Preparation method and application of silylene-based composite structure material for 3D printing
The preparation of silenium composite structural materials through 3D printing technology solves the complex problems of the existing porous material preparation process, realizes efficient storage of hydrogen and precise regulation of material structure, and is suitable for hydrogen storage and other gas adsorption applications.
Patent Information
- Application Number
- CN202410769462.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The existing porous materials preparation process is complex, and it is difficult to regulate the material structure through simple processes, which limits the efficient storage capacity of hydrogen storage materials.
Using 3D printing technology, silene nanosheets are mixed with graphene oxide and cellulose nanofibers to prepare a continuous-grade porous three-dimensional structure through direct-write 3D printing, simplifying the process and improving hydrogen storage performance.
It realizes efficient storage of hydrogen, simplifies the preparation process, and improves the active sites and mechanical properties of the material through precise control of the structure, and is suitable for hydrogen storage and other gas adsorption media.
Smart Images

Figure CN118908149A_ABST
Abstract
Description
Technical field:
[0001] The present invention relates to the technical field of hydrogen storage material preparation, and in particular to a preparation method and application of a 3D printed silicene-based composite structural material. Background technology:
[0002] Hydrogen energy is recognized as a clean energy that can replace fossil fuels. Hydrogen storage has always been the biggest bottleneck and obstacle restricting the large-scale use of hydrogen energy. Exploring suitable hydrogen storage materials is still one of the main research directions in the field of hydrogen storage today.
[0003] Studies have found that the structural characteristics of materials have an important influence on their hydrogen storage capacity. Among them, porous materials have been widely studied in the field of hydrogen storage because of their large specific surface area, rich pore structure and active sites. A Chinese patent discloses a platinum-loaded nitrogen / sulfur co-doped porous carbon nanofiber material and its preparation and application (authorization announcement number: CN113089136B). The porous composite material can significantly improve the catalytic activity and mass hydrogen storage density. A Chinese patent discloses a cobalt-sulfur hydrogen storage composite material containing porous polyaniline / reduced graphene oxide and its preparation method (application publication number: CN113054181A). The 3D network structure of the composite material can greatly improve the hydrogen storage performance of the cobalt-sulfur alloy. However, the preparation processes of the porous materials involved in these reports are relatively complicated. How to combine the advantages of the materials themselves and realize the regulation and preparation of porous materials through simple processes is the current research focus and difficulty in the field of hydrogen storage materials.
[0004] It should be noted that the above contents belong to the technical knowledge of the inventor and do not necessarily constitute prior art. Summary of the invention:
[0005] The purpose of the present invention is to solve the problems existing in the prior art and provide a preparation method and application of 3D printed silicene-based composite structural materials. Silicene nanosheets are used as the basic material, mixed with graphene oxide and cellulose nanofibers to prepare printing ink, and a three-dimensional structure with continuous hierarchical porosity is prepared by direct writing 3D printing, which not only simplifies the preparation process but also realizes efficient storage of hydrogen.
[0006] The present invention achieves the above-mentioned purpose by adopting the following technical solutions:
[0007] A method for preparing a 3D printed silicene-based composite structural material comprises the following steps:
[0008] (1) adding silicene nanosheets and graphene oxide to a cellulose nanofiber aqueous solution in sequence, and performing ultrasonic dispersion each time to obtain a high-concentration fluid; and subjecting the high-concentration fluid to planetary degassing stirring and centrifugal treatment to obtain a 3D printing ink;
[0009] (2) using the 3D printing ink obtained in step (1) and printing a three-dimensional structure using a direct writing 3D printer;
[0010] (3) The three-dimensional structure printed in step (2) is freeze-dried and high-temperature reduced to prepare a silicene-based composite structural material.
[0011] The mass solubility of the cellulose nanofiber aqueous solution in step (1) is 0.5-1.5%, and the mass ratio of the silicene nanosheets, graphene oxide and cellulose nanofiber aqueous solution is: 1-2: 1-5: 100-130.
