Polypropylene composite foamed sheet as well as preparation method and application thereof
Through the laminated structure of the polypropylene composite foam sheet, combined with the high-strength, high-impact, polypropylene composite sheet and polypropylene foam sheet, it is solved that it is difficult for the polypropylene foam sheet to have both high strength in the prior art. , the problems of high impact resistance and high peel strength improve compatibility and physical properties, and reduce recycling and processing costs.
Patent Information
- Application Number
- CN202310513111.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-08
AI Technical Summary
While improving physical properties, existing polypropylene foamed sheets are difficult to have high strength, high impact resistance and high peel strength, and have poor compatibility with other materials, resulting in difficult recycling and processing, and high production costs, which cannot be met. Market demand.
The polypropylene composite foam sheet adopts a laminated structure, and the high-strength, high-impact, polypropylene composite sheet is combined with the polypropylene foam sheet by hot pressing and bonding to form a BAB' structure, in which layer A is Containing homopolypropylene and impact copolymerized polypropylene, layer B and layer B' contains random copolymerized polypropylene and thermal bonding enhancer, and the melting point difference is used to improve interlayer peel strength.
The high strength, high impact resistance and high peel strength of polypropylene composite foam sheet is realized, while improving compatibility with other materials, reducing recycling and processing costs, and optimizing without reducing thermal insulation performance. Physical performance.
Smart Images

Figure BDA0004220499440000231 
Figure BDA0004220499440000241
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a polypropylene composite foam sheet and a preparation method and application thereof. Background Art
[0002] The global polypropylene foam sheet material market will grow at an annual rate of 6.9% between 2018 and 2023, from US$751.0 million in 2018 to US$1,048.8 million in 2023. Based on the type of foam material: The low-density segment is expected to lead the foam sheet market. The growth in demand for automotive, protective packaging, and insulation applications has driven the growth of this segment. The automotive industry dominates the consumption of low-density polypropylene foam sheets, which helps cars to be more impact-resistant and reduce the weight of the car body. This also requires further improvement in the physical properties of polypropylene foam sheets while minimizing the increase in production costs during molding.
[0003] Traditional means such as optimizing raw materials and processes are no longer able to meet the needs of the market. The use of filler modification can effectively improve the physical properties of polypropylene foam sheets, but it will also significantly weaken the foaming molding ability of special materials and the weight reduction effect of the appearance quality of products; by designing and adjusting the types and contents of catalysts and comonomers to optimize the molecular structure of special materials for polypropylene foam sheets, the physical properties of polypropylene foam sheet products can be improved while also improving the foaming molding ability, but the production promotion cycle is long and the cost is high; optimizing the foaming molding process conditions of polypropylene foam sheets requires upstream and downstream enterprises of polypropylene extrusion foam products to adjust the production process parameters and even equipment, which is difficult for manufacturers to accept.
[0004] In order to further improve the physical properties of polypropylene foam sheet products, it has become an emerging process to compound inorganic or organic reinforcing sheets on the surface of polypropylene foam sheets. The existing composite reinforcing sheets in this technology have high requirements for mechanical properties, and mainly use composite materials such as glass fiber / carbon fiber reinforced thermoplastic resins. These reinforcing sheets are prone to compatibility problems with polypropylene foam sheets, which makes it difficult to achieve ideal physical properties such as compression and thermal insulation. Even if a polypropylene foam sheet product that meets the product performance is successfully obtained, the presence of the reinforcing sheet brings problems such as high apparent density, long molding time and high energy consumption, and it is difficult to recycle after mixing with materials other than polypropylene.
[0005] If there is a polypropylene sheet material used as a reinforcing sheet material, the same polypropylene composition as the polypropylene sheet material can be used as the matrix resin of the polypropylene foam sheet material. The polypropylene foam sheet product does not need to be separated and processed during recycling, and can be directly crushed and melted, and then granulated and used again. However, conventional polypropylene sheets either do not meet the requirements in terms of strength, impact resistance, or interlayer peeling strength. There is no polypropylene sheet material with high strength, high impact resistance, and high peeling strength. Therefore, how to provide a polypropylene sheet material with high strength, high impact resistance, and high peeling strength as a reinforcing sheet of a polypropylene composite foam sheet is the research purpose of the present invention. Summary of the invention
[0006] In view of the deficiencies of the above-mentioned prior art, the present invention provides a polypropylene composite foam sheet and a preparation method and application thereof. The polypropylene composite foam sheet uses a high-strength and high-impact polypropylene composite sheet as a composite sheet, which not only has the advantages of high strength, high impact resistance and high peel strength, but also has excellent apparent density, physical properties and thermal insulation properties. Compared with other pre-reinforced sheets made of non-polypropylene materials on the market, the compatibility is greatly improved, and no separation treatment is required during recycling, and it can be directly crushed and melted, and then granulated and used again. It has broad market prospects in the field of polypropylene foam sheet technology.
[0007] The first aspect of the present invention is to provide a polypropylene composite foam sheet having a laminated structure, comprising at least one layer of a reinforced composite sheet and at least one layer of a polypropylene foam sheet bonded to the reinforced composite sheet by hot pressing fusion; each layer of the reinforced composite sheet comprises at least one layer of a polypropylene sheet and / or at least one layer of a polypropylene fabric woven from a polypropylene sheet; wherein the polypropylene sheet comprises a layer A and layers B and B' located on both sides of the layer A, and the structure is BAB'; wherein the layer A comprises a polypropylene composition A, and the layer B is the same as or different from the layer B', and each correspondingly comprises a polypropylene composition B and a polypropylene composition B', wherein the polypropylene composition A comprises a homopolymer polypropylene a and an impact copolymer polypropylene b; the polypropylene composition B and the polypropylene composition B' each comprise a random copolymer polypropylene x and a thermal bonding enhancer y;
[0008] The melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'.
[0009] According to the present invention, the film layers B and B' on both sides of the film layer A are the same or different. In a preferred embodiment of the present invention, the film layers B and B' on both sides of the film layer A are the same.
[0010] In a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b.
[0011] In a preferred embodiment of the present invention, based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each comprise 70-99 wt% of random copolymer polypropylene x and 1-30 wt% of thermal adhesion enhancer y; preferably, the polypropylene composition B and the polypropylene composition B' each comprise 80-90 wt% of random copolymer polypropylene x and 10-20 wt% of thermal adhesion enhancer y.
[0012] In a preferred embodiment of the present invention, based on the total thickness of the polypropylene sheet, the thickness of the layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.
[0013] In a preferred embodiment of the present invention, the melting point of the homopolymerized polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymerized polypropylene x in the polypropylene compositions B and B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees. In this preferred embodiment, the inventors of the present invention surprisingly found that the obtained polypropylene sheet laminated with the polypropylene foam sheet is hot-pressed to obtain a polypropylene composite foam sheet, and the polypropylene composite foam sheet has more excellent mechanical properties and better interlayer peeling strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the obtained polypropylene composite foam sheet has a higher interlayer peeling strength.
[0014] According to the present invention, the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'. In a preferred embodiment of the present invention, the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B, and the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B' are each greater than or equal to 5°C, preferably greater than or equal to 10°C, and more preferably greater than or equal to 20°C. In this preferred embodiment, the inventors of the present invention found that in this preferred embodiment, the obtained polypropylene sheet is laminated with a polypropylene foam sheet by hot pressing to obtain a polypropylene composite foam sheet, and the polypropylene composite foam sheet has more excellent mechanical properties and better interlayer peel strength. Even at a lower hot pressing temperature and in a wider hot pressing temperature range, the interlayer peel strength of the obtained polypropylene composite foam sheet is higher.
[0015] The thicknesses of the film layers B and B' on both sides of the film layer A may be the same or different, and are preferably the same.
[0016] The present invention does not limit the thickness of the polypropylene sheet, and can be selected in a wide range according to its practical application field. Preferably, the thickness of the polypropylene sheet can be 10-1000 μm, preferably 30-500 μm, and more preferably 50-300 μm.
[0017] According to the present invention, the thickness of the film layers A, B, B' can be controlled by the melt pump of the extruder during the processing.
[0018] In a preferred embodiment of the present invention, the homopolypropylene a has:
[0019] The melting point is 150-170°C, preferably 160-170°C; and / or,
[0020] The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or,
[0021] The isotacticity (mm) is not less than 96%.
