High-strength and high-impact polypropylene / metal composite material as well as preparation method and application thereof
Through the laminated hot pressing technology of polypropylene sheet and metal material, combined with specific polymer combinations and nucleating agents, the high energy consumption and complex process problems in the preparation technology of traditional polymer/metal composite materials are solved, and high strength is achieved , polypropylene/metal composite material with high impact resistance and excellent interlayer peel strength.
Patent Information
- Application Number
- CN202310507611.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-07
AI Technical Summary
Traditional polymer/metal composite preparation technology has problems such as high energy consumption, complex process and release of volatile pollution sources, and is not suitable for the bonding of non-polar polyolefin materials.
Polypropylene/metal composite materials are prepared by layering polypropylene sheets and metal materials, using homopolypolypropylene and impact copolymerized polypropylene compositions, combined with thermal bonding enhancer and β-crystal nucleating agent, to form The BAB' structure of layer A and layer B achieves efficient bonding of the polypropylene cladding layer and the metal material.
The high strength, high impact resistance and excellent interlayer peeling strength of polypropylene/metal composite materials are achieved, which reduces the hot pressing temperature and energy consumption, simplifies the process and improves production efficiency.
Smart Images

Figure BDA0004216469040000221 
Figure BDA0004216469040000231
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polyolefin / metal composite materials, and more particularly to a high-strength and high-impact polypropylene / metal composite material and a preparation method and application thereof. Background Art
[0002] Polymer / metal composites have the characteristics of high strength-to-weight ratio, good impact resistance and corrosion resistance, and are widely used in the automotive manufacturing industry, sports equipment manufacturing industry, electrical manufacturing industry and military field.
[0003] Due to the great differences in the physical and chemical properties of polymers and metals, the bonding of polymers to metals, especially the bonding of non-polar polyolefin polymers to metals, is challenging. Traditional techniques for preparing polymer / metal composites include activated metal surface polymerization, insert injection molding, 3D printing, mechanical fastening, adhesive bonding and other techniques. For example, CN 114096618A proposes to improve the adhesion between polyamide and metal by treating the metal surface with a solution of triazine thiol derivatives, and to prepare polyamide / metal composites by insert injection molding, coextrusion, or powder coating. CN 112974853 A discloses a method for preparing metal polymer composites by filling plastic powder into directly formed 3D printed metal holes.
[0004] Traditional polymer / metal composite material preparation technology has the disadvantages of high energy consumption, complex process, release of volatile pollutants, etc., and traditional preparation technology is not always applicable to non-polar polyolefins. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a high-strength and high-impact polypropylene / metal composite material and its preparation method and application. The present invention obtains a polypropylene / metal composite material by laminating and hot pressing a polypropylene sheet and a metal material layer (preferably a metal mesh), which has the advantages of simple molding process, safety and environmental protection. The polypropylene / metal composite material has excellent mechanical properties and good interlayer peeling strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the interlayer peeling strength of the obtained polypropylene / metal composite material is still high.
[0006] The first aspect of the present invention is to provide a polypropylene / metal composite material having a laminated structure, comprising at least one metal material layer and a plurality of polypropylene coating layers correspondingly coated on each metal material layer, wherein the metal material layer is provided with a plurality of through holes; each polypropylene coating layer is the same or different, and each comprises at least one layer of polypropylene sheet and / or at least one layer of polypropylene fabric woven from polypropylene sheets; wherein the polypropylene sheet comprises layer A and layers B and B' located on both sides of layer A, and the structure is BAB';
[0007] Wherein, layer A contains a polypropylene composition A, and the polypropylene composition A includes homopolymer polypropylene a and impact copolymer polypropylene b; layer B is the same as or different from layer B', and each correspondingly contains a polypropylene composition B and a polypropylene composition B', wherein the polypropylene composition B and the polypropylene composition B' each include a random copolymer polypropylene x and a thermal bonding enhancer y; wherein the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B', and preferably the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B, and the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B' are each greater than or equal to 5°C, preferably greater than or equal to 10°C, and more preferably greater than or equal to 20°C.
[0008] In a preferred embodiment of the present invention, the polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.
[0009] According to the present invention, the film layers B and B' on both sides of the film layer A are the same or different. In a preferred embodiment of the present invention, the film layers B and B' on both sides of the film layer A are the same.
[0010] The present invention does not limit the thickness of the polypropylene sheet, and can be selected in a wide range according to its practical application field. Preferably, the thickness of the polypropylene sheet can be 10-1000 μm, preferably 30-500 μm, and more preferably 50-300 μm.
[0011] According to the present invention, the thickness of the film layers A, B, B' can be controlled by the melt pump of the extruder during the processing.
[0012] In a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b.
[0013] In a preferred embodiment of the present invention, based on the total weight of the polypropylene compositions B and B', the polypropylene compositions B and B' each comprise 70-99 wt% of random copolymer polypropylene x and 1-30 wt% of thermal adhesion enhancer y; preferably, the polypropylene compositions B and B' each comprise 80-90 wt% of random copolymer polypropylene x and 10-20 wt% of thermal adhesion enhancer y.
[0014] In a preferred embodiment of the present invention, based on the total thickness of the polypropylene sheet, the thickness of the film layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.
[0015] In a preferred embodiment of the present invention, the melting point of the polypropylene composition A is greater than the melting points of the polypropylene compositions B and B'.
[0016] In a preferred embodiment of the present invention, the melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in each of the polypropylene compositions B and B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees.
[0017] In a preferred embodiment of the present invention, the homopolypropylene a has at least one of the following characteristics: the melting point of the homopolypropylene a is 160-170° C.; and / or,
[0018] The homopolypropylene a has a melt flow rate of 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min at 230° C. and 2.16 kg load; and / or
[0019] The isotacticity (mm) of the homopolypropylene a is not less than 96%.
[0020] In a preferred embodiment of the present invention, the impact-resistant copolymer polypropylene b has at least one of the following characteristics: the melting point of the impact-resistant copolymer polypropylene b is 150-170° C.; and / or,
[0021] The monomer of the impact-resistant copolymer polypropylene b and propylene copolymer is ethylene or butene, and the content of ethylene or butene is 2-50%wt, preferably 3-20%wt, and more preferably 5-15%wt, and / or,
[0022] The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or,
[0023] The impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 (Test conditions: 23℃).
[0024] According to the research conducted by the inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene composition A are within the above preferred ranges, the impact-resistant copolymerized polypropylene b in the composition can absorb impact energy well, meet the requirements of impact performance, and make the sheet have good impact performance. At the same time, since the macromolecular segments in the homopolymerized polypropylene a are relatively regular, crystallization occurs during the preparation of the sheet, so the sheet also has good tensile properties.
[0025] In a preferred embodiment of the present invention, the random copolymer polypropylene x has at least one of the following characteristics: the melting point of the random copolymer polypropylene x is 120-140° C.; and / or,
[0026] The random copolymer polypropylene x has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or,
[0027] The random copolymer polypropylene x is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer or a propylene-ethylene binary copolymer.