[0012] The power of the ultrasonic dispersion in step (1) is 200W, the dispersion time is 30min, the rotation speed of the planetary deaeration stirring is 1500-2000r / min, the time is 15-30min, and the rotation speed of the centrifugal treatment is 1500-2000r / min, and the time is 3-8min.
[0013] In step (2), the 3D printing ink obtained in step (1) is loaded into the syringe of a direct writing 3D printer, the diameter of the printing needle in the direct writing 3D printer is 300 to 500 μm, and the direct writing 3D printer deposits the 3D printing ink into a three-dimensional structure by printing in a three-dimensional space. The moving speed of the printing needle is 8 to 12 mm / s, and the gas pressure is 40 to 60 psi.
[0014] In step (3), the printed three-dimensional structure is placed in a refrigerator for 12 hours, freeze-dried at a temperature of -40 to -60°C for 48 to 72 hours, the dried three-dimensional structure is placed in a crucible, and the crucible is placed in a tubular atmosphere furnace, and reduced at a high temperature of 700 to 1000°C for 2 to 6 hours in a high-purity argon atmosphere to obtain a 3D printed silicene-based composite structure material.
[0015] In step (1), the silicene nanosheet is prepared by a topological chemical method, comprising the following steps:
[0016] (1) CaSi2 is placed in a NaOH solution, then filtered and dried to obtain product A;
[0017] (2) SnCl2 is added to methanol and stirred until it is completely dissolved to obtain a mixed solution, product A and sodium dodecylbenzene sulfonate are added to the mixed solution in sequence and stirred, and then placed in a constant temperature water bath for reaction. After the reaction is completed, product B is obtained, and product B is washed by centrifugation with methanol and methanol solution of hydrogen chloride, respectively, filtered and vacuum dried; finally, silicene nanosheets are obtained by supercritical drying.
[0018] The concentration of the NaOH solution is 2 mol / L, and the CaSi2 is allowed to stand in the NaOH solution for 10 min.
[0019] The temperature of the constant temperature water bath was set at 60° C., and the reaction time was 24 h.
[0020] The product B was washed three times by centrifugation with methanol and 5 wt% methanol solution of hydrogen chloride, respectively, filtered and vacuum dried at 80° C. for 24 h, and finally supercritically dried for 4 h.
[0021] In step (1), the graphene oxide is prepared by a modified Hummers method, comprising the following steps:
[0022] Pour sodium nitrate, flake graphite powder and concentrated sulfuric acid into a container, force stirring in an ice water bath, then add KMnO4 and stir, increase the water bath temperature twice in sequence to react respectively, after the reaction is completed, add hydrogen peroxide and let it stand, use deionized water to centrifuge and wash it to near neutrality, then perform ultrasonic and centrifugal treatment to obtain a thick slurry at the bottom, freeze-dry the bottom thick slurry in a vacuum freeze dryer to obtain graphene oxide dry powder, and store it in a vacuum for later use.
[0023] The water bath temperature was first raised to 35°C for 45 min, and then raised to 90°C for 15 min.
[0024] The ultrasonic dispersion was carried out for 30 minutes and the centrifugal treatment was carried out for 15 minutes.
[0025] The application of the 3D printed silicene-based composite structural material prepared above in the preparation of hydrogen storage products, capacitors and batteries.
[0026] The present invention adopts the above structure, which can bring the following beneficial effects:
[0027] (1) The hydrogen storage potential of silicene nanosheets and graphene is fully utilized, combined with the rich functional groups on the surface of cellulose nanofibers, to form a three-dimensional structure with certain hydrogen storage capacity and mechanical properties; at the same time, the three-dimensional structural material has abundant continuous layered pores, which can increase the active sites of the composite material and realize efficient storage of hydrogen.
