Plastic injection part thread shaping method

By using plastic shaping tool to correct the internal thread of injection molded parts and slowly cool it during baking, the thread problem caused by deformation during cooling of injection molded parts is solved, the consistency of threads and load-bearing strength are improved, valve leakage is avoided, and industrial Production quality control requirements.

CN118906509APending Publication Date: 2024-11-08SHANGHAI ZHILIN PRECISION MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411142382.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing injection molding process, plastic parts may shrink and deform non-uniformly during cooling, resulting in thread deformation, reducing the load-bearing strength of the connecting threads and causing valve leakage.

Method used

The internal threads of injection molded parts are corrected using plastic shaping tools, screwed into place by external threads, and slowly cooled during baking to release thermal stress, and then detected and ultrasonic cleaning is performed to ensure consistency of thread size.

Benefits of technology

Effectively correct the dimensional deviation of the internal thread of injection molded parts, improve the consistency of threads and load-bearing strength, avoid valve leakage, and meet the quality control needs of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906509A_ABST
    Figure CN118906509A_ABST
Patent Text Reader

Abstract

The invention discloses a reshaping method for threads of an injection-molded part, internal threads of the injection-molded part are reshaped through a reshaping tool, and external threads are arranged on the circumferential surface of the reshaping tool. The shaping tool is screwed into the through hole of the injection molding part; then, the injection molding part is put into a baking furnace to be heated, and after heating is finished, the injection molding part is naturally cooled along with the furnace; after the injection molding part is taken out of the baking furnace, the shaping tool is dismounted; detecting the size of the internal thread of the injection molding part; and then, the qualified plastic parts are put into an ultrasonic cleaning machine to be cleaned, then natural drying is conducted, and finally warehousing is conducted. By using the shaping tool, the dimensional deviation of the inner diameter of the internal thread of the injection molding part is effectively corrected, the consistency of the shaped injection molding part is ensured, a reliable guarantee is provided for subsequent use and assembly, and the requirement for quality control of industrial production is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of parts processing technology, and in particular to a shaping method for injection molded parts threads. Background Art

[0002] Ultrapure pipelines transport toxic, strong acid, strong alkali and other chemical media that are harmful to human contact. The valves and pipe fittings in the pipeline system are required to have reliable sealing and long service life. At present, the components of PFA valves are injection molded. The existing injection molding process is to first heat and melt the plastic particles, and then inject them into the mold through an injection molding machine. When the raw materials are solidified in the mold, the mold is opened to take out the parts. Since the plastic material may shrink and deform unevenly during the cooling process, the plastic parts will deform and lose roundness, resulting in thread deformation. The thread deformation reduces the limited load-bearing area of ​​the connecting thread, thereby reducing the load-bearing strength of the connecting thread, further resulting in insufficient valve thread connection force, causing the valve to leak. Summary of the invention

[0003] Based on this, in order to solve the above problems, the present invention provides a method for shaping the threads of injection molded parts.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for shaping the threads of an injection molded part, wherein the internal threads on the inner wall of a through hole of the injection molded part are shaped by a shaping tool, and the peripheral surface of the shaping tool has an external thread that can correct the internal threads of the injection molded part. The shaping method is as follows;

[0006] Step 1: Take an injection molded part with internal threads from the injection molding machine, and screw the external threads of the shaping tool into the internal threads of the injection molded part until it is screwed into place;

[0007] Step 2: Place the injection molded parts screwed with the shaping tooling into a baking furnace for heating. After heating, cool them naturally along with the furnace.

[0008] Step 3: Take out the cooled injection molded parts from the baking oven and remove the shaping tooling;

[0009] Step 4, detecting the size of the internal thread of the injection molded part;

[0010] Step 5: Place qualified plastic parts into an ultrasonic cleaning machine for cleaning, then dry them naturally and finally put them into storage.