[0028] In a preferred embodiment of the present invention, the melt flow rate of the thermal adhesion enhancer y at 190° C. and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min.
[0029] The thermal adhesion enhancer y is selected from one or more of polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA and petroleum resin; preferably,
[0030] The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or alpha olefin; further preferably, the alpha olefin is a C4-C12 alpha olefin, more preferably 1-butene and / or 1-octene; and / or,
[0031] The petroleum resin is a hydrogenated petroleum resin of C5 and / or C9, preferably having a softening point of 100-150° C.; more preferably, the petroleum resin is a cyclopentadiene type resin.
[0032] According to the research conducted by the present inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene compositions B and B' are within the preferred range, the low melting point random copolymer polypropylene x and thermal bonding enhancer y in the composition can significantly reduce the hot pressing temperature and broaden the hot pressing temperature window, and the thermal bonding enhancer y provides the sheet with good bonding properties, which can further improve the interlayer peeling strength.
[0033] In a preferred embodiment of the present invention, the layer A further contains a β-crystal nucleating agent; preferably,
[0034] The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or,
[0035] Based on 100 parts by weight of the total amount of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight. For example, the content of the β-crystal nucleating agent may be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5 parts by weight.
[0036] The inventors of the present invention surprisingly found that the obtained polypropylene sheet is subjected to hot pressing to obtain a polypropylene / metal composite material, and the polypropylene / metal composite material has more excellent mechanical properties and better interlayer peeling strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the interlayer peeling strength of the obtained polypropylene / metal composite material is higher.
[0037] The BAB' sheet structure of the polypropylene sheet can be prepared by a variety of methods. In a preferred embodiment of the present invention, the BAB' sheet structure of the polypropylene sheet is obtained by co-extruding components including a polypropylene composition A and polypropylene compositions B and B'. Preferably, the method comprises co-extruding, casting or calendering, stretching, and slitting the polypropylene composition A, the polypropylene composition B, and the B' according to the BAB' structure to obtain the polypropylene sheet.
[0038] The conditions and equipment for melt blending of the polypropylene composition A are the same as those for melt blending of polyolefins in the prior art. Preferably, the melting temperature is 150-170° C., and the equipment is preferably a twin-screw extruder.
[0039] In a preferred embodiment of the present invention, the preparation of the polypropylene composition B comprises melt blending the components including the random copolymer polypropylene x and the thermal adhesion enhancer y. The conditions and equipment for melt blending of the polypropylene composition B adopt the conditions and equipment for melt blending of polyolefins in the prior art, preferably, the melting temperature is 110-150° C., and the equipment is preferably a twin-screw extruder.
[0040] The selection range of the co-extrusion and casting temperatures is relatively wide. In a preferred embodiment of the present invention, in step (1), the co-extrusion and casting temperatures are independently selected from 200-240°C; the temperature of the calendering roll is 50-70°C.
[0041] The selection range of stretching conditions is relatively wide. In a preferred embodiment of the present invention, the stretching conditions include: the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is 90-165°C, preferably 90-140°C, and further preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.
[0042] In a preferred embodiment of the present invention, the longitudinal tensile strength of the stretched polypropylene sheet is greater than or equal to 30 MPa, more preferably 30 MPa-1 GPa; most preferably 300-800 MPa.
[0043] The polypropylene fabric is a three-dimensional polypropylene fabric obtained by weaving the polypropylene sheet mentioned above; preferably, the polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.
[0044] In order to facilitate weaving, the polypropylene sheet is preferably cut into polypropylene sheets with a width of 2-5 mm, and then woven to obtain the polypropylene fabric.
[0045] In a preferred embodiment of the present invention, the polypropylene / metal composite material is prepared by stacking multiple layers of the polypropylene sheets and / or polypropylene fabrics and the metal material layers in sequence, fusing them by hot pressing, and then cooling and shaping.
[0046] In a preferred embodiment of the present invention, the total number of layers of the polypropylene sheet and / or polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers.
[0047] In a preferred embodiment of the present invention, the surface density of the polypropylene / metal composite material is greater than or equal to 600 g / m 2 , more preferably 600-35000g / m 2 ; Most preferably 800-12000g / m 2 .
[0048] In a preferred embodiment of the present invention, the longitudinal tensile strength of the polypropylene / metal composite material is greater than or equal to 280 MPa, preferably greater than or equal to 300 MPa.
[0049] In a preferred embodiment of the present invention, the polypropylene / metal composite material has at least one of the following characteristics:
[0050] Longitudinal tensile strength ≥280Mpa, preferably ≥300Mpa;
[0051] Interlayer peel strength ≥1N / mm, preferably ≥1.1N / mm;
[0052] The tensile strength is measured according to the method specified in GB / T1040.1-2018, and the interlayer peel strength is measured according to the method specified in GB / T2358-98. The corresponding specimens in the above two tests are the standard specimens required in the above-mentioned test standards.
[0053] When the polypropylene / metal composite material is obtained by hot pressing 24 layers of polypropylene fabrics and 1 layer of metal mesh, and has a thickness of about 1.79 mm, the drop weight impact strength is ≥280J, preferably ≥300J.
[0054] The drop weight impact strength is measured according to the method specified in GB / T14153-1993, and the thickness of the sample is the thickness of the prepared product.
[0055] According to the present invention, as long as the metal material layer is provided with a plurality of through holes, the polypropylene coating layers on both sides of the metal material layer are in contact with each other to realize the present invention. The present invention does not require any special distribution form and shape of the holes on the metal material layer. In order to further improve the mechanical properties of the polypropylene / metal composite material and have better interlayer peeling strength, the metal material layer is preferably a metal mesh. The metal mesh includes but is not limited to a stainless steel mesh, a carbon steel mesh, a galvanized steel mesh and an alloy mesh.
[0056] Preferably, the metal mesh is selected from at least one of a stainless steel mesh, a carbon steel mesh, a galvanized steel mesh and an alloy mesh.
[0057] Preferably, the diameter of the metal wire in the metal mesh is 0.02-2 mm, preferably 0.03-1 mm; and / or the number of holes is 10-1000 meshes, preferably 50-500 meshes. In this preferred embodiment, the obtained polypropylene / metal composite material has further better interlayer peeling strength.
[0058] Preferably, the number of the metal material layers is greater than or equal to 1 layer, more preferably 1-50 layers, and most preferably 1-20 layers.
[0059] In a more preferred embodiment of the present invention, the polypropylene / metal composite material is prepared by laminating multiple layers of the polypropylene sheets and / or polypropylene fabrics described above and the metal mesh described above through hot pressing; preferably, the multiple layers of polypropylene sheets and / or multiple layers of polypropylene fabrics are stacked from top to bottom along their respective machine directions at 0-90°; preferably, the number of layers is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers. The metal mesh is placed in the middle of the polypropylene sheet and / or polypropylene fabric; the number of metal mesh layers is greater than or equal to 1 layer, more preferably 1-50 layers; most preferably 1-20 layers. The surface density of the polypropylene / metal composite material is greater than or equal to 600g / m 2, more preferably 600-35000g / m 2 ; Most preferably 800-12000g / m 2 In a preferred embodiment of the present invention, the polypropylene composition A contained in each layer of the stacked polypropylene fabrics may be the same or different, and the polypropylene fabric A contained in each layer may be independently selected, and preferably the polypropylene composition A of each layer is the same.