[0028] (2) By adopting 3D printing technology, the preparation process is simple, the structure can be precisely controlled, and it has strong practical application value;
[0029] (3) The 3D printed silicene-based composite structural material obtained by the present invention is not only suitable for applications in the field of hydrogen storage, but can also be used as a medium for adsorption of other gases. Description of the drawings:
[0030] Figure 1 XRD diagrams of silicene nanosheets, graphene oxide, and 3D printed silicene-based composite structural materials of the present invention;
[0031] Figure 2 is a rheological property curve diagram of the 3D printing ink of the present invention;
[0032] Figure 3 This is a SEM image of the 3D printed silicene-based composite structure material of the present invention;
[0033] Figure 4 This is the FT-IR image of the 3D printed silicene-based composite structure material of the present invention;
[0034] Figure 5 This is a PCT curve diagram of hydrogen storage of the 3D printed silicene-based composite structure material of the present invention;
[0035] Figure 6 This is a hydrogen storage kinetics curve diagram of the 3D printed silicene-based composite structure material of the present invention; Specific implementation method:
[0036] In order to more clearly illustrate the overall concept of the present invention, a detailed description is given below in an exemplary manner in conjunction with the accompanying drawings.
[0037] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0038] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0039] Example 1
[0040] A method for preparing a 3D printed silicene-based composite structural material comprises the following steps:
[0041] (1) 80 mg of silicene nanosheets and 200 mg of graphene oxide were sequentially added to a cellulose nanofiber aqueous solution with a mass concentration of 0.5%, and ultrasonic dispersion (power of 200 W, dispersion time of 30 min) was performed each time to obtain a high-concentration fluid. The high-concentration fluid was subjected to planetary degassing stirring (speed of 1500 r / min, time of 25 min) and centrifugal treatment (speed of 2000 r / min, time of 5 min) to finally prepare a uniformly dispersed high-concentration 3D printing ink;
[0042] (2) 3D printing ink is loaded into a syringe with a volume of 30 mL; the diameter of the printing needle is selected to be 400 μm; the printing path is set (i.e., modeling and slicing, which can be designed accordingly according to one's own needs), and the direct writing 3D printer prints according to the set printing path to obtain a three-dimensional structure formed by the accumulation of 3D printing ink (i.e., the three-dimensional structure is determined by the printing path). The printing process is: the needle moving speed is 10 mm / s, and the gas pressure is 45 psi;
[0043] (3) The printed three-dimensional structure is placed in a refrigerator and frozen for 12 hours; then, it is freeze-dried in a vacuum freeze dryer at -50°C for 60 hours; finally, the dried three-dimensional structure is placed in a crucible, placed in a tubular atmosphere furnace, and reduced at 700°C for 4 hours in a high-purity argon atmosphere to obtain a 3D printed silicene-based composite structure material.
[0044] The silicene nanosheets are prepared by a topological chemical method, and the steps are as follows:
[0045] (1) 1.2 g of CaSi2 was placed in a 2 mol / L NaOH solution for 10 min, then filtered and dried to obtain product A;
[0046] (2) 1.1 g SnCl2 was added to 60 ml methanol and stirred thoroughly until completely dissolved to obtain a mixed solution, 0.2 g product A was added to the mixed solution, and sodium dodecylbenzene sulfonate (SDBS) was weighed and added (the amount of SDBS added was 1% to 3% of the mass of SnCl2), and after stirring, it was placed in a 60°C constant temperature water bath to react for 24 hours; after the reaction, product B was obtained, and product B was washed three times by centrifugation with methanol and 5 wt% hydrogen chloride methanol solution, respectively, filtered and vacuum dried at 80°C for 24 hours; finally, supercritical drying was performed for 4 hours to obtain silicene nanosheets.
