivity and processing quality of olefin films.

CN118906471APending Publication Date: 2024-11-08安徽碳华新材料科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411065243.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the processing of graphene structural film, floating dust on the surface of the adhesive layer is easily introduced, which affects the subsequent bonding effect and reduces the thermal conductivity of the graphene film.

Method used

By using the cooperation of guide rods, limiting wheels and small electric extension rods during the calendering process, the release layer of the double-sided adhesive surface is peeled off and spiral winding is carried out to avoid dust bonding, and the winding is extended by the translation winding collector Length ensures high thermal conductivity of the graphene film.

Benefits of technology

It effectively avoids the introduction of floating dust, stabilizes the bonding effect of the adhesive layer, and ensures the high thermal conductivity and processing quality of the graphene film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906471A_ABST
    Figure CN118906471A_ABST
Patent Text Reader

Abstract

The invention relates to a high thermal conductivity graphene structure film and a synthetic method thereof applied to the field of graphene film processing, and the synthetic method comprises the following steps: S1, mounting a graphene film roll on a second roller, mounting a composite film roll on a third roller, and sleeving a first roller with a double-sided adhesive roll with a hollow section; s2, the ends of the graphene roll, the composite film roll and the double-faced adhesive tape roll with the same section width value are pulled to pass through the middle of two calendering rollers respectively, and calendering treatment is carried out; s3, in the calendering process, the release layers on the upper surface and the lower surface of the double-faced adhesive tape roll are stripped off through a dust prevention unit, and it is avoided that floating dust adheres to the surface of the double-faced adhesive tape due to the fact that the release layers are stripped off too early; and S4, the graphene structure film obtained through calendering is wound by a winding roller, in the synthesis process, it is avoided that floating dust adheres to the surface of the double-faced adhesive tape due to premature stripping, meanwhile, the release layer obtained after horizontal stripping is separated from the cross section range of the graphene film and then vertically connected to the surface of a winding rod in a wound mode, and effective winding treatment is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a high thermal conductivity graphene structure film and a synthesis method thereof, and in particular to a high thermal conductivity graphene structure film and a synthesis method thereof applied in the field of graphene film processing. Background Art

[0002] As a "rising star" in the new materials industry, graphene thermal conductive film has attracted much attention due to its outstanding ultra-high thermal conductivity and heat flux performance advantages, as well as excellent flexibility and light weight. When processing high thermal conductivity graphene heat dissipation film, an adhesive layer is usually used to achieve a composite connection operation between the graphene film and other types of films, and the corresponding high thermal conductivity graphene structure film is manufactured through calendering and other technologies.

[0003] The specification of Chinese invention patent CN202410392282.8 discloses a graphene heat dissipation film vacuum calendering device. According to the deformation occurring during the calendering process of the graphene heat dissipation film, the compression spring applies pressure to the end of the outer rod away from the scraper head. The two scrapers located on the top and bottom sides of the heat dissipation film can act on the outside of the release film and the protective film respectively. As the taut heat dissipation film is continuously transmitted outward by two sets of transmission rollers, the bubbles or raised parts inside the double-sided tape and the single-sided tape can be scraped flat. At the same time, the sides of the release film and the protective film are forcibly pressed to avoid warping between the release film and the protective film during the calendering process.

[0004] When the existing graphene structure membrane is processed and synthesized, the upper and lower sides of the adhesive layer are respectively the high thermal conductivity graphene membrane and other membranes. The surface of the double-sided tape in the middle layer is usually provided with release paper, which needs to be torn off and transported by the conveyor roller and calendered by the calendering roller before the corresponding synthesis operation can be realized. However, after being torn off, both sides of the double-sided tape are easily adhered to dust during the process of being transported to the calendering roller, which affects the subsequent bonding effect. At the same time, the introduction of dust will also affect the thermal conductivity of the graphene membrane to some extent. Summary of the invention

[0005] In view of the above-mentioned prior art, the technical problem to be solved by the present invention is to improve the floating dust adsorption phenomenon on the surface of the adhesive layer during the synthesis process of the graphene structure film.

[0006] To solve the above problems, the present invention provides a method for synthesizing a high thermal conductivity graphene structure film, comprising the following steps:

[0007] S1. Install the graphene film roll on the second roller, install the composite film roll on the third roller, and sleeve the double-sided film roll with a hollow cross-section design on the first roller;

[0008] S2, pulling the ends of the graphene roll, the composite film roll and the double-sided film roll with the same cross-sectional width through the middle of two calendering rollers for calendering treatment;

[0009] S3. During the calendering process, the release layers on the upper and lower surfaces of the double-sided tape are pulled and peeled off by using a dust avoidance unit, and the release layers are spirally staggered and wound up to avoid premature peeling of the release layers, which may cause dust to adhere to the surface of the double-sided tape.