[0060] In a more preferred embodiment of the present invention, the polypropylene / metal composite material comprises a polypropylene composite material matrix formed by stacking all polypropylene coating layers and at least one metal material layer arranged in the polypropylene composite material matrix; the polypropylene composite material matrix comprises a plurality of polypropylene sheet unit groups stacked in sequence; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n;
[0061] Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i ,
[0062] The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.
[0063] In a more preferred embodiment of the present invention, the polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' iThe difference in melting points is 5°C or more, preferably 10°C or more, more preferably 20°C or more, and even more preferably 20-60°C.
[0064] Through research, the inventors unexpectedly discovered that when the average melting point of all outer layers in the i-th group is greater than the average melting point of all outer layers in the i-1-th group, compared with the case where the two are equal, a better technical effect is achieved, that is, the polypropylene / metal composite material has further excellent mechanical properties and further better interlayer peel strength.
[0065] More preferably, the difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1-th group is the same or different, and is 1-40°C, preferably 1-10°C, and more preferably 1-5°C.
[0066] According to the present invention, the total number of stacked polypropylene sheet unit groups is 2n-1. The present invention has a wide selection range for the total number of stacked polypropylene sheet unit groups, preferably, 2≤n≤100, preferably, 2≤n≤50, and further preferably, 2≤n≤30.
[0067] According to the present invention, the selection range of the number of polypropylene sheet units included in each polypropylene sheet unit group is relatively wide. In a preferred embodiment of the present invention, each polypropylene sheet unit group independently includes 1 to 10, preferably 1 to 5, more preferably 1 to 3 identical or different polypropylene sheet units, more preferably 1 polypropylene sheet unit. Preferably, the number of polypropylene sheet units included in each polypropylene sheet unit group is the same.
[0068] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, more preferably within ±1°C of the average melting point of all outer layers in the group.
[0069] In the embodiment where each polypropylene sheet unit group includes only one polypropylene sheet unit, for example, the structure of the polypropylene composite material can be B from bottom to top. n A n B' n ……B i A i B' i ...B2A2B'2, B1A1B'1, B2A2B'2...B i A i B' i ……B n A n B' n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n.
[0070] In the embodiment where each polypropylene ply unit group includes 2 or more polypropylene ply units, for example, the structure of the i-th polypropylene ply unit group is B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip The structure of the polypropylene composite material can be sequentially as follows from bottom to top: n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A 12 B' 12 ……B 1j A 1j B' 1j )(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……Bip A ip B' ip )……(B n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq ), the total number of stacked polypropylene sheet units is j+2k+...2p+...2q; j, k, p, q are each independently an integer not less than 2, preferably an integer from 2 to 10, more preferably from 2 to 5, and more preferably from 2 to 3.
[0071] The arrangement of the metal material layer in the polypropylene composite material matrix can be selected in a wide range. Preferably, the number of polypropylene sheet units on both sides of each metal material layer is close. For example, when the metal material layer is a single layer, the metal material layer is preferably arranged at a relatively close position to the middle of the polypropylene composite material matrix. Preferably, the difference in the number of polypropylene sheet units on both sides of each metal material layer is less than or equal to 5, preferably less than or equal to 2.
[0072] The second aspect of the present invention is to provide a method for preparing the polypropylene / metal composite material described in the first aspect, comprising stacking multiple layers of the polypropylene sheets and / or polypropylene fabrics and the metal material layers in sequence, fusing them by hot pressing, and then cooling and shaping to prepare the polypropylene / metal composite material.
[0073] Preferably, the multiple layers of polypropylene sheets are stacked from top to bottom in an angle of 0-90° along their respective machine directions.
[0074] Preferably, the multiple layers of polypropylene fabric are stacked from top to bottom with an angle of 0-90 degrees between the warp directions.
[0075] Preferably, the total number of layers of the multi-layer polypropylene sheets and / or multi-layer polypropylene fabrics is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers.
[0076] Preferably, the number of the metal material layers is greater than or equal to 1 layer, more preferably 1-50 layers, and most preferably 1-20 layers.
[0077] In a preferred embodiment of the present invention, the temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C.
[0078] Preferably, the pressure of the hot pressing fusion is 2-10Mpa.
[0079] Preferably, the preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s.
[0080] Preferably, the cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s.
[0081] In a preferred embodiment of the present invention, adjacent layers of the polypropylene sheet laminate are placed at 0-90° along respective machine directions, wherein the machine direction is the stretching direction (MD).
[0082] In a preferred embodiment of the present invention, adjacent layers of the polypropylene fabric laminate are placed at an angle of 0-90° along the warp direction.
[0083] The metal mesh is placed between the polypropylene sheet and / or the polypropylene fabric.
[0084] In a more preferred embodiment of the present invention, the method for preparing the high-strength and high-impact polypropylene / metal composite material comprises the following steps:
[0085] Step a: co-extrude the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B' according to the BAB' structure and cast or calender to obtain a polypropylene co-extruded sheet; preferably, the extrusion casting or calendering temperature is 200-240° C., and the temperature of the calendering roller is 50-70° C.;
[0086] Step b: stretching the coextruded polypropylene sheet at a certain temperature to obtain a stretched polypropylene sheet; preferably, the stretching temperature is 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-15 times, preferably 2-9 times.
[0087] Step c: cutting the polypropylene stretched sheet to prepare polypropylene flat strips, and weaving the flat strips to prepare polypropylene fabrics; preferably, the width of the polypropylene flat strips is 2-5 mm, and the polypropylene fabrics include plain weave, twill, satin weave or other three-dimensional polypropylene fabrics;
[0088] Step d: laminating the polypropylene sheet and / or the polypropylene fabric and the metal mesh by hot pressing and fusing, and then cooling and shaping to form a polypropylene / metal composite material; preferably, in the step d, the hot pressing conditions are: hot pressing temperature 115-170°C, preferably 115-159°C, and more preferably 140-159°C; hot pressing pressure 2-10Mpa, preheating time 5-600s, hot pressing time 1-600s, preferably 10-500s, cooling pressure 2-8Mpa, cooling time 30s-700s; preferably, adjacent polypropylene fabrics in the polypropylene composite material can be placed at 0-90° between the warp and the warp, and the metal mesh is placed between the polypropylene sheet and / or polypropylene fabric.
[0089] According to some embodiments of the present invention, in step c, a high-speed slitting machine with multiple blades can be used for cutting to obtain an oriented polypropylene flat ribbon with a width of 2-5 mm; a commercial weaving machine is used to weave the oriented flat ribbon according to the designed fabric structure to obtain plain, twill, satin or other three-dimensional polypropylene fabrics.