[0047] The graphene oxide is prepared by a modified Hummers method, and the steps are as follows:
[0048] Pour 2.5g sodium nitrate, 5g flake graphite powder and 115mL concentrated sulfuric acid into a beaker and force stir in an ice water bath for 45min; then add 15g KMnO4 and stir for 50min; raise the water bath temperature to 35℃ and react for 45min; then raise the temperature to 90℃ and react for 15min; after the reaction, add 25mL hydrogen peroxide and let stand for 24h; use deionized water for centrifugal washing until close to neutral; ultrasonically disperse for 30min and centrifuge for 15min to obtain a thick slurry at the bottom, freeze-dry the thick slurry at the bottom in a vacuum freeze dryer to obtain graphene oxide dry powder, and store it in a vacuum for later use.
[0049] Example 2
[0050] The difference between this embodiment and the above embodiment is that:
[0051] A method for preparing a 3D printed silicene-based composite structural material comprises the following steps:
[0052] (1) 100 mg of silicene nanosheets and 200 mg of graphene oxide were sequentially added to a cellulose nanofiber aqueous solution with a mass concentration of 0.5%, and ultrasonic dispersion (power of 200 W, dispersion time of 30 min) was performed each time to obtain a high-concentration fluid, and the high-concentration fluid was subjected to planetary degassing stirring (speed of 2000 r / min, time of 40 min), centrifugal treatment (speed of 2000 r / min, time of 10 min), and finally a uniformly dispersed high-concentration 3D printing ink was prepared;
[0053] (2) 3D printing ink was loaded into a syringe with a volume of 30 mL; the diameter of the printing needle was selected to be 450 μm; the printing path was set (the same as the printing path in Example 1), and the ink was deposited in three-dimensional space using a direct writing 3D printer to obtain a 3D printed three-dimensional structure. The printing process was: the needle moving speed was 8 mm / s, and the gas pressure was 50 psi;
[0054] (3) The printed three-dimensional structure is placed in a refrigerator and frozen for 12 hours; then, it is freeze-dried in a vacuum freeze dryer at -50°C for 72 hours; finally, the dried three-dimensional structure is placed in a crucible, placed in a tubular atmosphere furnace, and reduced at 700°C for 6 hours in a high-purity argon atmosphere to obtain a 3D printed silicene-based composite structure material.
[0055] Example 3
[0056] A method for preparing a 3D printed silicene-based composite structural material comprises the following steps:
[0057] (1) 120 mg of silicene nanosheets and 200 mg of graphene oxide were sequentially added to a cellulose nanofiber aqueous solution with a mass concentration of 1%, and ultrasonic dispersion was performed each time (power was 200 W, and dispersion time was 45 min) to obtain a high-concentration fluid. The high-concentration fluid was subjected to planetary degassing stirring (speed was 2000 r / min, time was 45 min), and centrifugal treatment (speed was 2500 r / min, time was 5 min), and finally a uniformly dispersed high-concentration 3D printing ink was prepared;
[0058] (2) 3D printing ink was loaded into a syringe with a volume of 30 mL; the diameter of the printing needle was selected to be 500 μm; the printing path was set (the same as the printing path in Example 1), and the ink was deposited in three-dimensional space using a direct writing 3D printer to obtain a 3D printed three-dimensional structure. The printing process was: the needle moving speed was 10 mm / s, and the gas pressure was 55 psi;
[0059] (3) The printed three-dimensional structure is placed in a refrigerator and frozen for 12 hours; then, it is freeze-dried in a vacuum freeze dryer at -55°C for 72 hours; finally, the dried printed structure is placed in a crucible, placed in a tubular atmosphere furnace, and reduced at 700°C for 6 hours in a high-purity argon atmosphere to obtain a 3D printed silicene-based composite structure material.
[0060] Example 4
[0061] A method for preparing a 3D printed silicene-based composite structural material comprises the following steps:
[0062] (1) 100 mg of silicene nanosheets and 150 mg of graphene oxide were sequentially added to a 1.5% mass concentration aqueous solution of cellulose nanofibers, and ultrasonic dispersion was performed each time (power was 200 W, and dispersion time was 30 min) to obtain a high-concentration fluid. The high-concentration fluid was subjected to planetary degassing stirring (speed was 1500 r / min, time was 60 min), and centrifugal treatment (speed was 2500 r / min, time was 10 min) to finally prepare a uniformly dispersed high-concentration 3D printing ink.