[0022] In a preferred embodiment of the present invention, the impact-resistant copolymer polypropylene b has: the melting point of the impact-resistant copolymer polypropylene b is 150-170° C.: and / or,
[0023] The monomer of the impact copolymer polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or,
[0024] The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or,
[0025] The cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 (Test conditions: 23℃).
[0026] In a preferred embodiment of the present invention, the random copolymer polypropylene x has:
[0027] The melting point is 110-150°C, preferably 120-140°C; and / or,
[0028] The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or,
[0029] The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or,
[0030] It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.
[0031] According to the research conducted by the inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene composition A are within the above preferred ranges, the high impact copolymer polypropylene b in the composition can absorb impact energy well, meet the requirements of impact performance, and make the sheet have good impact performance. At the same time, since the macromolecular segments in the homopolymer polypropylene a are relatively regular, crystallization occurs during the sheet preparation process, so the sheet also has good tensile properties.
[0032] In a preferred embodiment of the present invention, the thermal adhesion enhancer y has:
[0033] The melting point or viscosity flow temperature is 70-110°C; and / or,
[0034] The melt flow rate at 190°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or,
[0035] One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, and petroleum resin; preferably, polyolefin elastomer and / or petroleum resin.
[0036] In a preferred embodiment of the present invention, the polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or α-olefin, and the α-olefin is preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene.
[0037] In a preferred embodiment of the present invention, the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin having a softening point of 100-150° C.; preferably, it is a cyclopentadiene type resin.
[0038] In a preferred embodiment of the present invention, the layer A further contains a β-crystal nucleating agent; preferably,
[0039] The β-crystal nucleating agent is selected from at least one of condensed ring aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates.
[0040] According to the research conducted by the present inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene compositions B and B' are within the preferred range, the low melting point random copolymer polypropylene x and thermal bonding enhancer y in the composition can significantly reduce the hot pressing temperature and broaden the hot pressing temperature window, and the thermal bonding enhancer y provides the sheet with good bonding properties, which can further improve the interlayer peeling strength.
[0041] The content of the β-crystal nucleating agent in layer A can be selected within a wide range. In a preferred embodiment of the present invention, relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight, for example, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5 parts by weight, and any two values or any interval between any two values.
[0042] According to the research of the present inventors, when the melt mass flow rate, polymer composition ratio and thickness distribution of the film layer A of the polypropylene composition A and the polypropylene combinations B and B' are within the preferred range, the preparation process of the composite material can be made smoother, so that the composite material has better uniformity, tensile strength, impact performance and interlayer peeling strength.
[0043] The BAB' layer structure of the polypropylene sheet can be prepared by various methods. In a preferred embodiment of the present invention, the BAB' layer structure of the polypropylene sheet is obtained by co-extruding components including the polypropylene composition A and the polypropylene compositions B and B'.
[0044] According to the present invention, the formula of the polypropylene foam sheet can be selected within a wide range. In a preferred embodiment of the present invention, the polypropylene foam sheet (i.e., the composition of the polypropylene foam sheet) contains a polypropylene composition. Preferably, the polypropylene foam sheet contains at least one of the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B', and optional auxiliary agents.
[0045] In a preferred embodiment of the present invention, the composition of the polypropylene foam sheet is composed of at least one of the polypropylene compositions A, B, and B' described above and a common processing aid. In the composition, the polypropylene composition A and the polypropylene compositions B and B' can be mixed in any ratio between 0-100.
[0046] Preferably, the auxiliary agent is selected from one or more of antioxidants, antistatic agents, lubricants, anti-aging agents, flame retardants, and color powders.
[0047] As an example, the composition of the polypropylene foam sheet may also contain one or more of the following processing aids commonly used in the polypropylene foaming process, such as but not limited to:
[0048] Graphite toner: added amount 1%-8%, preferably 2-5%; antioxidant: added amount 0.1-15‰, preferably 0.1-5‰; antistatic agent: added amount 0.1-10%, preferably 0.5-5%; lubricant: added amount 0.1-10%, preferably 0.5-3%; anti-aging agent: added amount 0.01-5%, preferably 0.1-2%. Flame retardant: added amount 0.1-25%, preferably 1-20%. The content of processing aids is well known in the industry and will not be repeated here.
[0049] The polypropylene composition foamed sheet of the present invention is prepared from the above-mentioned polypropylene foamed sheet composition.
[0050] As a preferred embodiment of the polypropylene composition foamed sheet provided by the present invention, the preparation method of the foamed sheet comprises: adding a foaming agent to the polypropylene composition, and foaming the foamed sheet.
[0051] The blowing agent used in the present invention can be a chemical blowing agent or a physical blowing agent.
[0052] Among them, chemical foaming agents include but are not limited to at least one of azodicarbonamide (AC foaming agent), p-toluenesulfonyl hydrazide, semicarbazide, tetrazoles, sodium bicarbonate and sodium citrate. The physical foaming agent can be an organic physical foaming agent or an inorganic physical foaming agent. Organic physical foaming agents include but are not limited to aliphatic hydrocarbons such as propane, butane, pentane, hexane and heptane, alicyclic hydrocarbons such as cyclobutane and cyclohexane, and halogenated hydrocarbons such as chlorofluoromethane, trifluoromethane, 1,2-difluoroethane, 1,2,2,2-tetrafluoroethane, methyl chloride, ethyl chloride and dichloromethane. The inorganic physical foaming agent includes but is not limited to at least one of air, nitrogen, carbon dioxide, oxygen and water.
[0053] Preferably, the polypropylene foam sheet is foamed by an inorganic physical foaming agent and / or contains a foaming agent; preferably, the inorganic physical foaming agent is selected from at least one of air, nitrogen, carbon dioxide, oxygen and water; and / or, the foaming agent is selected from a chemical foaming agent and / or an organic physical foaming agent; more preferably, the chemical foaming agent is selected from at least one of azodicarbonamide, p-toluenesulfonyl hydrazide, semicarbazides, tetrazoles, sodium bicarbonate and sodium citrate; the organic physical foaming agent is selected from at least one of an aliphatic hydrocarbon foaming agent, an alicyclic hydrocarbon foaming agent, and a halogenated hydrocarbon foaming agent.
[0054] According to some embodiments of the present invention, the preparation method of the polypropylene foam sheet provided by the present invention includes an extrusion foaming process and a compression foaming process. The specific foaming molding process conditions can be conventionally selected in the art, and the specific process is known to those skilled in the art and will not be described in detail here.
[0055] According to some embodiments of the present invention, the foam sheet has an apparent density of 60±0.3 g / L and a thickness of 1 mm. The conventional apparent density of the foam sheet selected in the art may include but is not limited to 10-300 g / L, and the thickness may include but is not limited to 0.2 mm-5 mm. Those skilled in the art are aware of this and will not be elaborated herein.
[0056] The polypropylene fabric in the present invention is obtained by weaving the polypropylene sheet mentioned above; preferably, the polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.
[0057] In order to facilitate weaving, the polypropylene sheet is preferably cut into polypropylene sheets with a width of 2-5 mm, and then woven to obtain the polypropylene fabric.
[0058] In a more preferred embodiment of the present invention, the polypropylene fabric is a plain, twill, satin or three-dimensional polypropylene fabric obtained by weaving three layers of co-extruded polypropylene stretched flat strips.
[0059] In a preferred embodiment of the present invention, the polypropylene composite foam sheet has a multi-layer sandwich structure.
[0060] In a preferred embodiment of the present invention, the polypropylene composition A contained in each stacked layer of polypropylene fabric may be the same or different, and the polypropylene fabric A contained in each layer may be independently selected, and preferably the polypropylene composition A of each layer is the same.
[0061] According to a preferred embodiment of the present invention, each layer of the reinforced composite sheet comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the reinforced composite sheet is nth group...ith group...2nd group, 1st group, 2nd group...ith group...nth group from bottom to top, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n;
[0062] Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition Bi , polypropylene composition B' i , the polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.
[0063] According to the present invention, the polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The melting point of the polypropylene composition A is preferably i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points is 5°C or more, preferably 10°C or more, and more preferably 20°C or more.
[0064] In a preferred embodiment of the present invention, the average value of the melting points of all outer layers in the i-th group is greater than or equal to the average value of the melting points of all outer layers in the i-1th group; preferably, the difference between the average value of the melting points of all outer layers in the i-th group and the average value of the melting points of all outer layers in the i-1th group are the same or different, and are each 1-40°C, preferably 1-10°C, and more preferably 1-5°C.