[0090] According to the present invention, in a preferred specific embodiment, the pressure is preferably maintained continuously during the hot pressing and cooling process without being reduced. The hot pressing process is carried out continuously, and preferably a continuous hot pressing composite material molding equipment consisting of a preheating machine, a crawler-type continuous flat hot press, a crawler-type continuous flat cooling press, a sheet cutting machine and a sheet stacking machine arranged in sequence is used; preferably, the crawler-type continuous flat hot press has a preheating unit, an independent heating and pressurizing unit, an air cooling unit and a lifting mechanism.
[0091] During the preparation, the polypropylene sheet and / or the polypropylene fabric and the metal mesh are sequentially stacked and then preheated by a preheater. The preheated samples are sequentially hot-pressed and fused by a crawler-type flat hot press, and then cooled and shaped by a crawler-type continuous flat cooling press to form a polypropylene / metal composite material, i.e., a stacked hot-pressed product. Afterwards, the sheet is sliced by a sheet cutter as needed, and the hot-pressed products are stacked and arranged by a sheet stacker. The hot-pressing temperature is controlled by a preheating unit, an independent heating and pressurizing unit, and an air-cooling unit in the crawler-type flat hot press, and the hot-pressing pressure is controlled by a lifting mechanism. According to the research of the inventors, when the preparation process parameters are within the preferred range, the polypropylene / metal composite material is preferably prepared using the equipment, and the polypropylene / metal composite material has better tensile strength, impact resistance and interlayer peeling strength.
[0092] The third aspect of the present invention is to provide an application of the polypropylene / metal composite material described in the first aspect and the polypropylene / metal composite material prepared by the preparation method described in the second aspect in the fields of sports protection, automobile manufacturing, military materials and consumer goods.
[0093] According to a specific embodiment of the present invention, the material fields include luggage and transportation industry, shoemaking industry, automobile manufacturing industry, sports equipment manufacturing industry, audio equipment manufacturing industry and military field.
[0094] Compared with the prior art, the present invention has the following beneficial effects:
[0095] (1) The polypropylene / metal composite material of the present invention has good tensile strength, impact resistance and interlayer peeling strength;
[0096] The polypropylene / metal composite material has the following characteristics:
[0097] The longitudinal tensile strength is ≥280Mpa, preferably ≥300Mpa; the interlayer peel strength is ≥1N / mm, preferably ≥1.1N / mm; when the polypropylene / metal composite material is obtained by hot pressing 24 layers of polypropylene fabric and 1 layer of metal mesh, and the thickness is about 1.79mm, the drop weight impact strength is ≥280J, preferably ≥300J.
[0098] (2) The polypropylene / metal composite material of the present invention can be prepared at a relatively low hot pressing temperature and within a relatively wide hot pressing temperature range, which effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high-temperature operation. At the same time, when prepared at a relatively low hot pressing temperature, it still has good interlayer peeling strength.
[0099] (3) The preparation method can reduce the hot pressing operation time, while improving production efficiency and reducing production energy consumption.
[0100] (4) The present invention reduces the hot pressing temperature and expands the hot pressing temperature range to 50°C; it effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high temperature operation. DETAILED DESCRIPTION
[0101] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0102] In the following examples and comparative examples:
[0103] The extrusion calender and stretching equipment were purchased from Tianjin Hengrui Company, and the model was HRPC-800 three-layer co-extrusion plastic stretching sheet production line.
[0104] The properties of the polypropylene / metal composite material, polypropylene composition and sheet are tested according to the following methods. The test results of the polypropylene / metal composite material are shown in Table 1:
[0105] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682.2-2018, where the test temperature for homopolymer polypropylene and impact copolymer polypropylene is 230°C and the load is 2.16 kg; the test temperature for thermal bonding enhancer is 190°C and the load is 2.16 kg;
[0106] (2) Melting point: measured according to the method specified in GB / T 28724-2012;
[0107] (3) Tensile strength: measured according to the method specified in GB / T1040.1-2018;
[0108] (4) Drop weight impact strength: measured according to the method specified in GB / T14153-1993;
[0109] (5) Interlayer peel strength: measured according to the method specified in QB / T2358-98.
[0110] (6) Density: measured according to the method specified in GB / T 1033.1-2008;
[0111] (7) Area density: measured according to the method specified in ASTM D1622-2020.
[0112] In the following examples, the β-crystal nucleating agent with the brand name VP101B is sourced from Beijing Research Institute of Chemical Industry of Sinopec Corporation; the sources of some raw materials are described in the examples, and the other raw materials are commercially available unless otherwise specified.
[0113] Example 1
[0114] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0115] (1) Preparation of polypropylene composition A:
[0116] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry (under 23°C test conditions, the impact strength is 23KJ / m 2 ), ethylene content is 11%wt, melt flow rate is 2.0g / 10min, and melting point is 155℃.
[0117] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade of VP101B is added. Then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melt-mixed, extruded, granulated and dried, a polypropylene composition pellet is obtained. The melt mass flow rate MFRA is detected to be 4.6 / 10min; the melting point of the polypropylene composition A is 157°C.
[0118] (2) Preparation of polypropylene composition B:
[0119] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C and a melt flow rate of 6.6 g / 10 min; component y is a polyolefin elastomer with a grade of 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene content of 16%wt and a melt flow rate of 1.4 g / 10 min at 190°C and a load of 2.16 kg;
[0120] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 15 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained, and the melt mass flow rate MFRB is 5.2 g / 10 min, and the melting point is 138° C.;
[0121] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0122] The pellets of polypropylene composition A and polypropylene composition B obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering machine, and the polypropylene composition B is added to the upper and lower surface layer extruders of the multi-layer extrusion casting machine.
[0123] After the pellets are co-extruded and compounded out from the die of the extruder, they are sequentially passed through a calendering roller and a traction roller, and then subjected to solid phase stretching, edge cutting and winding, thereby obtaining the sheet.
[0124] The temperature of the extrusion casting was 230°C, and the temperature of the calendering roller was 55°C. The temperature during the solid phase stretching process was 135°C, the stretching rate was 2m / min, and the stretching ratio was 7 times. After stretching, the film was rolled up to form a polypropylene sheet (composite film), which consisted of an upper surface layer (film layer B), a core layer (film layer A) and a lower surface layer (film layer B).
[0125] The thickness of the polypropylene sheet (composite film) is 80 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.
[0126] (4) Preparation of polypropylene fabric:
[0127] The three-layer co-extruded polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon is woven by a commercial weaving machine according to the designed fabric structure to obtain a plain weave polypropylene fabric.
[0128] (5) Preparation of polypropylene / metal composite materials:
[0129] The polypropylene fabric and metal mesh obtained in the above step (4) are laminated and hot-pressed, and then cooled and shaped to form a polypropylene / metal composite material. The polypropylene / metal composite material includes 24 layers of polypropylene fabric and 1 layer of stainless steel mesh with a metal wire diameter of 0.08 mm and a hole number of 100 meshes. The stainless steel mesh is placed in the middle of the polypropylene fabric, and 12 layers of polypropylene fabric are arranged on both sides of the stainless steel mesh. The polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5Mpa, preheating time 180s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene / metal composite material is 1.79mm, and the surface density is shown in Table 1.