[0010] The second roller, the first roller and the third roller are installed on the material rack, a support frame is installed on one side of the material rack, and a support rod frame is installed on the surfaces of the support frames close to each other. The dust-proof unit includes vertical plates installed on both sides of the support rod frame, and rotating motors are installed on the surfaces of the two vertical plates. A connecting frame is installed through a long rod on the surfaces of the two vertical plates close to each other. Guide rods arranged up and down about the double-sided film are installed on the surfaces of the two vertical plates close to each other, and the upper and lower guide rods are connected through a conveyor belt transmission. The output end of the rotating motor is connected to the surface of one of the guide rods, and two limiting wheels are arranged on the surface of the guide rods. Small electric extension rods symmetrically arranged about the guide rods are installed on the surfaces of each connecting frame that are away from each other, and the power end of the small electric extension rod is connected to a stroking block whose surface slides and fits on the surface of the guide rod, and the length of the stroking block is greater than the diameter value of the limiting wheel;

[0011] S31, winding two release layers on the surface of the double-sided film roll around the surfaces of guide rods arranged above and below the double-sided film roll respectively;

[0012] S32, rubbing the release layer wound on the surface of the guide rod to form a spiral winding structure, and then the tail end of the release layer is located outside the double-sided adhesive and then vertically wound downward on the surface of the winding rod;

[0013] S4. The graphene structure film obtained by calendering is rolled up by a winding roller.

[0014] In the above-mentioned method for synthesizing the high thermal conductivity graphene structure film, the cooperation of the guide rod, the limiting wheel, the small electric extension rod and the winding rod is utilized to prevent the surface of the double-sided tape from being adhered to dust. At the same time, through the spiral winding method, the release layer after horizontal peeling can be separated from the cross-sectional range of the graphene film and then vertically wound to the surface of the winding rod, thereby realizing effective winding processing.

[0015] As a further improvement of the present application, two calendering rollers and one winding roller are installed on the support rod frame, and the top tangent position of the winding roller is at the same height as the horizontal line between the two calendering rollers, a heat dissipation fan box is arranged on one side of the two calendering rollers, and the air outlets of the two heat dissipation fan boxes are connected to the interior of the two calendering rollers, the interior of the calendering roller is hollow and an air outlet is provided at the other end of the calendering roller.

[0016] As a further improvement of the present application, a release layer is wound around the surface of each guide rod, wherein the winding area of ​​the release layer on the guide rod surface is in the middle of the two limiting wheels, and the release layer is spirally wound around the surface of the guide rod, wherein the spiral winding amplitude of the release layer on the upper guide rod surface is smaller than the spiral winding amplitude of the release layer on the lower guide rod surface.

[0017] As a further improvement of the present application, a winding unit is installed on the inner side of the support frame, wherein the winding unit includes a winding rod installed inside the support frame, a servo motor is installed on the surface of one side of the support frame, and the output end of the servo motor is connected to one end of the winding rod, the number of spiral winding turns of the release layer on the surface of the guide rod is one turn, and the projection of the tail end of the upper release layer after winding in the vertical direction is located on the outside of the double-sided film and is wound on the surface of the winding rod.

[0018] As another improvement of the present application, the replacement structure of the winding unit is a translational winder, which includes two movable rods, a movable plate is slidably connected to the inside of the support frame, a driving motor is installed on the top of the movable plate, the output end of the driving motor is connected to the movable rod, the movable rod is inserted into the interior of the support frame, electric telescopic rods are installed on both side surfaces of the support frame, and the power end of the electric telescopic rods is connected to the bottom of the movable plate.

[0019] As another improved supplement of the present application, the sum of the lengths of the movable rods is less than half of the cross-sectional width of the support frame, and the two electric telescopic rods move in the same direction when working.

[0020] As another improved supplement of the present application, the sum of the lengths of the two guide rods is smaller than the length of the long rod, and the length of the guide rod is smaller than the horizontal distance between the connecting frame and the vertical plate, and the limiting wheels on the upper and lower guide rod surfaces are staggered.