[0065] According to the present invention, the total number of stacked groups of the polypropylene sheet unit group is 2n-1. The present invention has a wide range of selection for the total number of stacked groups of the polypropylene sheet unit group. In a preferred embodiment of the present invention, 3≤n≤23 is selected, and more preferably, 3≤n≤16. According to the present invention, the number of polypropylene sheet units included in each polypropylene sheet unit group is selected in a wide range. In a preferred embodiment of the present invention, each polypropylene sheet unit group, independently, includes 1 to 10, preferably 1 to 5, more preferably 1 to 3 identical or different polypropylene sheet units, more preferably 1 polypropylene sheet unit. Preferably, the number of polypropylene sheet units included in each polypropylene sheet unit group is the same.
[0066] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, more preferably within ±1°C of the average melting point of all outer layers in the group.
[0067] In the embodiment where each polypropylene sheet unit group includes only one polypropylene sheet unit, for example, the structure of the polypropylene composite material can be B from bottom to top. n An B' n ……B i A i B' i ...B2A2B'2, B1A1B'1, B2A2B'2...B i A i B' i ……B n A n B' n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n.
[0068] In the embodiment where each polypropylene ply unit group includes 2 or more polypropylene ply units, for example, the structure of the i-th polypropylene ply unit group is B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip The structure of the polypropylene composite material can be sequentially as follows from bottom to top: n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A 12 B' 12 ……B 1j A 1j B' 1j )(B21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq ), the total number of stacked polypropylene sheet units is j+2k+...2p+...2q; j, k, p, q are each independently an integer not less than 2, preferably an integer from 2 to 10, more preferably from 2 to 5, and more preferably from 2 to 3.
[0069] In a preferred embodiment of the present invention, the polypropylene foam composite material has at least one of the following characteristics:
[0070] Longitudinal tensile strength ≥10MPa, preferably ≥20MPa;
[0071] Interlayer peel strength ≥ 0.8 N / mm, preferably ≥ 1.0 N / mm;
[0072] The tensile strength is measured according to the method specified in GB / T1040.1-2018, and the interlayer peel strength is measured according to the method specified in GB / T2358-98. The corresponding specimens in the above two tests are the standard specimens required in the above-mentioned test standards.
[0073] In a preferred embodiment of the present invention, based on the total thickness of the polypropylene composite foam sheet, the total thickness of the reinforced composite sheet accounts for 5%-60%, preferably 15%-45% of the total thickness of the polypropylene composite foam sheet.
[0074] In a preferred embodiment of the present invention, the total number of layers of all polypropylene sheets and polypropylene fabrics and the polypropylene foam sheet is 6-50 layers, more preferably 7-35 layers.
[0075] In a preferred embodiment of the present invention, the polypropylene foam sheets are stacked from top to bottom at an angle of 0-90° along their respective machine directions, with 1 to 6 layers, and most preferably 2 to 4 layers.
[0076] In a preferred embodiment of the present invention, the reinforced composite sheets are stacked from top to bottom in sequence at 0-90° along their respective machine directions, and preferably the total number of layers of polypropylene sheets and polypropylene fabrics in each layer of the reinforced composite sheet is 5-45 layers, and most preferably 5-30 layers.
[0077] In a preferred embodiment of the present invention, the apparent density of the multi-layer polypropylene composite foam sheet is ≤200g / m 2 , more preferably ≤150g / m 2 ; Most preferably ≤100g / m 2 .
[0078] The thermal insulation capacity of the composite foam sheet is not more than 20%, preferably not more than 12%, compared with the non-composite foam sheet prepared by the same process, and the thermal conductivity is reduced by 25%, preferably by 33% compared with the composite sheet with other reinforcement methods. Test method: The thermal conductivity is measured according to the method specified in GB / T 10294.
[0079] The polypropylene composite foam sheet is prepared by the following method: laminating at least one group of the polypropylene sheets and / or the polypropylene fabric with at least one layer of the polypropylene foam sheet, fusing them by hot pressing, and then cooling and shaping to obtain the polypropylene composite foam sheet; wherein each group of the polypropylene sheets and / or the polypropylene fabric is laminated in the order of forming the reinforced composite sheets of the corresponding layers.
[0080] In the present invention, "the polypropylene sheet and / or the polypropylene fabric" refers to one or both of the polypropylene sheet and the polypropylene fabric.
[0081] According to the present invention, preferably, the method for preparing the polypropylene sheet comprises co-extruding, casting or calendering, and stretching the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B' according to the BAB' structure to obtain the polypropylene sheet.
[0082] In a preferred embodiment of the present invention, the preparation of the polypropylene composition A comprises melt blending the components including the homopolypropylene a and the impact copolymer polypropylene b; and / or, the preparation of the polypropylene compositions B and B' comprises melt blending the components including the random copolymer polypropylene x and the thermal adhesion enhancer y; and / or, the coextrusion and casting temperatures are independently selected from 200-240°C; and / or, the temperature of the calendering roll is 50-70°C; and / or, the stretching conditions include: the stretching temperature is 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-20 times; preferably 1-15 times.
[0083] According to some embodiments of the present invention, polypropylene composition A, polypropylene composition B, polypropylene composition B', according to the BAB' structure, are co-extruded and cast or calendered to obtain a polypropylene co-extruded sheet. The process of the extrusion calendering method may include passing the co-extruded polypropylene sheet through a calendering roller, a traction roller, and then solid phase stretching, trimming and winding to obtain the sheet. The temperature of the extrusion casting is 200-230°C, and the temperature of the calendering roller is 50-70°C. The specific process of preparing the film by the extrusion calendering method is a commonly used choice in the art and will not be repeated here.
[0084] The second aspect of the present invention is to provide a method for preparing the polypropylene composite foam sheet described in the first aspect, comprising laminating at least one group of the polypropylene sheets and / or the polypropylene fabric with at least one layer of the polypropylene foam sheet, fusing them by hot pressing, and then cooling and shaping to obtain the polypropylene composite foam sheet.
[0085] According to the present invention, preferably, each group of the polypropylene sheets and / or the polypropylene fabrics are stacked in the order of the reinforced composite sheets forming the corresponding layers.
[0086] In a preferred embodiment of the present invention, the temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C.
[0087] In a preferred embodiment of the present invention, the pressure of the hot pressing fusion is 2-10 MPa.
[0088] In a preferred embodiment of the present invention, the preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-900s, preferably 10-600s.
[0089] In a preferred embodiment of the present invention, the cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-900 s.
[0090] In a preferred embodiment of the present invention, adjacent layers of the polypropylene sheet laminate are placed at 0-90° along respective machine directions, wherein the machine direction is the stretching direction (MD).
[0091] In a preferred embodiment of the present invention, adjacent layers of the polypropylene fabric laminate are placed at an angle of 0-90° along the warp direction.
[0092] In some preferred embodiments of the present invention, the hot pressing temperature is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or the hot pressing pressure is 2-10MPa, the preheating time is 5-600s, and the hot pressing time is 1-900s, preferably 10-600s; and / or the cooling pressure is 2-8MPa, and the cooling time is 30-900s.
[0093] In a more preferred embodiment of the present invention, as an example, the preparation method of the polypropylene composite foam sheet comprises the following steps:
[0094] Step a: co-extrude the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B' according to the BAB' structure and cast or calender to obtain a polypropylene co-extruded sheet; preferably, the extrusion casting or calendering temperature is 200-240° C., and the temperature of the calendering roller is 50-70° C.;
[0095] Step b: stretching the coextruded polypropylene sheet at a certain temperature to obtain a stretched polypropylene sheet; the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is preferably 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.
[0096] Step c: cutting the polypropylene stretched sheet to prepare polypropylene flat strips, and weaving the flat strips to prepare polypropylene fabrics; preferably, the width of the polypropylene flat strips is 2-5 mm, and the polypropylene fabrics include plain weave, twill, satin weave or other three-dimensional polypropylene fabrics;
[0097] Step d: After measuring the components of the polypropylene foam sheet according to the formula, add them into a high-speed mixer, stir them continuously at high speed for 1-10 minutes, preferably 2-5 minutes at room temperature, and then add them into a twin-screw extruder, extrude them at 180-230° C., and granulate them.