[0130] Example 2
[0131] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0132] (1) Preparation of polypropylene composition A:
[0133] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an impact strength of 25KJ / m under 23°C test conditions. 2 , ethylene content is 8%wt, melt flow rate is 3.2g / 10min, and melting point is 155℃.
[0134] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 70 parts by weight, and the mass fraction Wb of component b is 30 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with the grade VP101B is added. Then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melt-mixed, extruded, granulated and dried, a polypropylene composition pellet is obtained. The melt mass flow rate MFRA is detected to be 7.3 / 10min, and the melting point of the polypropylene composition A is 161°C.
[0135] (2) Preparation of polypropylene composition B:
[0136] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 134°C, an ethylene-propylene-butene terpolymer, and a melt flow rate of 5.2 g / 10 min; component y is a polyolefin elastomer produced by Sinopec Beijing Research Institute of Chemical Industry, an ethylene-propylene copolymer, with an ethylene content of 15% wt, a melting point of 105°C, and a melt flow rate of 9 g / 10 min at 190°C and a load of 2.16 kg;
[0137] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 80 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained, and its melt mass flow rate MFRB is detected to be 9.6 g / 10 min. The melting point of the polypropylene composition B is 130°C.
[0138] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0139] The preparation process is the same as step (3) of Example 1.
[0140] (4) Preparation of polypropylene fabric:
[0141] The preparation process is the same as step (4) of Example 1.
[0142] (5) Preparation of polypropylene / metal composite materials:
[0143] The preparation process is the same as step (5) of Example 1.
[0144] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0145] Example 3
[0146] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0147] (1) Preparation of polypropylene composition A:
[0148] Same as Example 1, wherein the mass fraction Wa of component a is 90 parts by weight, and the mass fraction Wb of component b is 10 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with a grade of VP101B is added. A pellet of polypropylene composition A is obtained, and its melt mass flow rate MFRA is detected to be 6.8 / 10min, and the melting point of polypropylene composition A is 158°C.
[0149] (2) Preparation of polypropylene composition B:
[0150] The same as Example 1, wherein the mass fraction Wx of component x is 90 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and finally the polypropylene composition B pellets are obtained. The melt mass flow rate MFRB is 8.7 g / 10 min, and the melting point of the polypropylene composition B is 139°C.
[0151] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0152] The preparation process is the same as step (3) of Example 1.
[0153] (4) Preparation of polypropylene fabric:
[0154] The preparation process is the same as step (4) of Example 1.
[0155] (5) Preparation of polypropylene / metal composite materials:
[0156] The preparation process is the same as step (5) of Example 1.
[0157] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0158] Example 4
[0159] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0160] (1) Preparation of polypropylene composition A:
[0161] The preparation process is the same as step (1) of Example 1.
[0162] (2) Preparation of polypropylene composition B:
[0163] The preparation process is the same as step (2) of Example 1.
[0164] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0165] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 80 μm, wherein the thickness of the film layer A accounts for 90% of the total thickness of the sheet.
[0166] (4) Preparation of polypropylene fabric:
[0167] The preparation process is the same as step (4) of Example 1.
[0168] (5) Preparation of polypropylene / metal composite materials:
[0169] The preparation process is the same as step (5) of Example 1.
[0170] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0171] Example 5
[0172] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0173] (1) Preparation of polypropylene composition A:
[0174] The preparation process is the same as step (1) of Example 1.
[0175] (2) Preparation of polypropylene composition B:
[0176] The preparation process is the same as step (2) of Example 1.
[0177] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0178] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 80 μm, wherein the thickness of the film layer A accounts for 70% of the total thickness of the sheet.
[0179] (4) Preparation of polypropylene fabric:
[0180] The preparation process is the same as step (4) of Example 1.
[0181] (5) Preparation of polypropylene / metal composite materials:
[0182] The preparation process is the same as step (5) of Example 1.
[0183] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0184] Example 6
[0185] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0186] (1) Preparation of polypropylene composition A:
[0187] The preparation process is the same as step (1) of Example 1.
[0188] (2) Preparation of polypropylene composition B:
[0189] The preparation process is the same as step (2) of Example 1.
[0190] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0191] The preparation process is the same as step (3) of Example 1.
[0192] (4) Preparation of polypropylene fabric:
[0193] The main steps are the same as step (4) of Example 1. The oriented flat tape is woven according to the designed fabric structure using a commercial weaving machine to obtain a satin polypropylene fabric.
[0194] (5) Preparation of polypropylene / metal composite materials:
[0195] The preparation process is the same as step (5) of Example 1.
[0196] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0197] Example 7
[0198] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0199] (1) Preparation of polypropylene composition A:
[0200] The preparation process is the same as step (1) of Example 1.
[0201] (2) Preparation of polypropylene composition B:
[0202] The preparation process is the same as step (2) of Example 1.
[0203] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0204] The main preparation process is the same as step (3) of Example 1. The stretching ratio of the sheet is 10 times. The thickness of the polypropylene sheet (composite film) is 70 μm.
[0205] (4) Preparation of polypropylene fabric:
[0206] The preparation process is the same as step (4) of Example 1.
[0207] (5) Preparation of polypropylene / metal composite materials:
[0208] The preparation process is the same as step (5) of Example 1.
[0209] The thickness of the prepared polypropylene / metal composite material is 1.71 mm, and the surface density is shown in Table 1.
[0210] Example 8
[0211] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0212] (1) Preparation of polypropylene composition A:
[0213] The preparation process is the same as step (1) of Example 1.
[0214] (2) Preparation of polypropylene composition B:
[0215] The preparation process is the same as step (2) of Example 1.
[0216] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0217] The preparation process is the same as step (3) of Example 1.
[0218] (4) Preparation of polypropylene fabric:
[0219] The preparation process is the same as step (4) of Example 1.
[0220] (5) Preparation of polypropylene / metal composite materials:
[0221] The main preparation process is the same as step (5) of Example 1. The polypropylene fabric is placed at 45° between the warp directions.
[0222] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0223] Example 9
[0224] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0225] (1) Preparation of polypropylene composition A:
[0226] The preparation process is the same as step (1) of Example 1.
[0227] (2) Preparation of polypropylene composition B:
[0228] The preparation process is the same as step (2) of Example 1.
[0229] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0230] The preparation process is the same as step (3) of Example 1.
[0231] (4) Preparation of polypropylene fabric:
[0232] The preparation process is the same as step (4) of Example 1.
[0233] (5) Preparation of polypropylene / metal composite materials:
[0234] The main preparation process is the same as step (5) of Example 1. The polypropylene fabric is placed at 0° between the warp directions.
[0235] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0236] Example 10
[0237] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, and the three-layer co-extruded polypropylene sheet provided by the present invention.
[0238] (1) Preparation of polypropylene composition A:
[0239] The preparation process is the same as step (1) of Example 1.
[0240] (2) Preparation of polypropylene composition B:
[0241] The preparation process is the same as step (2) of Example 1.
[0242] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0243] The preparation process is the same as step (3) of Example 1.