[0021] As another improvement of the present application, a high thermal conductivity graphene structure film is synthesized using a method for synthesizing a high thermal conductivity graphene structure film.

[0022] To summarize, when synthesizing a high thermal conductivity graphene structure film, the present application utilizes the cooperation of a guide rod, a limiting wheel, a small electric extension rod, and a winding rod to peel off the release layer on the surface of the double-sided adhesive near the calendering position, thereby avoiding premature peeling that causes dust to adhere to the surface of the double-sided adhesive. At the same time, through the spiral winding method, the release layer wound on the surface of the guide rod after horizontal peeling can be displaced a small distance to escape from the cross-sectional range of the graphene film and then vertically wound to the surface of the winding rod, thereby achieving effective winding processing. The release layer can also be threadedly wound using a translation winder to extend the effective winding length. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a flow chart of the synthesis method of the first embodiment of the present application;

[0024] Figure 2 A schematic diagram of the composition of the high thermal conductivity graphene structure film synthesized in this application;

[0025] Figure 3 This is a schematic diagram of the overall appearance structure of the first embodiment of the present application;

[0026] Figure 4 This is a schematic diagram of the structure of the dust protection unit of the first embodiment of the present application;

[0027] Figure 5 This is a wiring arrangement diagram of the first embodiment of the present application, connecting the frame, the guide rod and the release layer;

[0028] Figure 6 This is a structural diagram of a guide rod, a connecting frame and a small electric extension rod in the first embodiment of the present application;

[0029] Figure 7 This is a schematic diagram of the installation of a translation reel according to a second embodiment of the present application;

[0030] Figure 8 This is a bottom view of the structure of the translation reel according to the second embodiment of the present application;

[0031] Fig. 9 This is a schematic diagram of the working state of the translation reel according to the second embodiment of the present application.

[0032] Description of the numbers in the figure:

[0033] 001, support frame; 1, roller No. 1; 2, roller No. 2; 3, roller No. 3; 4, calendering roller; 5, winding roller; 6, dust protection unit; 7, heat dissipation fan box; 8, winding rod; 9, rotating motor; 10, connecting frame; 11, gear; 12, small electric extension rod; 13, guide rod; 131, limiting wheel; 14, release layer; 15, driving motor; 16, moving plate; 17, electric telescopic rod; 18, movable rod. DETAILED DESCRIPTION

[0034] Two implementation modes of the present application are described in detail below with reference to the accompanying drawings.

[0035] The first implementation method:

[0036] Figure 1 A method for synthesizing a high thermal conductivity graphene structure film is shown, comprising the following steps:

[0037] S1, install the graphene film roll on the second roller 2, install the composite film roll on the third roller 3, and sleeve the double-sided film with a hollow cross-section design on the first roller 1;

[0038] S2, pulling the ends of the graphene roll, the composite film roll and the double-sided film roll with the same cross-sectional width through the middle of two calendering rollers 4 for calendering treatment;

[0039] S3. During the calendering process, the dust-avoiding unit 6 is used to pull and peel off the release layers 14 on the upper and lower surfaces of the double-sided adhesive tape and to spirally stagger the rolls, so as to avoid premature peeling of the release layers 14 and causing dust to adhere to the surface of the double-sided adhesive tape;

[0040] S31, winding the two release layers 14 on the surface of the double-sided film around the surfaces of the guide rods 13 arranged above and below the double-sided film respectively;

[0041] S32, rubbing the release layer 14 wound on the surface of the guide rod 13 to form a spiral winding structure, and then the tail end of the release layer 14 is located outside the double-sided tape and then vertically wound downward on the surface of the winding rod 8;

[0042] S4, the graphene structure film obtained by calendering is rolled up by the winding roller 5.

[0043] Specifically, Figure 2 It is shown that a high thermal conductivity graphene structure membrane synthesized by a synthesis method of a high thermal conductivity graphene structure membrane has a sandwich structure, the upper layer is a graphene layer, the middle layer is a double-sided adhesive with a hollow inside, which can achieve the purpose of bonding while reducing the use of glue, controlling costs and the interference of glue on the thermal conductivity of the graphene membrane, and the lower layer is a composite membrane layer (selected according to needs), so as to meet the processing requirements of different graphene structure membranes;