[0098] Step e-1: Continuously add the polypropylene composition particles in step d into the extrusion foaming equipment, the foaming temperature is between 120℃-260℃, preferably 140℃-200℃, the foaming pressure is between 60bar-250bar, preferably 80bar-200bar, add the foaming agent, and melt-knead in the screw, the screw speed is 3-50rpm, preferably 4-30rpm; the extrusion rate is 10-100kg / h, preferably 4-30rpm. The melt with the physical foaming agent evenly dispersed inside is extruded from the O-type die. Due to the rapid decrease in pressure, the foaming agent escapes from the melt to form bubbles, which are collected by a calibrated cutting and pulling winding device to obtain the polypropylene foam sheet. Or,
[0099] Step e-2: Heat the mold installed between the molding presses to a foaming temperature of 130°C-200°C, preferably 140°C-170°C; place the sheet prepared by extruding the polypropylene composition in step d into it, close the molding press, and seal the mold. Allow the gas generated by the foaming agent to diffuse into the polypropylene composition resin particles, and the foaming pressure is between 50bar-200bar, preferably 80bar-160bar. After saturation for 0.1-5 hours, preferably 0.3-2 hours, diffusion equilibrium is reached, and the pressure is released through the pressure relief valve once or multiple times, preferably 1-3 times, to open the mold for foaming, cool and shape, obtain a polypropylene composition foamed sheet, and then cut to obtain a polypropylene foam sheet of required thickness.
[0100] Step f: laminating and hot-pressing the polypropylene fabric and the foamed sheet prepared in step e-1 or e-2 in sequence, and then cooling and shaping to form a polypropylene composite material; preferably, in the step f, the hot pressing conditions are: hot pressing temperature 115-170°C, preferably 115-159°C, and more preferably 140-159°C; hot pressing pressure 2-10MPa, preheating time 5-600s, hot pressing time 1-900s, preferably 10-600s, cooling pressure 2-8MPa, cooling time 30s-900s; preferably, adjacent polypropylene fabrics in the polypropylene composite foamed sheet can be placed at 0-90° between the warp and the warp.
[0101] According to some embodiments of the present invention, in step c, a high-speed slitting machine with multiple blades can be used for cutting to obtain an oriented polypropylene flat ribbon with a width of 2-5 mm; a commercial weaving machine is used to weave the oriented flat ribbon according to the designed fabric structure to obtain plain, twill, satin or other three-dimensional polypropylene fabrics.
[0102] According to the present invention, in a preferred specific embodiment, the pressure is preferably maintained continuously during the hot pressing and cooling process without being reduced. The hot pressing process is carried out continuously, and preferably a continuous hot pressing composite material molding equipment consisting of a preheating machine, a crawler-type continuous flat hot press, a crawler-type continuous flat cooling press, a sheet cutting machine and a sheet stacking machine arranged in sequence is used; preferably, the crawler-type continuous flat hot press has a preheating unit, an independent heating and pressurizing unit, an air cooling unit and a lifting mechanism.
[0103] During the preparation, the polypropylene sheet and / or the polypropylene fabric and the polypropylene foam sheet are sequentially stacked and preheated by a preheater. The preheated samples are sequentially hot-pressed and fused by a crawler-type flat hot press, and then cooled and shaped by a crawler-type continuous flat cooling press to form a polypropylene composite foam sheet, i.e., a stacked hot-pressed product. Afterwards, the sheets are sliced by a sheet cutter as needed, and the hot-pressed products are stacked and arranged by a sheet stacker. The hot-pressing temperature is controlled by a preheating unit, an independent heating and pressing unit, and an air-cooling unit in the crawler-type flat hot press, and the hot-pressing pressure is controlled by a lifting mechanism. According to the research of the inventors, when the preparation process parameters are within the preferred range, preferably when the polymer foam sheet is prepared using the preparation equipment, the polymer composite foam sheet has better tensile strength, impact resistance, and interlayer peeling strength.
[0104] The third aspect of the present invention is to provide an application of the polypropylene composite foam sheet described in the first aspect or the polypropylene composite foam sheet prepared by the preparation method described in the second aspect in materials used in at least one of the following fields: automobiles, communications, aircraft, logistics, insulation, precision machinery and electronic turnover, and packaging.
[0105] Compared with the prior art, the present invention has the following beneficial effects:
[0106] (1) The polypropylene composite foam sheet provided by the present invention is a composite of a high-strength and high-impact polypropylene sheet and a polypropylene foam sheet. The polypropylene composite foam sheet has good tensile strength, impact resistance and interlayer peeling strength. The polypropylene composite material has the following characteristics:
[0107] The tensile strength in the longitudinal direction (MD) is ≥10 MPa, preferably ≥20 MPa; the interlayer peel strength is ≥0.8 N / mm, preferably ≥1.0 N / mm.
[0108] (2) Compared with the glass fiber nylon composite pre-set sheet or metal sheet reinforced molded body used in the currently common composite reinforced polypropylene composite foam sheet, the compatibility between the pre-set sheet and the matrix resin is greatly improved in the present invention, which can effectively reduce the apparent density and thermal conductivity of the product.
[0109] (3) The polypropylene foam sheet of the present invention can be prepared by various existing foaming and molding processes, and polypropylene foam sheets with different properties can be prepared by using different process methods and different types of foaming agents according to the needs of downstream applications.
[0110] (4) The polypropylene composite foamed sheets of the present invention are all polypropylene, and the components are more uniform. No separation treatment is required during recycling, and they can be directly used in other processing and application fields after crushing, melting and granulation, thereby reducing recycling costs.
[0111] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0112] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0113] In the following examples and comparative examples:
[0114] The extrusion calender and solid phase drawing equipment were purchased from Tianjin Hengrui Company, and the model was HRPC-800 three-layer co-extrusion plastic stretching sheet production line.
[0115] The polypropylene composition and sheet properties were tested according to the following methods:
[0116] The test results of composite sheets are shown in Table 1:
[0117] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682, where the test temperature is 230°C and the load is 2.16 kg;
[0118] (2) Density: measured according to the methods specified in GB / T 1033.1 and GB / T 6343;
[0119] (3) Melting point: measured according to the method specified in GB / T 28724;
[0120] (4) Tensile strength: measured according to the method specified in GB / T1040.1;
[0121] (5) Drop weight impact strength: measured according to the method specified in GB / T14153;
[0122] (6) Interlayer peel strength: measured according to the method specified in QB / T2358-98.
[0123] (7) Test method for thermal insulation capability of the composite foam sheet: The thermal conductivity is measured in accordance with the method specified in GB / T 10294.
[0124] In the following examples, the β-crystal nucleating agent with the brand name VP101B is sourced from Beijing Research Institute of Chemical Industry of Sinopec Corporation; the sources of some raw materials are described in the examples, and the other raw materials are commercially available unless otherwise specified.
[0125] Example 1
[0126] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0127] (1) Preparation of polypropylene composition A:
[0128] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate (melt mass flow rate) of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 11wt%, a melting point of 155°C, and an Izod impact strength of 23KJ / m 2 (23°C), the melt flow rate is 2.0 g / 10 min. The components prepared above are weighed and mixed according to the proportions, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight.
[0129] 0.05 parts by weight of a β-crystal nucleating agent of grade VP101B was added. The mixture was then added to a high-speed stirrer for uniform mixing, and then the mixed material was added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material entered the twin screw through the feeder. During the processing, the temperature of the screw was maintained between 200-230° C. The screw was melt-mixed uniformly, extruded, granulated and dried to obtain a polypropylene composition pellet A. The melting point of the polypropylene composition pellet A was found to be 157° C.
[0130] (2) Polypropylene composition B i Preparation:
[0131] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 8.9, a melt flow rate of 8.1 g / 10 min and a melting point of 130°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.6, a melt flow rate of 7.2 g / 10 min and a melting point of 135°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.3, a melt flow rate of 6.6 g / 10 min and a melting point of 140°C; component y is a polyolefin elastomer with a brand number of 6102, purchased from Exxon, and is an ethylene-propylene copolymer.
[0132] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction of component xi is W xi is 85 parts by weight, and the mass fraction of component y is W y The other steps are the same as step (1), and finally a polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3), after testing, the melting point of B1 is 127°C, the melting point of B2 is 132°C, and the melting point of B3 is 138°C.
[0133] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0134] The polypropylene composition A and the polypropylene composition B obtained in the above steps (1) and (2) are i The pellets are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering, and the polypropylene composition B is added to the core layer extruder of the multi-layer extrusion calendering. i Add to the upper and lower surface extruders of the multi-layer extrusion casting machine. After the pellets are co-extruded and compounded through the extruder die, they pass through the calendering roller and the traction roller in sequence, and then undergo solid phase stretching, trimming and winding to obtain sheets B1AB1, B2AB2, and B3AB3 respectively. Among them, the temperature of the extrusion casting is 230°C, and the temperature of the calendering roller is 58°C. The temperature during the solid phase stretching process is 140°C, the stretching rate is 2m / min, and the stretching ratio is 7 times.