[0244] (4) Preparation of polypropylene / metal composite materials:
[0245] The polypropylene fabric was not prepared, but the three-layer co-extruded polypropylene sheet prepared in step (3) was used to replace the polypropylene fabric obtained in step (4) of Example 1, and the three-layer co-extruded polypropylene sheet was laminated and hot-pressed in accordance with step (5) of Example 1. The thickness of the prepared polypropylene / metal composite material was 1.76 mm, and the surface density was shown in Table 1.
[0246] Embodiment 11
[0247] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0248] (1) Preparation of polypropylene composition A:
[0249] The preparation process is the same as step (1) of Example 1.
[0250] (2) Preparation of polypropylene composition B:
[0251] The preparation process is the same as step (2) of Example 1.
[0252] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0253] The preparation process is the same as step (3) of Example 1.
[0254] (4) Preparation of polypropylene fabric:
[0255] The preparation process is the same as step (4) of Example 1.
[0256] (5) Preparation of polypropylene / metal composite materials:
[0257] The main steps are the same as those in Example 1. The temperature is 155°C, the hot pressing pressure is 10 MPa, the preheating time is 300 seconds, the hot pressing time is 300 seconds, and the cooling time is 700 seconds. The thickness of the prepared polypropylene / metal composite material is 1.72 mm, and the surface density is shown in Table 1.
[0258] Example 12
[0259] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0260] (1) Preparation of polypropylene composition A:
[0261] The preparation process is the same as step (1) of Example 1.
[0262] (2) Preparation of polypropylene composition B:
[0263] The preparation process is the same as step (2) of Example 1.
[0264] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0265] The preparation process is the same as step (3) of Example 1.
[0266] (4) Preparation of polypropylene fabric:
[0267] The preparation process is the same as step (4) of Example 1.
[0268] (5) Preparation of polypropylene / metal composite materials:
[0269] The polypropylene fabric and metal mesh obtained in the above step (4) are laminated and hot-pressed, and then cooled and shaped to form a polypropylene / metal composite material. The polypropylene / metal composite material includes 48 layers of polypropylene fabric and 4 layers of stainless steel mesh with a metal wire diameter of 0.1 mm and a hole number of 500 mesh. The stainless steel mesh is placed in the middle of the polypropylene fabric, and 8 layers of polypropylene fabric are placed between the stainless steel. The polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 155°C, hot pressing pressure 10Mpa, preheating time 300s, hot pressing time 300s, and cooling time 700s. The thickness of the prepared polypropylene / metal composite material is 4.12mm, and the surface density is shown in Table 1.
[0270] Example 13
[0271] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0272] (1) Preparation of polypropylene composition A:
[0273] The preparation process is the same as step (1) of Example 1.
[0274] (2) Preparation of polypropylene composition B:
[0275] The preparation process is the same as step (2) of Example 1. The difference is that component B i and x i The materials are as follows:
[0276] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 110°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 115°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 120°C; component x4 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 125°C; component x5 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry , which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; component x6 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x7 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 138°C; component x8 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x9 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 143°C; component x 10 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 145°C; component x 11 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 148°C; component x 12 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 150°C; among them, components x1-x 12 The molecular weight distribution Mw / Mn is between 7 and 10, and the components x1-x 12 The melt flow rate is 1-20g / 10min.
[0277] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3, 4, 5, 6, 7, 8, 9, 11, 12), after testing, the melting point of B1 is 110℃, the melting point of B2 is 113℃, the melting point of B3 is 117℃, the melting point of B4 is 123℃, the melting point of B5 is 127℃, the melting point of B6 is 133℃, the melting point of B7 is 135℃, the melting point of B8 is 137℃, the melting point of B9 is 140℃, and the melting point of B 10 The melting point of B is 142°C. 11 The melting point of B is 146℃. 12 The melting point is 148°C.
[0278] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0279] The preparation process is the same as step (3) of Example 1.
[0280] (4) Preparation of polypropylene fabric:
[0281] The preparation process is the same as step (4) of Example 1.
[0282] (5) Preparation of polypropylene / metal composite materials:
[0283] The polypropylene fabric and the metal mesh obtained in the above step (4) are laminated and hot-pressed to fuse, and then cooled and shaped to form a polypropylene / metal composite material. The polypropylene / metal composite material includes 23 layers of polypropylene fabric and 1 layer of stainless steel mesh with a metal wire diameter of 0.08 mm and a mesh number of 100. The stainless steel mesh is placed in the middle of the polypropylene fabric, and 12 layers and 11 layers of polypropylene fabric are arranged on both sides of the stainless steel mesh respectively. The polypropylene fabric and the stainless steel mesh are stacked in sequence, from bottom to top, B 12 A 12 B 12… B9A9B 9… B3A3B3, B2A2B2, B1A1B1, stainless steel mesh, B2A2B2, B3A3B3, ... B9A9B9 ... B 12 A 12 B 12 , wherein the total number of polypropylene fabric layers is 23, and the polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5Mpa, preheating time 180s, hot pressing time 120s, and cooling time 600s. The thickness of the prepared polypropylene / metal composite material is 1.75mm, and the surface density is shown in Table 1.
[0284] Embodiment 14
[0285] This example is used to illustrate the preparation of the polypropylene / metal composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, and the polypropylene fabric provided by the present invention.
[0286] (1) Preparation of polypropylene composition A:
[0287] The preparation process is the same as step (1) of Example 1.
[0288] (2) Preparation of polypropylene composition B:
[0289] The main preparation process is the same as step (2) of Example 1. The difference is that component B i and x i The materials are as follows:
[0290] Components x1-x3 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 120°C; components x4-x6 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 130°C; components x7-x9 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 140°C; components x 10 -x 12 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, an ethylene-propylene-butene terpolymer with a melting point of 150°C; wherein the molecular weight distribution Mw / Mn of components x1-x9 is all between 7-10, and the melt flow rate of components x1-x9 is all between 1-20g / 10min.
[0291] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3, 4, 5, 6, 7, 8, 9...12), after testing, the melting point of B1-B3 is 117℃, the melting point of B4-B6 is 127℃, and the melting point of B7-B9 is 137℃. 10 -B 12 The melting point is 148°C.
[0292] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0293] The preparation process is the same as step (3) of Example 1.
[0294] (4) Preparation of polypropylene fabric:
[0295] The preparation process is the same as step (4) of Example 1.
[0296] (5) Preparation of polypropylene / metal composite materials:
[0297] The polypropylene fabric and the metal mesh obtained in the above step (4) are laminated and hot-pressed to fuse, and then cooled and shaped to form a polypropylene / metal composite material. The polypropylene / metal composite material includes 23 layers of polypropylene fabric and 1 layer of stainless steel mesh with a metal wire diameter of 0.08 mm and a mesh number of 100. The stainless steel mesh is placed in the middle of the polypropylene fabric, and 12 layers and 11 layers of polypropylene fabric are arranged on both sides of the stainless steel mesh respectively. The polypropylene fabric and the stainless steel mesh are stacked in sequence, from bottom to top, B 12 A 12 B 12… B9A9B 9… B3A3B3, B2A2B2, B1A1B1, stainless steel mesh, B2A2B2, B3A3B3, ... B9A9B9 ... B12 A 12 B 12 , wherein the total number of polypropylene fabric layers is 23, and the polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5Mpa, preheating time 180s, hot pressing time 120s, and cooling time 600s. The thickness of the prepared polypropylene / metal composite material is 1.72mm, and the surface density is shown in Table 1.