[0044] In the process of synthesizing the graphene structure film by the above-mentioned synthesis method, since the dust-avoiding unit 6 is close to the double-sided adhesive calendering position, the release layer 14 on the surface of the double-sided adhesive is peeled off near this position, so that the release layer 14 can remain on the surface of the double-sided adhesive for as long as possible, avoiding premature peeling to cause floating dust on the surface of the double-sided adhesive, thereby ensuring the stability of the bonding effect of the double-sided adhesive, and at the same time, it can also reduce the entry of floating dust and foreign matter into the interior of the graphene structure film during the synthesis process, thereby ensuring the high thermal conductivity of the graphene structure film;

[0045] After peeling off the release layer 14, the dust protection unit 6 can also assist in staggering the release layer 14 wound on the surface of the guide rod 13 to the outside of the double-sided tape so that it can be subsequently wound on the surface of the winding rod 8 in the lower area of ​​the support frame 001 to receive the roll, thereby avoiding long-term winding that causes the thickness of the release layer 14 on the surface of the guide rod 13 to be too large, causing squeezing of the graphene film and composite film above and below.

[0046] Figure 3-6It is shown that roller No. 2, roller No. 1 and roller No. 3 are installed on the material rack, and a support frame 001 is installed on one side of the material rack, and a support rod frame is installed on the surfaces of the support frames 001 close to each other. The dust protection unit 6 includes vertical plates installed on both sides of the support rod frame, and rotating motors 9 are installed on the surfaces of the two vertical plates. A connecting frame 10 is installed on the surfaces of the two vertical plates close to each other through a long rod, and guide rods 13 arranged up and down about the double-sided film are installed on the surfaces of the two vertical plates close to each other, and the upper and lower guide rods 13 are connected through a conveyor belt transmission. The output end of the rotating motor 9 is connected to the surface of one of the guide rods 13, and two limiting wheels 11 are arranged on the surface of the guide rods 13, and small electric extension rods 12 symmetrically arranged about the guide rods 13 are installed on the surfaces of each connecting frame 10 that are away from each other, and the power end of the small electric extension rod 12 is connected to a stroking block whose surface slides and fits on the surface of the guide rod 13, and the length of the stroking block is greater than the diameter value of the limiting wheel 11.

[0047] A release layer 14 is wound around the surface of each guide rod 13, wherein the winding area of ​​the release layer 14 on the surface of the guide rod 13 is in the middle of the two limiting wheels 11, and the release layer 14 is spirally wound on the surface of the guide rod 13, wherein the spiral winding amplitude of the release layer 14 on the surface of the upper guide rod 13 is smaller than the spiral winding amplitude of the release layer 14 on the surface of the lower guide rod 13.

[0048] Specifically, the initial state of the release layer 14 on the surface of the guide rod 13 is a spiral winding state. In the subsequent winding and receiving process, the small electric extension rods 12 on both sides of the guide rod 13 are started to make the extension lengths thereof different, and the release layer 14 obliquely wound on the surface of the guide rod 13 is constrained at two points, so that the subsequent release layer 14 wound on the surface of the guide rod 13 can be in a spiral winding state. Through the spiral winding, the release layer 14 originally peeled off horizontally can be changed to a vertical downward state after a horizontal displacement, and then the release layer 14 vertically downward is wound on the surface of the winding rod 8. In this process, the horizontal displacement can make the release layer 14 originally peeled off horizontally be able to pass through the composite film below and be smoothly wound on the surface of the winding rod 8 with a larger winding space below;

[0049] In addition, the spiral winding amplitudes of the release layers 14 on the upper and lower guide rods 13 are different, so the two release layers 14 on the upper and lower sides of the double-sided adhesive tape can be staggered and rolled up on the surface of the winding rod 8 .

[0050] Two calendering rollers 4 and a winding roller 5 are installed on the support rod frame, and the top tangent position of the winding roller 5 is at the same height as the horizontal line between the two calendering rollers 4. A heat dissipation fan box 7 is arranged on one side of the two calendering rollers 4, and the air outlets of the two heat dissipation fan boxes 7 are connected with the interior of the two calendering rollers 4. The interior of the calendering roller 4 is hollow and an air outlet is provided at the other end of the calendering roller 4.

[0051] Specifically, the No. 2 roller 2, the No. 1 roller 1 and the No. 3 roller 3 are respectively used to arrange the raw materials required for the graphene structure film, and cooperate with the calendering roller 4 and the winding roller 5 to form a complete calendering and winding device. During the calendering process, a heat dissipation fan box 7 is designed to dissipate heat and cool the calendering roller 4.