[0135] The composite film (polypropylene sheet) made by stretching and rolling is composed of the upper surface layer (the outer layer of the film B i ), core layer (film A) and lower surface layer (outer film B i The thickness of the composite film is 80 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.
[0136] (4) Preparation of polypropylene fabric:
[0137] The three-layer co-extruded polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon is woven by a commercial weaving machine according to the designed fabric structure to obtain plain polypropylene fabrics B1AB1, B2AB2, B3AB3.
[0138] (5) Preparation of polypropylene composition for foamed sheet:
[0139] Take 5kg of the polypropylene composition A prepared in step (1) and 5kg of the polypropylene composition B3 pellets prepared in step (2), add 30g of antioxidant 1010, 100g of 2000 mesh commercial talc as a nucleating agent, and 200g of commercial graphite color powder, mix them in a high-speed mixer for 3 minutes, use a twin-screw extruder for granulation, the die temperature is 220°C, the screw speed is 300rpm, and the torque is 60%, to obtain a polypropylene composition AB3-1. The melt mass flow rate MFRB is detected to be 4.9g / 10min, and the melting point is 151°C.
[0140] (6) Preparation of polypropylene foam sheet
[0141] In the extrusion foaming device, 100 parts by weight of polypropylene composition resin particles (i.e., polypropylene composition AB3-1) are added to the screw extruder, the foaming temperature is 180°C, the foaming pressure is 150 bar, supercritical carbon dioxide is added as a foaming agent, and melt mixing is performed in the screw, the screw speed is 6rpm, and the extrusion amount is 50kg / h. The melt with the physical foaming agent evenly dispersed inside is extruded from the O-type die head. Due to the rapid reduction in pressure, the foaming agent escapes from the melt to form bubbles. It can be observed that the annular melt bundle is foamed, the appearance is white and delicate, and the bubbles are uniform. The annular melt bundle is cooled, shaped, cut, and pulled and rolled up, and the pulling speed is 3.2m / min. The thickness of the obtained polypropylene foam sheet is 1mm and the apparent density is 60.1g / L.
[0142] (7) Preparation of polypropylene composite foam sheet:
[0143] The polypropylene fabric obtained in the above step (4) is stacked in sequence, and the polypropylene fabric obtained in the above step (4) is stacked in sequence, from bottom to top, B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3, and the total number of stacked layers is 5. The two polypropylene foam sheets obtained in the above step 5 are placed on both sides thereof, and hot pressed to form a laminated polypropylene sheet. The polypropylene fabric is placed in a direction of 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 180s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene composite foam sheet is 2.35mm, wherein the total thickness of the reinforced composite sheet is 0.38mm.
[0144] Example 2
[0145] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0146] (1) Preparation of polypropylene composition A:
[0147] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 8wt%, a melting point of 155°C, a melt flow rate of 3.2g / 10min, and an cantilever beam impact strength of 25KJ / m 2 (23°C). The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 70 parts by weight, and the mass fraction Wbn of component b is 30 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade VP101B is added. Then the mixture is added to a high-speed stirrer and mixed evenly, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melt-mixed evenly, extruded, granulated and dried, a polypropylene composition pellet A is obtained. After testing, the melting point of the polypropylene composition pellet A is 161°C.
[0148] (2) Polypropylene composition B i Preparation:
[0149] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 8.4, a melting point of 128°C, and a melt flow rate of 7.8 g / 10 min; Component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.6, a melting point of 134°C, and a melt flow rate of 6.9 g / 10 min; Component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.1, a melting point of 142°C, and a melt flow rate of 5.2g / 10min; component y is a polyolefin elastomer produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene copolymer with an ethylene content of 15%wt, a melting point of 105°C, and a melt flow rate of 9g / 10min under a load of 2.16kg.
[0150] The components prepared above are weighed and mixed according to the ratio, wherein component x i The mass fraction W xi is 80 parts by weight, and the mass fraction of component y is W y The other steps are the same as step (1), and finally a polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3), after testing, the melting point of B1 is 126°C, the melting point of B2 is 133°C, and the melting point of B3 is 140°C.
[0151] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0152] The preparation process is the same as step (3) of Example 1.
[0153] (4) Preparation of polypropylene fabric:
[0154] The preparation process is the same as step (4) of Example 1.
[0155] (5) Preparation of polypropylene composition for foamed sheet:
[0156] The preparation process is the same as step (5) of Example 1, except that 5 kg of the polypropylene composition A prepared in step (1) of this example and 5 kg of the polypropylene composition B3 pellets prepared in step (2) are used to obtain a polypropylene composition AB3-2. The melt mass flow rate MFRB is 8.8 g / 10 min, and the melting point is 158°C.
[0157] (6) Preparation of polypropylene foam sheet
[0158] The preparation process is the same as step (6) of Example 1, except that the polypropylene composition AB3-2 prepared in the above step (6) is used as the base resin.
[0159] (7) Preparation of polypropylene composite foam sheet:
[0160] The polypropylene fabrics obtained in the above step (4) are stacked in sequence, and the polypropylene fabrics obtained in the above step (4) are stacked in sequence, from bottom to top, B3AB3, B2AB2, B1AB1, B2AB2, B3AB3, and the total number of stacked layers is 5, and two sheets are prepared respectively. Then, a piece of polypropylene foam sheet obtained in the above step 5 is placed in the middle, and hot pressed to form a laminated polypropylene sheet. The polypropylene fabric is placed in a direction of 90° between the warp and the warp. The hot pressing conditions used are: temperature 152°C, hot pressing pressure 5.5MPa, preheating time 240s, hot pressing time 200s, and cooling time 600s. The thickness of the prepared polypropylene composite foam sheet is 1.75mm, wherein the total thickness of the reinforced composite sheet is 0.78mm.
[0161] Example 3
[0162] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0163] (1) Preparation of polypropylene composition A:
[0164] The preparation process is the same as step (1) of Example 1.
[0165] (2) Polypropylene composition B i Preparation:
[0166] The preparation process is the same as step (2) of Example 1.
[0167] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0168] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 80 μm, wherein the thickness of the film layer A accounts for 90% of the total thickness of the sheet.
[0169] (4) Preparation of polypropylene fabric:
[0170] The preparation process is the same as step (4) of Example 1.
[0171] (5) Preparation of polypropylene composition for foamed sheet:
[0172] The preparation process is the same as step (5) of Example 1.
[0173] (6) Preparation of polypropylene foam sheet
[0174] The preparation process is the same as step (6) of Example 1.
[0175] (7) Preparation of polypropylene composite foam sheet:
[0176] The preparation process is the same as step (7) of Example 1.
[0177] The thickness of the prepared polypropylene composite foam sheet is close to that of Example 1.
[0178] Example 4
[0179] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0180] (1) Preparation of polypropylene composition A:
[0181] The preparation process is the same as step (1) of Example 1.
[0182] (2) Polypropylene composition B i Preparation:
[0183] The preparation process is the same as step (2) of Example 1.
[0184] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0185] The main preparation process is the same as step (3) of Example 1, wherein the sheet stretching ratio is 10 times.
[0186] (4) Preparation of polypropylene fabric:
[0187] The preparation process is the same as step (4) of Example 1.
[0188] (5) Preparation of polypropylene composition for foamed sheet:
[0189] The preparation process is the same as step (5) of Example 1.
[0190] (6) Preparation of polypropylene foam sheet
[0191] The preparation process is the same as step (6) of Example 1.
[0192] (7) Preparation of polypropylene composite foam sheet:
[0193] The preparation process is the same as step (7) of Example 1.
[0194] The thickness of the prepared polypropylene composite foam sheet is close to that of Example 1.
[0195] Example 5
[0196] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0197] (1) Preparation of polypropylene composition A:
[0198] The preparation process is the same as step (1) of Example 1.
[0199] (2) Polypropylene composition B i Preparation:
[0200] The preparation process is the same as step (2) of Example 1.
[0201] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0202] The preparation process is the same as step (3) of Example 1.
[0203] (4) Preparation of polypropylene fabric:
[0204] The preparation process is the same as step (4) of Example 1.
[0205] (5) Preparation of polypropylene composition for foamed sheet:
[0206] The preparation process is the same as step (5) of Example 1.