[0063] (2) The 3D printing ink was loaded into a syringe with a volume of 30 mL, and the printing needle diameter was selected to be 500 μm; the printing path was set (the same as the printing path in Example 1), and the ink was deposited in three-dimensional space using a direct writing 3D printer to obtain a 3D printed three-dimensional structure. The printing process was: the needle moving speed was 8 mm / s, and the gas pressure was 60 psi.
[0064] (3) The printed three-dimensional structure is placed in a refrigerator and frozen for 12 hours; then, it is freeze-dried in a vacuum freeze dryer at -60°C for 72 hours; finally, the dried three-dimensional structure is placed in a crucible, placed in a tubular atmosphere furnace, and reduced at 1000°C for 4 hours in a high-purity argon atmosphere to obtain a 3D printed silicene-based composite structure material.
[0065] In order to fully verify the technical effect of this method, the above examples are carried out, and the accompanying drawings are given for auxiliary explanation:
[0066] from Figure 1 It can be seen that the graphene oxide prepared by the Hummers method in Example 1 has only an obvious characteristic peak at 11.4°, proving that the graphite is completely oxidized; the silicene nanosheets prepared by the chemical topology method have four significant characteristic peaks at 17.25°, 28.45°, 47.25° and 56.1°, indicating that the prepared silicene nanosheets have a high degree of crystallinity. The silicene-based composite structural material prepared by 3D printing has a typical characteristic peak of graphite at around 26°, indicating that after high-temperature reduction, the graphene oxide is completely reduced to reduced graphene oxide.
[0067] Figure 2 A graph showing the relationship between the apparent viscosity of the 3D printing ink and the shear rate is shown. It can be seen from the figure that the static apparent viscosity of the 3D printing ink prepared in Examples 1 to 4 is greater than 105 Pa.s, which meets the requirements of the direct writing extrusion 3D printing technology involved in the present invention (the ink viscosity is generally required to be above 102 Pa.s). At the same time, it is found that the apparent viscosity of all inks gradually decreases with the increase of the shear rate, which is a typical feature of a "non-Newtonian fluid" and can ensure the smooth implementation of the direct writing extrusion 3D printing process.
[0068] Figure 3 Figure (a) is a top view of the 3D printed silicene-based composite structure. It can be seen that the upper and lower layers of the silicene-based composite structure constructed by 3D printing are interlaced in longitude and latitude, the holes between the printed lines are clear, and the structure is very regular; Figure (b) is a SEM image of the lines in the 3D printed silicene-based composite structure. It can be clearly observed from the figure that silicene nanosheets and reduced graphene oxide sheets are interlaced with each other, evenly dispersed, and connected by nanofibers. The three construct a rich hierarchical porous structure; Figure (c) is a SEM image of the lines with a further magnification of the scanning factor. Figure (c) further confirms the positional relationship between the silicene nanosheets and reduced graphene oxide in Figure (b). It can be seen from the figure that the silicene nanosheets are covered by a thin and flexible layer of reduced graphene oxide, and the two are coordinated with each other, which is beneficial to improving the hydrogen storage performance of the structural material.
[0069] Figure 4 The infrared spectrum of 3D printed silicene-based composite structural materials is shown. In the figure, 3430cm-1 belongs to the stretching vibration peak of -OH; after high-temperature reduction, the stretching vibration peak of -OH basically disappears; the peaks between 1600cm-1-1620cm-1 indicate that the material contains C=C functional groups, which is a typical feature of graphene oxide reduction; the obvious Si-O-Si peak appears at 1050cm-1-1200cm-1, indicating that the silicene nanosheets and graphene oxide have partial chemical bonding during the preparation of the ink, which is very beneficial for the establishment of the internal network of the material and the transmission of hydrogen between the two.