[0052] A winding unit is installed on the inner side of the support frame 001, wherein the winding unit includes a winding rod 8 installed inside the support frame 001, a servo motor is installed on the surface of one side of the support frame 001, and the output end of the servo motor is connected to one end of the winding rod 8, the number of spiral winding turns of the release layer 14 on the surface of the guide rod 13 is one turn, and the projection of the tail end of the upper release layer 14 after winding in the vertical direction is located on the outside of the double-sided film and is wound on the surface of the winding rod 8.

[0053] Specifically, the number of winding turns of the release layer 14 on the surface of the guide rod 13 is only one layer, so that the friction between the release layer 14 in a spirally wound state and the surface of the guide rod 13 can be controlled.

[0054] The sum of the lengths of the two guide rods 13 is smaller than the length of the long rod, and the length of the guide rod 13 is smaller than the horizontal distance between the connecting frame 10 and the vertical plate, and the limiting wheels 11 on the surfaces of the upper and lower guide rods 13 are staggered.

[0055] Specifically, the connecting frame 10 provides support for the installation of the small electric extension pole 12, and the staggered arrangement of the limiting wheels 11 for limiting with different spiral amplitudes also provides a control limiting effect.

[0056] The second implementation method:

[0057] Figure 7-8 The replacement structure of the winding unit is shown to be a translational winder, which includes two movable rods 18. A movable plate 16 is slidably connected to the inside of the support frame 001. A drive motor 15 is installed on the top of the movable plate 16. The output end of the drive motor 15 is connected to the movable rod 18. The movable rod 18 passes through and is inserted into the inside of the support frame 001. Electric telescopic rods 17 are installed on the surfaces of both sides of the support frame 001, and the power end of the electric telescopic rod 17 is connected to the bottom of the movable plate 16.

[0058] The sum of the lengths of the movable rods 18 is less than half of the cross-sectional width of the support frame 001 , and the two electric telescopic rods 17 move in the same direction when working.

[0059] Different from the first embodiment, this embodiment improves the problem that in the first embodiment, the surface of the winding rod 8 can only achieve winding in a single plane, which causes the winding thickness to increase rapidly. In this way, the effective winding length of the surface of the winding rod 8 is extended, and the winding time of the winding rod 8 is extended.

[0060] Specifically, during winding, the electric telescopic rod 17 is used to drive the movable plate 16 to move back and forth horizontally, so that the release layer 14 wound on the surface of the movable rod 18 is in a threaded structure, so that the horizontal amplitude of the winding on the surface of the movable rod 18 is increased (such as Fig. 9 shown).

[0061] In summary, when synthesizing a high thermal conductivity graphene structure film, the present application utilizes the cooperation of the guide rod 13, the limiting wheel 11, the small electric extension rod 12 and the winding rod 8 to peel off the release layer 14 on the surface of the double-sided adhesive near the calendering position, so as to avoid premature peeling that causes dust to adhere to the surface of the double-sided adhesive. At the same time, through the spiral winding method, the release layer 14 wound on the surface of the guide rod 13 after horizontal peeling can be displaced a small section to leave the cross-sectional range of the graphene film and then vertically wound to the surface of the winding rod 8, thereby achieving effective winding processing. The release layer 14 can also be threadedly wound using a translation winder to extend the effective winding length.

[0062] In view of current practical needs, the above-mentioned implementation mode adopted in this application is not limited to the scope of protection. Various changes made within the knowledge scope of technical personnel in this field without departing from the concept of this application still fall within the scope of protection of the present invention.