[0207] (6) Preparation of polypropylene foam sheet
[0208] The preparation process is the same as step (6) of Example 1.
[0209] (7) Preparation of polypropylene composite foam sheet:
[0210] The main steps are the same as step (7) of Example 1. The difference is that the polypropylene fabrics obtained in the above step (4) are stacked in sequence, from bottom to top, B3AB3, B2AB2, B1AB1, B2AB2, B3AB3, the total number of stacked layers is 5, and three sheets are made. Then the 4 polypropylene foam sheets obtained in the above step 5 are respectively inserted between the upper and lower sides and both ends of the 3 stacked sheets, and hot pressed to form a laminated polypropylene sheet. The polypropylene fabric is placed in the direction of 90° between the warp and the warp. The hot pressing conditions used are: temperature 155°C, hot pressing pressure 6.5MPa, preheating time 240s, hot pressing time 300s, and cooling time 600s. The thickness of the prepared polypropylene composite foam sheet is 5.01mm, of which the total thickness of the reinforced composite sheet is 1.11mm.
[0211] Example 6
[0212] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0213] (1) Preparation of polypropylene composition A:
[0214] The preparation process is the same as step (1) of Example 1.
[0215] (2) Polypropylene composition B i Preparation:
[0216] The preparation process is the same as step (2) of Example 1.
[0217] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0218] The preparation process is the same as step (3) of Example 1.
[0219] (4) Preparation of polypropylene composition for foamed sheet:
[0220] The preparation process is the same as step (5) of Example 1.
[0221] (5) Preparation of polypropylene foam sheet
[0222] The preparation process is the same as step (6) of Example 1.
[0223] (6) Preparation of polypropylene composite foam sheet:
[0224] The polypropylene fabric was not prepared, but the three-layer co-extruded polypropylene sheet prepared in step (3) was used to replace the polypropylene fabric obtained in step (4) of Example 1, and the three-layer co-extruded polypropylene sheet was laminated and hot-pressed in sequence according to step (5) of Example 1. The thickness of the prepared polypropylene composite foam sheet was 2.38 mm, wherein the total thickness of the reinforced composite sheet was 0.39 mm.
[0225] Example 7
[0226] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0227] (1) Preparation of polypropylene composition A:
[0228] The preparation process is the same as step (1) of Example 1.
[0229] (2) Polypropylene composition B i Preparation:
[0230] The preparation process is the same as step (2) of Example 1.
[0231] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0232] The preparation process is the same as step (3) of Example 1.
[0233] (4) Preparation of polypropylene fabric:
[0234] The preparation process is the same as step (4) of Example 1.
[0235] (5) Preparation of polypropylene composition for foamed sheet:
[0236] The preparation process is the same as step (5) of Example 1. The preparation process is the same as step (6) of Example 1, except that 0.5 kg of the polypropylene composition A prepared in step (1) and 9.5 kg of the polypropylene composition B3 pellets prepared in step (2) are taken. The melt mass flow rate MFRA is detected to be 4.6 g / 10 min; the melting point of the polypropylene composition AB3-3 is 139°C.
[0237] (6) Preparation of polypropylene foam sheet:
[0238] The preparation process is the same as step (6) of Example 1, except that the polypropylene composition AB3-3 is used as the base resin.
[0239] (7) Preparation of polypropylene composite foam sheet:
[0240] The preparation process is the same as step (7) of Example 1.
[0241] The thickness of the prepared polypropylene composite foam sheet is close to that of Example 1.
[0242] Example 8
[0243] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0244] (1) Preparation of polypropylene composition A:
[0245] The preparation process is the same as step (1) of Example 1.
[0246] (2) Polypropylene composition B i Preparation:
[0247] The preparation process is the same as step (2) of Example 1.
[0248] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0249] The preparation process is the same as step (3) of Example 1.
[0250] (4) Preparation of polypropylene fabric:
[0251] The preparation process is the same as step (4) of Example 1.
[0252] (5) Preparation of polypropylene composition for foamed sheet:
[0253] The preparation process is the same as step (6) of Example 1, except that 9.5 kg of the polypropylene composition A prepared in step (1) and 0.5 kg of the polypropylene composition B3 pellets prepared in step (2) of this example are taken. The melt mass flow rate MFR is 5.2 g / 10 min, and the melting point of the polypropylene composition AB3-4 is 157°C.
[0254] (6) Preparation of polypropylene foam sheet
[0255] The preparation process is the same as step (6) of Example 1, except that the polypropylene composition AB3-4 is used as the base resin.
[0256] (7) Preparation of polypropylene composite foam sheet:
[0257] The preparation process is the same as step (7) of Example 1.
[0258] The thickness of the prepared polypropylene composite foam sheet is close to that of Example 1.
[0259] Example 9
[0260] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0261] (1) Preparation of polypropylene composition A:
[0262] The preparation process is the same as step (1) of Example 1.
[0263] (2) Polypropylene composition B i Preparation:
[0264] The preparation process is the same as step (2) of Example 1.
[0265] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0266] The preparation process is the same as step (3) of Example 1.
[0267] (4) Preparation of polypropylene fabric:
[0268] The preparation process is the same as step (4) of Example 1.
[0269] (5) Preparation of polypropylene composition for foamed sheet:
[0270] The preparation process is the same as step (5) of Example 1.
[0271] (6) Preparation of polypropylene foam sheet
[0272] The preparation process is the same as step (6) of Example 1.
[0273] (7) Preparation of polypropylene composite foam sheet:
[0274] The preparation process is the same as step (7) of Example 1. The difference is that the polypropylene fabrics obtained in the above step (4) are stacked in sequence, from bottom to top, B3AB3, B2AB2, B1AB1, B2AB2, B3AB3, and the total number of cyclic stacking layers is 15 layers. The two polypropylene foam sheets obtained in the above step 5 are placed on both sides thereof and hot pressed to form a laminated polypropylene sheet. The polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 180s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene composite foam sheet is 3.11mm, of which the total thickness of the reinforced composite sheet is 1.14mm.
[0275] Example 10
[0276] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0277] (1) Preparation of polypropylene composition A:
[0278] The preparation process is the same as step (1) of Example 1.
[0279] (2) Polypropylene composition B i Preparation:
[0280] The preparation process is the same as step (2) of Example 1.
[0281] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0282] The preparation process is the same as step (3) of Example 1.
[0283] (4) Preparation of polypropylene fabric:
[0284] The preparation process is the same as step (4) of Example 1.
[0285] (5) Preparation of polypropylene composition for foamed sheet:
[0286] The preparation process is the same as step (5) of Example 1.
[0287] (6) Preparation of polypropylene foam sheet
[0288] The preparation process is the same as step (6) of Example 1.
[0289] (7) Preparation of polypropylene composite foam sheet:
[0290] The preparation process is the same as step (7) of Example 1. The difference is that the polypropylene fabrics prepared in the above step (4) are stacked in order, from bottom to top, B3AB3, B2AB2, B1AB1, B2AB2, B3AB3, and the number of layers is 5. A 1 mm foam sheet prepared in step (6) is placed on top of the stacked sheets. The thickness of the prepared polypropylene composite foam sheet is 1.38 mm, wherein the total thickness of the reinforced composite sheet is 0.38 mm.
[0291] Embodiment 11
[0292] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition, polypropylene foam sheet and polypropylene composition composite foam sheet provided by the present invention.
[0293] (1) Preparation of polypropylene composition A:
[0294] The preparation process is the same as step (1) of Example 1.
[0295] (2) Polypropylene composition B i Preparation:
[0296] The preparation process is the same as step (2) of Example 1.
[0297] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0298] The preparation process is the same as step (3) of Example 1.
[0299] (4) Preparation of polypropylene fabric:
[0300] The preparation process is the same as step (4) of Example 1.
[0301] (5) Preparation of polypropylene composition for foamed sheet:
[0302] The preparation process is the same as step (5) of Example 1.
[0303] (6) Preparation of polypropylene foam sheet
[0304] The mold installed between the molding presses was heated to a foaming temperature of 158°C, and the sheet prepared by extruding the polypropylene composition in step (5) was placed therein. The molding presses were closed and the molds were sealed. The gas generated by the foaming agent was diffused into the polypropylene composition resin particles, and the foaming pressure was 105 bar. After saturation for 1.2 hours, diffusion equilibrium was reached, and the pressure was released once through the pressure relief valve to open the mold for foaming, and the foaming was cooled and shaped to obtain a polypropylene composition foamed sheet with a density of 59.9 g / L, which was then cut to obtain a polypropylene foamed sheet with a thickness of 1 mm.