[0011] In a specific embodiment of the present invention; in step 1, the screwing into place refers to screwing the upper end surface of the shaping tooling until it is flush with the upper end surface of the injection molded part.

[0012] In a specific embodiment of the present invention; in step 2, the heating temperature is 100°C and the heating time is 2-3 hours.

[0013] In a specific embodiment of the present invention: in step 2, the cooling time of the injection molded part is 4 hours.

[0014] In a specific embodiment of the present invention: during testing, the injection molded part is qualified if the size deviation of the internal thread is within 0-0.19 mm.

[0015] In a specific implementation manner of the present invention: the length of the external thread of the shaping tool is longer than the length of the internal thread of the injection molded part.

[0016] In a specific implementation manner of the present invention: the shaping tool further has a clamping portion extending downward, and the rotating wrench clamps the clamping portion to screw the external thread of the shaping tool into the internal thread of the injection molded part.

[0017] In a specific implementation manner of the present invention: the shaping tool is made of aluminum alloy or stainless steel.

[0018] In summary, in the present invention, by using shaping tooling, the dimensional deviation of the inner diameter of the internal thread of the injection molded part is effectively corrected, the consistency of the injection molded part after shaping is ensured, a reliable guarantee is provided for subsequent use and assembly, and the quality control requirements of industrial production are met. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The present invention will be further described below in conjunction with the accompanying drawings.

[0020] Figure 1 The invention is a structural schematic diagram of a method for shaping threads of an injection molded part. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] See also Figure 1 As shown, the present invention is a method for shaping the threads of injection molded parts, wherein the internal threads 13 on the inner wall of the through hole 12 of the injection molded part 11 are shaped by a shaping tool 10, and the peripheral surface of the shaping tool 10 has an external thread 14 that can correct the internal threads 13 of the injection molded part 11.

[0023] The shaping method is as follows;

[0024] Step 1: Take an injection molded part 11 with internal threads from the injection molding machine, and screw the external threads 14 of the shaping tool 10 into the internal threads 13 of the injection molded part 11 until it is screwed into place.

[0025] In this step, when the shaping tool 10 is screwed until the upper end surface of the shaping tool 10 is flush with the upper end surface of the injection molded part 11, the internal thread of the injection molded part 11 is screwed into place with the external thread of the shaping tool 10. In this way, intuitive assembly instructions can be provided to the assembler without the need for additional measuring or positioning tools, simplifying the assembly process.

[0026] The shaping tool 10 has a downwardly extending clamping portion 15. The clamping portion 15 of the shaping tool 10 can be clamped with a rotary wrench to screw the shaping tool 10 into the through hole 12 of the injection molded part 11.

[0027] Step 2: Put the injection molded part 11 screwed with the shaping tool 10 into a baking furnace for heating. After the heating is completed, it is naturally cooled in the furnace.

[0028] In this step, the injection molded part 11 is heated in a baking furnace at a temperature of 100°C for 2-3 hours. After heating, the injection molded part is placed in a baking furnace and cooled in the furnace for 4 hours. During the heating process, the injection molded part will produce certain thermal stress and deformation due to the high temperature and high pressure. Furnace cooling can slowly reduce the temperature of the injection molded part, help release the internal stress of the part, and avoid defects such as deformation, cracks, pores, and scratches of the injection molded part caused by rapid cooling and heating.

[0029] Step 3: Take the cooled injection molded part 11 out of the baking oven, and then remove the shaping tool 10.

[0030] Step 4: Detect the inner diameter of the internal thread 13 of the injection molded part.

[0031] In this step, when testing, the dimensional deviation of the internal thread of the injection molded part is within 0-0.19mm and it is a qualified product.

[0032] Step 5: Then, put the qualified plastic parts into the ultrasonic cleaning machine for cleaning, then dry naturally and finally put them into storage.

[0033] In this embodiment, the length of the external thread 14 of the shaping tool 10 is longer than the length of the internal thread 13 of the injection molded part 11 .