[0298] Comparative Example 1
[0299] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 80 μm. A polypropylene fabric and a polypropylene / metal composite material were prepared according to the method of Example 1.
[0300] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0301] Comparative Example 2
[0302] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that only the polypropylene composition B was used for extrusion casting into a single-layer film with a thickness of 80 μm. A polypropylene fabric and a polypropylene / metal composite material were prepared according to the method of Example 1.
[0303] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0304] Comparative Example 3
[0305] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that the polypropylene composition A contained only component b. A polypropylene fabric and a polypropylene / metal composite material were prepared according to the method of Example 1.
[0306] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0307] Comparative Example 4
[0308] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that the polypropylene composition B contained only component y. A polypropylene fabric and a polypropylene / metal composite material were prepared according to the method of Example 1.
[0309] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0310] Comparative Example 5
[0311] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that the thickness of the film layer A accounted for 95% of the total thickness of the sheet. A polypropylene fabric and a polypropylene / metal composite material were prepared according to the method of Example 1.
[0312] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0313] Comparative Example 6
[0314] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that the thickness of the film layer A accounted for 50% of the total thickness of the sheet. A polypropylene fabric and a polypropylene / metal composite material were prepared according to the method of Example 1.
[0315] The thickness of the prepared polypropylene / metal composite material is close to that of Example 1.
[0316] Comparative Example 7
[0317] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.
[0318] A polypropylene composite material was prepared according to the method of Example 1, except that only 24 layers of polypropylene fabric were used for hot pressing. The thickness of the prepared polypropylene composite material was 1.67 mm, and the surface density was shown in Table 1.
[0319] Comparative Example 8
[0320] A coextruded polypropylene sheet was prepared according to the method of Example 13, except that component B i and x i The materials are as follows:
[0321] Component x 12 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 110°C; component x 11 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 115°C; component x 10It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 120°C; component x9 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 125°C; component x8 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; component x7 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x6 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 138°C; component x5 is The random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x4 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 143°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 145°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 148°C; component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 150°C; among them, components x1-x 12 The molecular weight distribution Mw / Mn is between 7 and 10, and the components x1-x 12 The melt flow rate is 1-20g / 10min.
[0322] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i = 1, 2, 3, 4, 5, 6, 7, 8, 9, 11, 12), after testing, B 12 The melting point of B is 110℃. 11 The melting point of B is 113℃. 10 The melting point of B is 117℃, the melting point of B9 is 123℃, the melting point of B8 is 127℃, the melting point of B7 is 133℃, the melting point of B6 is 135℃, the melting point of B5 is 137℃, the melting point of B4 is 140℃, the melting point of B3 is 142℃, the melting point of B2 is 146℃ and the melting point of B1 is 148℃.
[0323] According to the method of Example 13, a polypropylene fabric and a polypropylene / metal composite material were prepared.
[0324] The thickness of the prepared polypropylene / metal composite material is close to that of Example 13.
[0325] Experimental example
[0326] The polypropylene / metal composite materials obtained in the above examples and comparative examples were tested according to the following method. The test results are shown in Table 1.
[0327] (1) Tensile strength: Prepare samples and measure them according to the method specified in GB / T1040.1-2018;
[0328] (2) Interlayer peel strength: Sample preparation and measurement shall be carried out according to the method specified in QB / T2358-98.
[0329] (3) Drop hammer impact strength: measured according to the method specified in GB / T14153-1993. The thicknesses of the polypropylene / metal composite materials obtained in Examples 1-11 and Comparative Examples 1-6 are similar, about 1.7 mm, and are all within the range of 1.7 mm ± 1 mm.
[0330] Table 1
[0331]
[0332]
[0333] From the results of the examples in Table 1, it can be concluded that the longitudinal (MD) tensile strength of the polypropylene / metal composite material of the present invention is ≥280Mpa, and the interlayer peeling strength is ≥1N / mm; the polypropylene / metal composite material is obtained by hot pressing 24 layers of polypropylene fabric and 1 layer of metal mesh, and when the thickness is about 1.79mm, the drop hammer impact strength is ≥280J. It can be seen that the polypropylene / metal composite material prepared according to the present invention has both good tensile properties and impact resistance, and has good interlayer peeling strength at a relatively low hot pressing temperature.
[0334] It can be seen from preferred embodiments 1-3 that the longitudinal (MD) tensile strength of the polypropylene / metal composite material prepared by the present invention is ≥300Mpa, and the interlayer peel strength is ≥1.1N / mm; the polypropylene / metal composite material is obtained by hot pressing 24 layers of polypropylene fabric and 1 layer of metal mesh, and when the thickness is about 1.79mm, the drop hammer impact strength is ≥300J.
[0335] It can be seen from Comparative Examples 1-6 that using only a single-layer sheet structure or using an interlayer ratio outside the scope of the embodiment will lead to a decrease in the performance of the laminated polypropylene sheet or fabric, resulting in a significant decrease in the tensile strength, impact properties or interlayer peeling strength of the obtained polypropylene / metal composite material.
[0336] It can be seen from Comparative Example 7 that the polypropylene composite material prepared by laminating and hot pressing only polypropylene sheets or fabrics cannot achieve the tensile strength and impact properties of the polypropylene / metal composite material.
[0337] It can be known from the more preferred embodiments 13 and 14 that the present invention provides a composite material of a polypropylene composite material matrix with a melting point gradient structure combined with metal through the melting point gradient structure design of laminated polypropylene sheets in a polypropylene composite material matrix. The polypropylene / metal composite material has further improved tensile properties and impact resistance, and further improved interlayer peeling strength at a lower hot pressing temperature.
[0338] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0339] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A polypropylene / metal composite material having a laminated structure, comprising at least one metal layer and a plurality of polypropylene coating layers correspondingly coated on each metal layer, wherein the metal layer has a plurality of through holes distributed thereon; Each polypropylene covering layer is the same or different and comprises at least one layer of polypropylene sheet and / or at least one layer of polypropylene fabric woven from polypropylene sheets; wherein, The polypropylene sheet comprises a layer A and layers B and B' located on both sides of the layer A, with a structure of BAB'; Wherein, layer A contains a polypropylene composition A, and the polypropylene composition A includes homopolymer polypropylene a and impact copolymer polypropylene b; layer B and layer B' are the same or different, and each contains a polypropylene composition B and a polypropylene composition B', wherein the polypropylene composition B and the polypropylene composition B' each contain a random copolymer polypropylene x and a thermal adhesion enhancer y; The melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'.