[0305] (7) Preparation of polypropylene composite foam sheet:
[0306] The main steps are the same as step (7) of Example 1, except that the molded foamed polypropylene sheet provided in step (6) is used. The thickness of the prepared polypropylene composite foamed sheet is close to that of Example 1.
[0307] Comparative Example 1
[0308] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 80 μm.
[0309] The preparation process of the polypropylene composition for foam sheet is the same as step (5) of Example 1, except that only polypropylene composition A is used. The preparation process of the polypropylene foam sheet is the same as step (6) of Example 1. The preparation process of the polypropylene composite foam sheet is the same as step (7) of Example 1, and a polypropylene composition composite foam sheet is obtained, and the thickness is close to that of Example 1.
[0310] Comparative Example 2
[0311] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1 except that only polypropylene composition B was used. i The extrusion casting was a single-layer film with a thickness of 80 μm. A polypropylene fabric was prepared according to the method of Example 1.
[0312] The preparation process of the polypropylene composition for the foamed sheet is the same as step (5) of Example 1, except that only the polypropylene composition B is used. i The preparation process of the polypropylene foam sheet is the same as step (6) of Example 1, and the preparation process of the polypropylene composite foam sheet is the same as step (7) of Example 1, to obtain a polypropylene composition composite foam sheet with a thickness close to that of Example 1.
[0313] Comparative Example 3
[0314] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that the polypropylene composition A contained only component b. A polypropylene fabric was prepared according to the method of Example 1.
[0315] The preparation process of the polypropylene composition for the foam sheet is the same as step (5) of Example 1, except that only component b is used in the polypropylene composition A. The preparation process of the polypropylene foam sheet is the same as step (6) of Example 1, and the preparation process of the polypropylene composite foam sheet is the same as step (7) of Example 1, to obtain a polypropylene composition composite foam sheet with a thickness close to that of Example 1.
[0316] Comparative Example 4
[0317] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1. i The polypropylene fabric was prepared according to the method of Example 1.
[0318] The preparation process of the polypropylene composition for foaming sheet is the same as step (5) of Example 1, except that the polypropylene composition B i The polypropylene foam sheet is prepared in the same manner as step (6) of Example 1, and the polypropylene composite foam sheet is prepared in the same manner as step (7) of Example 1 to obtain a polypropylene composite foam sheet having a thickness close to that of Example 1.
[0319] Comparative Example 5
[0320] A coextruded polypropylene sheet was prepared according to the method of Example 6, except that component B i The materials are selected in the following manner: component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; the melt flow rates of components x1-x3 are all 2-10g / 10min.
[0321] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3), after testing, the melting point of B1 is 138° C., the melting point of B2 is 132° C., and the melting point of B3 is 127° C. According to the method of Example 1, a polypropylene fabric is prepared.
[0322] The preparation process of the polypropylene composition for foam sheet is the same as step (5) of Example 1, the preparation process of the polypropylene foam sheet is the same as step (6) of Example 1, and the preparation process of the polypropylene composite foam sheet is the same as step (7) of Example 1, to obtain a polypropylene composition composite foam sheet with a thickness close to that of Example 1.
[0323] Comparative Example 6
[0324] The preparation process of the polypropylene composition for the foam sheet is the same as step (5) of Example 1, the preparation process of the polypropylene foam sheet is the same as step (6) of Example 1, and the preparation process of the polypropylene composite foam sheet is the same as step (7) of Example 1, except that the foaming temperature is 200° C., the foaming pressure is 120 bar, and only two pieces of the polypropylene foam sheets prepared in step (6) are hot-pressed and composited, with a thickness of 1.95 mm and a density of 180 g / L.
[0325] Comparative Example 7
[0326] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.
[0327] The preparation process of the polypropylene composition for the foam sheet is the same as step (5) of Example 1, the preparation process of the polypropylene foam sheet is the same as step (6) of Example 1, and the preparation process of the polypropylene composite foam sheet is the same as step (7) of Example 1, except that the polypropylene fabrics obtained in the above step (4) are stacked in sequence, from bottom to top, B3AB3, B2AB2, B1AB1, B2AB2, B3AB3, and the total number of cyclic stacking layers is 50 layers. Two polypropylene foam sheets are placed on both sides thereof and hot pressed to form a laminated polypropylene sheet. Among them, the total thickness of the reinforced composite sheet is 3.88mm. As a result, a polypropylene composition composite foam sheet of qualified quality was not obtained, and the layers were not tightly adhered to each other, and even warped and cracked.
[0328] Comparative Example 8
[0329] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.
[0330] The preparation process of the polypropylene composition for the foam sheet is the same as step (5) of Example 1, the preparation process of the polypropylene foam sheet is the same as step (6) of Example 1, and the preparation process of the polypropylene composite foam sheet is the same as step (7) of Example 1, except that a square glass fiber / nylon composite sheet with a thickness of 0.4 mm is compounded between two polypropylene foam sheets prepared in step (6) to obtain a polypropylene composition composite foam sheet with a thickness close to that of Example 1.
[0331] Comparative Example 9
[0332] The preparation process of the polypropylene composition for the foam sheet is the same as step (5) of Example 1, the preparation process of the polypropylene foam sheet is the same as step (6) of Example 11, and the preparation process of the polypropylene composite foam sheet is the same as step (7) of Comparative Example 6, except that the foaming temperature is 150°C and the foaming pressure is 85 bar. The polypropylene composition foam sheet is obtained with a thickness of 1.95 mm and a density of 180 g / L.
[0333] Comparative Example 10.
[0334] The preparation process of the polypropylene composition for the foam sheet is the same as step (5) of Example 1, the preparation process of the polypropylene foam sheet is the same as step (6) of Example 11, and the preparation process of the polypropylene composite foam sheet is the same as step (7) of Comparative Example 8, to obtain a polypropylene composition composite foam sheet with a thickness close to that of Example 1.
[0335] Experimental example
[0336] The polypropylene composite foam sheets obtained in the above examples and comparative examples were tested according to the following method. The test results are shown in Table 1.
[0337] (1) Tensile strength: Prepare samples and measure them according to the method specified in GB / T1040.1-2018;
[0338] (2) Interlayer peel strength: Sample preparation and measurement shall be carried out according to the method specified in QB / T2358-98.
[0339] (3) Drop weight impact strength: measured according to the method specified in GB / T14153-1993.
[0340] (4) The apparent density of the composite foam sheet shall be prepared and measured according to the method specified in GB / T6343.
[0341] (5) The thermal conductivity of the composite foam sheet shall be prepared and measured according to the method specified in GB / T 10294.
[0342] Table 1
[0343]
[0344]
[0345] The strength of the composite foam sheet obtained by the test is determined by the weakest part. The polypropylene composite foam sheet of the present invention is a polypropylene composite sheet reinforced foam sheet. As can be seen from the examples, the tensile properties are greatly improved compared with comparative examples 6 and 9 without composite reinforcement. The peel strength should also depend on the ability of the weakest foam sheet and the reinforced sheet inside the foam sheet to adhere to each other. As can be seen from the examples, the peel strength of the polypropylene composite foam sheet of the present invention has been greatly improved compared with comparative examples 8 and 10.
[0346] It can be seen from the results of the embodiment in Table 1 that, compared with the common foam sheets without composite reinforcement in Comparative Examples 6 and 9, the polypropylene composite foam sheet prepared according to the present invention has both good tensile properties and good interlayer peeling strength at a lower hot pressing temperature without significantly reducing its thermal insulation ability.
[0347] From Examples 7 and 8, it can be seen that the polypropylene composition A and B of the foam sheet matrix resin are regulated. i The ratio has no significant effect on the performance of the final product.
[0348] From Comparative Examples 1-4, it can be seen that only using a single-layer sheet structure, a single polymer component, or using an interlayer ratio outside the scope of the embodiment will lead to a decrease in the performance of the laminated polypropylene sheet or fabric, thereby causing a decrease in various properties of the final composite foam sheet. Comparative Example 5 verifies that the melting point does not follow the gradient in this application and the inventive effect cannot be achieved.
[0349] Comparative Example 7 of the present invention did not obtain qualified products. It can be seen from Examples 5, 9, 10 and Comparative Example 7 that the amount of polypropylene fabric and the amount of foamed sheets have a significant impact on the final product. With the increase of the amount of fabric and the amount of foamed sheets, the physical properties are improved. When the number of added sheets is too high, it is difficult to obtain a foamed product of qualified quality.