Claims

1. A method for synthesizing a high thermal conductivity graphene structure film, characterized in that: The following steps are included: S1, installing the graphene film roll on the second roller (2), installing the composite film roll on the third roller (3), and sleeve-mounting the double-sided film roll with a hollow cross-section design on the first roller (1); S2, pulling the ends of the graphene roll, the composite film roll and the double-sided film roll with the same cross-sectional width respectively through the middle of two calendering rollers (4) for calendering treatment; S3. During the calendering process, the dust-avoiding unit (6) is used to pull and peel off the release layers (14) on the upper and lower surfaces of the double-sided adhesive roll and to spirally stagger the roll to avoid premature peeling of the release layers (14) and causing dust to adhere to the surface of the double-sided adhesive roll; The second roller (2), the first roller (1) and the third roller (3) are mounted on a material rack, a support frame (001) is mounted on one side of the material rack, and a support rod frame is mounted on the surfaces of the support frame (001) close to each other, the dust protection unit (6) comprises vertical plates mounted on both sides of the support rod frame, a rotating motor (9) is mounted on the surfaces of the two vertical plates, a connecting frame (10) is mounted on the surfaces of the two vertical plates close to each other via a long rod, and guide rods (13) arranged up and down with respect to the double-sided film are mounted on the surfaces of the two vertical plates close to each other, The upper and lower guide rods (13) are connected by a conveyor belt transmission, the output end of the rotary motor (9) is connected to the surface of one of the guide rods (13), the surface of each guide rod (13) is provided with two limiting wheels (11), and each of the mutually diverging surfaces of the connecting frame (10) is provided with a small electric extension rod (12) symmetrically arranged with respect to the guide rod (13), and the power end of the small electric extension rod (12) is connected to a stroking block whose surface is slidably fitted on the surface of the guide rod (13), and the length of the stroking block is greater than the diameter value of the limiting wheel (11); S31, winding two release layers (14) on the surface of the double-sided film roll around the surfaces of guide rods (13) arranged above and below the double-sided film roll respectively; S32, the release layer (14) wound on the surface of the guide rod (13) is rubbed to form a spiral winding structure, and the tail end of the release layer (14) is located outside the double-sided adhesive tape and then vertically wound downward on the surface of the winding rod (8); S4, the graphene structure film obtained after calendering is rolled up by a winding roller (5).

2. The method for synthesizing a high thermal conductivity graphene structure film according to claim 1, characterized in that: Two calendering rollers (4) and a winding roller (5) are installed on the support rod frame, and the top tangent position of the winding roller (5) is at the same height as the horizontal line between the two calendering rollers (4). A heat dissipation fan box (7) is arranged on one side of the two calendering rollers (4), and the air outlets of the two heat dissipation fan boxes (7) are connected to the interior of the two calendering rollers (4). The interior of the calendering roller (4) is hollow and an air outlet is provided at the other end of the calendering roller (4).

3. The method for synthesizing a high thermal conductivity graphene structure film according to claim 1, characterized in that: A release layer (14) is wound around the surface of each guide rod (13), wherein the winding area of ​​the release layer (14) on the surface of the guide rod (13) is located between the two limiting wheels (11), and the release layer (14) is spirally wound around the surface of the guide rod (13), wherein the spiral winding amplitude of the release layer (14) on the surface of the upper guide rod (13) is smaller than the spiral winding amplitude of the release layer (14) on the surface of the lower guide rod (13).

4. The method for synthesizing a high thermal conductivity graphene structure film according to claim 3, characterized in that: A winding unit is installed on the inner side of the support frame (001), wherein the winding unit includes a winding rod (8) installed inside the support frame (001), a servo motor is installed on the surface of one side of the support frame (001), and the output end of the servo motor is connected to one end of the winding rod (8), the number of spiral winding turns of the release layer (14) on the surface of the guide rod (13) is one turn, and the projection of the tail end of the upper release layer (14) after winding in the vertical direction is located on the outside of the double-sided film and is wound on the surface of the winding rod (8).

5. The method for synthesizing a high thermal conductivity graphene structure film according to claim 4, characterized in that: The replacement structure of the winding unit is a translational winding device, which includes two movable rods (18). The support frame (001) is slidably connected to a movable plate (16). A driving motor (15) is installed on the top of the movable plate (16). The output end of the driving motor (15) is connected to the movable rod (18). The movable rod (18) penetrates and is inserted into the inside of the support frame (001). Electric telescopic rods (17) are installed on the two side surfaces of the support frame (001), and the power end of the electric telescopic rod (17) is connected to the bottom of the movable plate (16).

6. The method for synthesizing a high thermal conductivity graphene structure film according to claim 5, characterized in that: The sum of the lengths of the movable rods (18) is less than half the cross-sectional width of the support frame (001), and the two electric telescopic rods (17) move in the same direction when in operation.

7. The method for synthesizing a high thermal conductivity graphene structure film according to claim 1, characterized in that: The sum of the lengths of the two guide rods (13) is smaller than the length of the long rod, and the length of the guide rod (13) is smaller than the horizontal distance between the connecting frame (10) and the vertical plate, and the limiting wheels (11) on the surfaces of the upper and lower guide rods (13) are staggered.

8. A high thermal conductivity graphene structure film synthesized according to the method for synthesizing a high thermal conductivity graphene structure film according to any one of claims 1 to 7.

Citation Information

Cited By

  • Release film re-pasting method capable of avoiding graphene damage

    CN121573671A