2. The polypropylene / metal composite material according to claim 1, characterized in that: The polypropylene fabric has a plain, twill and / or satin three-dimensional structure; and / or, Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99 wt% of homopolypropylene a and 1-50 wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90 wt% of homopolypropylene a and 10-30 wt% of impact copolymer polypropylene b; and / or, Based on the total weight of each of the polypropylene compositions B and B', each of the polypropylene compositions B and B' comprises 70-99 wt% of random copolymerized polypropylene x and 1-30 wt% of thermal adhesion enhancer y; preferably, each of the polypropylene compositions B and B' comprises 80-90 wt% of random copolymerized polypropylene x and 10-20 wt% of thermal adhesion enhancer y.
3. The polypropylene / metal composite material according to claim 1, characterized in that: Based on the total thickness of the polypropylene sheet, the thickness of the layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, more preferably 71%-80%; and / or, The melting point of the homopolypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in each of the polypropylene compositions B and B'. Preferably, the temperature difference between the corresponding melting points is greater than or equal to 10 degrees.
4. The polypropylene / metal composite material according to claim 1, characterized in that: The melting point of the homopolypropylene a is 160-170° C.; and / or, The homopolypropylene a has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, more preferably 2.5-18 g / 10 min; and / or, The isotacticity (mm) of the homopolypropylene a is not less than 96%.
5. The polypropylene / metal composite material according to claim 1, characterized in that: The melting point of the impact-resistant copolymer polypropylene b is 150-170° C.; and / or, The monomer of the impact-resistant copolymer polypropylene b and propylene copolymer is ethylene or butene, and the content of ethylene or butene is 2-50%wt, preferably 3-20%wt, more preferably 5-15%wt, and / or, The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or The impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 .
6. The polypropylene / metal composite material according to claim 1, characterized in that: The melting point of the random copolymer polypropylene x is 120-140° C.; and / or, The random copolymer polypropylene x has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, more preferably 3-18 g / 10 min; and / or, The random copolymer polypropylene x is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer or a propylene-ethylene binary copolymer.
7. The polypropylene / metal composite material according to claim 1, characterized in that: The melt flow rate of the thermal adhesion enhancer y at 190° C. and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, more preferably 1-18 g / 10 min; and / or, The thermal adhesion enhancer y is selected from one or more of polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA and petroleum resin; preferably, The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or α-olefin; further preferably, the α-olefin is a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or, The petroleum resin is a C5 and / or C9 hydrogenated petroleum resin, preferably having a softening point of 100-150° C.; more preferably, the petroleum resin is a cyclopentadiene type resin.
8. The polypropylene / metal composite material according to claim 1, characterized in that: The layer A further contains a β-crystal nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed ring aromatic hydrocarbons, Group IIA two-component complexes, aromatic diamides, rare earth compounds, and cyclic dicarboxylates; and / or, Based on 100 parts by weight of the total amount of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.
9. The polypropylene / metal composite material according to any one of claims 1 to 8, characterized in that: The BAB' layer structure of the polypropylene sheet is obtained by co-extruding components including the polypropylene composition A and the polypropylene compositions B and B'; and / or, The polypropylene / metal composite material is prepared by stacking multiple layers of the polypropylene sheets and / or polypropylene fabrics and the metal material layers in sequence, fusing them through hot pressing, and then cooling and shaping; and / or, The total number of layers of the polypropylene sheet and / or polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers; and / or, The surface density of the polypropylene / metal composite material is greater than or equal to 600g / m 2 , more preferably 600-35000g / m 2 ; Most preferably 800-12000g / m 2 and / or, The longitudinal tensile strength of the polypropylene / metal composite material is greater than or equal to 280 MPa, preferably greater than or equal to 300 MPa.
10. The polypropylene / metal composite material according to any one of claims 1 to 8, characterized in that: The metal material layer is a metal mesh; preferably, The metal mesh is selected from at least one of stainless steel mesh, carbon steel mesh, galvanized steel mesh and alloy mesh; and / or, The diameter of the metal wire in the metal mesh is 0.02-2 mm, preferably 0.03-1 mm; and / or, the number of holes is 10-1000 meshes, preferably 50-500 meshes; and / or, The number of the metal material layers is greater than or equal to 1 layer, more preferably 1-50 layers, and most preferably 1-20 layers.
11. The polypropylene / metal composite material according to any one of claims 1 to 8, characterized in that: The polypropylene / metal composite material comprises a polypropylene composite material matrix formed by stacking all polypropylene coating layers and at least one metal material layer arranged in the polypropylene composite material matrix; The polypropylene composite material matrix comprises a plurality of polypropylene sheet unit groups stacked in sequence; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, each polypropylene sheet unit comprises a core layer A i and located in the core layer A i Outer layer B on both sides i , B' i , structure B i A i B' i The structure of the polypropylene composite material is from bottom to top: nth group...ith group...2nd group, 1st group, 2nd group...ith group...nth group, and the total number of stacked polypropylene sheet unit groups is 2n-1; Both i and n are integers not less than 2, and i≤n; Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.
12. The polypropylene / metal composite material according to claim 11, characterized in that: Polypropylene composition A i The melting point of polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers in group i and the average melting point of all outer layers in group i-1, which are the same or different, is 1-40°C, preferably 1-10°C, more preferably 1-5°C; and / or 2≤n≤100, preferably, 2≤n≤50; and / or, Each polypropylene sheet unit group, independently, comprises 1 to 10, preferably 1 to 5, identical or different polypropylene sheet units; and / or, The number of polypropylene sheet units on both sides of each metal material layer is close.
13. The method for preparing the polypropylene / metal composite material according to any one of claims 1 to 12, comprising stacking multiple layers of the polypropylene sheet and / or polypropylene fabric and the metal material layer in sequence, fusing them by hot pressing, and then cooling and shaping to obtain the polypropylene / metal composite material.
14. The preparation method according to claim 13, characterized in that: The multi-layer polypropylene sheets are stacked from top to bottom at an angle of 0-90° along their respective machine directions; and / or, The multiple layers of polypropylene fabric are stacked from top to bottom with the warp angle between them being 0-90 degrees; and / or, The total number of layers of the multi-layer polypropylene sheet and / or multi-layer polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers; and / or, The number of the metal material layers is greater than or equal to 1 layer, more preferably 1-50 layers, and most preferably 1-20 layers.
15. The preparation method according to claim 13, characterized in that: The temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, more preferably 140-159°C; and / or, The pressure of the hot pressing fusion is 2-10 MPa; and / or, The preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s; and / or, The cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s.
16. Application of the polypropylene / metal composite material according to any one of claims 1 to 12 and the polypropylene / metal composite material prepared by the preparation method according to any one of claims 13 to 15 in the fields of sports protection, automobile manufacturing, military materials and consumer goods.
Citation Information
Patent Citations
3D printing device and method for directly forming metal polymer composite material
CN112974853A
Method for producing metal-polymer composites
CN114096618A
Continuous fiber-strengthened metal laminated composite plate and manufacturing method thereof
CN103847165A
Anisotropic polypropylene plate-metal compound material and preparation method thereof
CN106273897A
Thermoplastic fiber metal laminate and preparation method thereof
CN108202513A