[0350] From Comparative Examples 8 and 10, it can be seen that although the use of glass fiber / nylon composite sheets and other commonly used sheet composite reinforcement means in the industry can also improve the physical properties of the composite foamed sheet to the level of the embodiment, due to the poor compatibility of the reinforced sheet with the polypropylene foamed sheet, the peel strength and thermal insulation performance are greatly reduced. The apparent density is also significantly improved.
[0351] From Example 11 and Comparative Examples 9 and 10, the physical properties of the foamed sheets prepared by different foaming processes will change to a certain extent before and after composite reinforcement due to the different pore structures brought about by different processes, but the difference is not significant; and the change trends of their physical properties after composite reinforcement under the same conditions are basically the same.
[0352] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0353] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A polypropylene composite foam sheet having a laminated structure, comprising at least one layer of a reinforced composite sheet and at least one layer of a polypropylene foam sheet bonded to the reinforced composite sheet by hot pressing fusion; Each layer of the reinforced composite sheet comprises at least one layer of polypropylene sheet and / or at least one layer of polypropylene fabric woven from polypropylene sheets; wherein, The polypropylene sheet comprises a layer A and layers B and B' located on both sides of the layer A, and has a structure of BAB'; Wherein layer A contains polypropylene composition A, layer B and layer B' are the same or different, and each correspondingly contains polypropylene composition B and polypropylene composition B', wherein the polypropylene composition A includes homopolymer polypropylene a and impact copolymer polypropylene b; the polypropylene composition B and the polypropylene composition B' each include random copolymer polypropylene x and thermal bonding enhancer y; The melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'.
2. The polypropylene composite foam sheet according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b; and / or, Based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each include 70-99wt% of random copolymer polypropylene x and 1-30wt% of thermal adhesion enhancer y; preferably, the polypropylene composition B and the polypropylene composition B' each include 80-90wt% of random copolymer polypropylene x and 10-20wt% of thermal adhesion enhancer y.
3. The polypropylene composite foam sheet according to claim 1, characterized in that: Based on the total thickness of the polypropylene sheet, the thickness of the layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%; and / or, The melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene compositions B and B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees; and / or, The difference between the melting points of the polypropylene composition A and the polypropylene composition B and the difference between the melting points of the polypropylene composition A and the polypropylene composition B' are each equal to or greater than 5°C, preferably equal to or greater than 10°C, more preferably equal to or greater than 20°C.
4. The polypropylene composite foam sheet according to claim 1, characterized in that: The homopolymer polypropylene a has: The melting point is 150-170°C, preferably 160-170°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The isotacticity (mm) is not less than 96%.
5. The polypropylene composite foam sheet according to claim 1, characterized in that: The melting point of the impact-resistant copolymer polypropylene b is 150-170° C.: and / or, The monomer of the impact copolymer polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or, The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 .
6. The polypropylene composite foam sheet according to claim 1, characterized in that: The random copolymer polypropylene x has: The melting point is 110-150°C, preferably 120-140°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or, The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or, It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.
7. The polypropylene composite foam sheet according to claim 1, characterized in that: The thermal bonding enhancer y has: The melting point or viscosity flow temperature is 70-110°C; and / or, The melt flow rate at 190°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or, One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, and petroleum resin; preferably, polyolefin elastomer and / or petroleum resin.
8. The polypropylene composite foam sheet according to claim 7, characterized in that: The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or alpha olefin, wherein the alpha olefin is preferably a C4-C12 alpha olefin, more preferably 1-butene and / or 1-octene; and / or, The petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150° C. and is preferably a cyclopentadiene type resin.
9. The polypropylene composite foam sheet according to claim 1, characterized in that: The layer A also contains a β-crystalline nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or, Relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.
10. The polypropylene composite foam sheet according to any one of claims 1 to 9, characterized in that: The polypropylene foam sheet contains a polypropylene composition, preferably the polypropylene foam sheet contains at least one of the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B', and an optional auxiliary agent; preferably, the auxiliary agent is selected from one or more of an antioxidant, an antistatic agent, a lubricant, an anti-aging agent, a flame retardant, and a toner; and / or, The polypropylene foam sheet is foamed by an inorganic physical foaming agent and / or contains a foaming agent; preferably, the inorganic physical foaming agent is selected from at least one of air, nitrogen, carbon dioxide, oxygen and water; and / or, the foaming agent is selected from a chemical foaming agent and / or an organic physical foaming agent; more preferably, the chemical foaming agent is selected from at least one of azodicarbonamide, p-toluenesulfonyl hydrazide, semicarbazides, tetrazoles, sodium bicarbonate and sodium citrate; the organic physical foaming agent is selected from at least one of an aliphatic hydrocarbon foaming agent, an alicyclic hydrocarbon foaming agent, and a halogenated hydrocarbon foaming agent.
11. The polypropylene composite foam sheet according to any one of claims 1 to 9, characterized in that: Each layer of the reinforced composite sheet comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the reinforced composite sheet is nth group...ith group...2nd group, 1st group, 2nd group...ith group...nth group from bottom to top, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group; preferably, Polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1th group is the same or different, and is 1-40°C, preferably 1-10°C, more preferably 1-5°C; and / or, 3≤n≤23, preferably, 3≤n≤16; and / or, Each group of polypropylene ply units, independently of one another, comprises 1 to 10, preferably 1 to 5, identical or different polypropylene ply units.
12. The polypropylene composite foam sheet according to any one of claims 1 to 9, characterized in that: The polypropylene composite foam sheet has a multi-layer sandwich structure; and / or, Based on the total thickness of the polypropylene composite foam sheet, the total thickness of the reinforced composite sheet accounts for 5%-60%, preferably 15%-45% of the total thickness of the polypropylene composite foam sheet; and / or, The total number of layers of all polypropylene sheets and polypropylene fabrics and the polypropylene foamed sheet is 6-50 layers, more preferably 7-35 layers; and / or, The polypropylene foam sheets are stacked in order from top to bottom at 0-90 degrees along their respective machine directions, with 1 to 6 layers, and most preferably 2 to 4 layers; and / or, The reinforced composite sheets are stacked in order from top to bottom at 0-90° along their respective machine directions, preferably, the total number of polypropylene sheets and polypropylene fabrics in each layer of the reinforced composite sheet is 5-45 layers, most preferably 5-30 layers; and / or, The polypropylene composite foam sheet is prepared by the following method: Laminating at least one group of the polypropylene sheets and / or the polypropylene fabric with at least one layer of the polypropylene foam sheet, fusing them by hot pressing, and then cooling and shaping to obtain the polypropylene composite foam sheet; Wherein, each group of the polypropylene sheets and / or the polypropylene fabrics are stacked in the order of forming the reinforced composite sheets of the corresponding layers.
13. A method for preparing the polypropylene composite foam sheet according to any one of claims 1 to 12, comprising laminating at least one group of the polypropylene sheets and / or the polypropylene fabric with at least one layer of the polypropylene foam sheet, fusing them by hot pressing, and then cooling and shaping to obtain the polypropylene composite foam sheet; preferably, Each group of the polypropylene sheets and / or the polypropylene fabrics are stacked in the order of forming the reinforced composite sheets of the corresponding layers.
14. The preparation method according to claim 13, characterized in that: The hot pressing temperature is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or, the hot pressing pressure is 2-10MPa, the preheating time is 5-600s, the hot pressing time is 1-900s, and preferably 10-600s; and / or, the cooling pressure is 2-8MPa, and the cooling time is 30-900s.
15. Use of the polypropylene composite foam sheet according to any one of claims 1 to 12 or the polypropylene composite foam sheet prepared by the preparation method according to any one of claims 13 to 14 in materials used in at least one of the following fields: automobiles, communications, aircraft, logistics, thermal insulation, precision machinery and electronic turnover, and packaging.
Citation Information
Patent Citations
Low-density toughened polypropylene foam material composition, low-density toughened polypropylene foam material and preparation method of low-density toughened polypropylene foam material
CN115850783A
High-adhesiveness and high-impact polypropylene composite film as well as preparation method and application thereof
CN115991033A
Low-haze high-impact-resistance coloring heat-sealing polypropylene composite film as well as preparation method and application thereof
CN115991040A
Foamable polyolefin compositions and methods thereof
US20190382549A1