[0034] A first stop step 121 is provided on the upper portion of the through hole 12 of the injection molded part 11. A second stop step 101 is provided on the upper portion of the shaping tool 10 to cooperate with the first stop step 121. Thus, the precise position of the shaping tool 10 in the injection molded part 11 is ensured by the mutual cooperation between the second stop step 101 and the first stop step 121. At the same time, the screwing depth of the shaping tool 10 is limited to prevent the internal damage or deformation of the injection molded part 11 that may be caused by excessive screwing.

[0035] In this embodiment, the shaping tool 10 is made of aluminum alloy or stainless steel.

[0036] Select 4 injection molded parts, and test the internal thread sizes of the 4 injection molded parts before and after shaping;

[0037] Test results:

[0038] 1. Table 1 shows the internal thread size data of 4 injection molded parts before shaping (unit: mm)

[0039] Table 1

[0040]

[0041] As can be seen from Table 1, the internal thread size of the injection molded parts ranges from 62.04mm to 62.23mm, with a deviation of 0.19mm. Among the four injection molded parts, the maximum deviation is 0.6mm and the minimum deviation is 0.48mm, which shows that none of them meet the requirements.

[0042] 2. Table 2 shows the internal thread size data of 4 injection molded parts after shaping (unit: mm)

[0043] Table 2

[0044]

[0045] It can be seen from Table 2 that the internal thread sizes of the four injection molded parts after shaping have a maximum deviation of 0.19 mm and a minimum deviation of 0.1 mm, which shows that they all meet the requirements.

[0046] In summary, in the present invention, by using shaping tooling, the dimensional deviation of the inner diameter of the internal thread of the injection molded part is effectively corrected, the consistency of the injection molded part after shaping is ensured, a reliable guarantee is provided for subsequent use and assembly, and the quality control requirements of industrial production are met.

[0047] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for shaping the thread of an injection molded part, wherein the internal thread on the inner wall of a through hole of the injection molded part is shaped by a shaping tool, characterized in that: The peripheral surface of the shaping tool is provided with external threads capable of correcting the internal threads of the injection molded parts, and the shaping method is as follows; Step 1: Take an injection molded part with internal threads from the injection molding machine, and screw the external threads of the shaping tool into the internal threads of the injection molded part until it is screwed into place; Step 2: Place the injection molded parts screwed with the shaping tooling into a baking furnace for heating. After heating, cool them naturally along with the furnace. Step 3: Take out the cooled injection molded parts from the baking oven and remove the shaping tooling; Step 4, detecting the size of the internal thread of the injection molded part; Step 5: Place qualified plastic parts into an ultrasonic cleaning machine for cleaning, then dry them naturally and finally put them into storage.

2. The method for shaping the thread of an injection molded part according to claim 1, characterized in that: In step 1, screwing into place refers to screwing the upper end surface of the shaping tooling until it is flush with the upper end surface of the injection molded part.

3. The method for shaping the thread of an injection molded part according to claim 1, characterized in that: In step 2, the heating temperature is 100° C. and the heating time is 2-3 hours.

4. The method for shaping the thread of an injection molded part according to claim 1, characterized in that: The cooling time for the molded parts in step 2 was 4 hours.

5. The method for shaping the thread of an injection molded part according to claim 1, characterized in that: During testing, the dimensional deviation of the internal thread of the injection molded parts is within 0-0.19mm and is considered a qualified product.

6. The method for shaping the thread of an injection molded part according to claim 2, characterized in that: The length of the external thread of the shaping tool is longer than the length of the internal thread of the injection molded part.

7. The method for shaping the thread of an injection molded part according to claim 1, characterized in that: The shaping tool also has a clamping portion extending downward, and the rotating wrench clamps the clamping portion to screw the external thread of the shaping tool into the internal thread of the injection molded part.

8. The method for shaping the thread of an injection molded part according to claim 1, characterized in that: The shaping tool is made of aluminum alloy or stainless steel.