[0070] from Figure 5 It can be seen that the 3D printed silicene-based composite structural materials have good hydrogen adsorption and desorption cycle stability, and the surface hydrogenation of silicene nanosheets is a reversible process; and the hydrogen storage capacity of the structural material gradually increases with the increase of the proportion of silicene nanosheets in the material; the hydrogen storage performance of the 3D printed silicene-based composite structural material at room temperature can reach 2.5wt%, the hydrogen adsorption rate is high, and the hydrogen storage effect is good.
[0071] from Figure 6It can be seen that under room temperature conditions, the 3D printed silicene-based composite structural materials all show a faster hydrogen adsorption rate; comparison shows that the composite structural material corresponding to Example 4 has the largest hydrogen absorption rate.
[0072] The above specific implementation manner cannot be used as a limitation on the protection scope of the present invention. For those skilled in the art, any substitution, improvement or change made to the implementation manner of the present invention falls within the protection scope of the present invention.
[0073] The matters not described in detail in the present invention are all known technologies to those skilled in the art.
Claims
1. A method for preparing a 3D printed silicene-based composite structural material, characterized in that: The following steps are involved: (1) adding silicene nanosheets and graphene oxide to a cellulose nanofiber aqueous solution in sequence, and performing ultrasonic dispersion each time to obtain a high-concentration fluid; and subjecting the high-concentration fluid to planetary degassing stirring and centrifugal treatment to obtain a 3D printing ink; (2) using the 3D printing ink obtained in step (1) and printing a three-dimensional structure using a direct writing 3D printer; (3) The three-dimensional structure printed in step (2) is freeze-dried and high-temperature reduced to prepare a silicene-based composite structural material.
2. The method for preparing a 3D printed silicene-based composite structural material according to claim 1, characterized in that: The mass solubility of the cellulose nanofiber aqueous solution in step (1) is 0.5-1.5%, and the mass ratio of the silicene nanosheets, graphene oxide and cellulose nanofiber aqueous solution is: 1-2: 1-5: 100-130.
3. A method for preparing a 3D printed silicene-based composite structural material according to claim 1 or 2, characterized in that: The power of the ultrasonic dispersion in step (1) is 200W, the dispersion time is 30min, the rotation speed of the planetary deaeration stirring is 1500-2000r / min, the time is 15-30min, and the rotation speed of the centrifugal treatment is 1500-2000r / min, and the time is 3-8min.
4. The method for preparing a 3D printed silicene-based composite structural material according to claim 3, characterized in that: In step (2), the 3D printing ink obtained in step (1) is loaded into the syringe of a direct writing 3D printer, the diameter of the printing needle in the direct writing 3D printer is 300 to 500 μm, and the direct writing 3D printer deposits the 3D printing ink into a three-dimensional structure by printing in a three-dimensional space. The moving speed of the printing needle is 8 to 12 mm / s, and the gas pressure is 40 to 60 psi.
5. The method for preparing a 3D printed silene-based composite structural material according to claim 4, characterized in that: In step (3), the printed three-dimensional structure is placed in a refrigerator for 12 hours, freeze-dried at a temperature of -40 to -60°C for 48 to 72 hours, the dried three-dimensional structure is placed in a crucible, and the crucible is placed in a tubular atmosphere furnace, and reduced at a high temperature of 700 to 1000°C for 2 to 6 hours in a high-purity argon atmosphere to obtain a 3D printed silicene-based composite structure material.
6. The method for preparing a 3D printed silicene-based composite structural material according to claim 1, characterized in that: In step (1), the silicene nanosheet is prepared by a topological chemical method, comprising the following steps: (1) CaSi2 is placed in a NaOH solution, then filtered and dried to obtain product A; (2) SnCl2 is added to methanol and stirred until it is completely dissolved to obtain a mixed solution, product A and sodium dodecylbenzene sulfonate are added to the mixed solution in sequence and stirred, and then placed in a constant temperature water bath for reaction. After the reaction is completed, product B is obtained, and product B is washed by centrifugation with methanol and methanol solution of hydrogen chloride, respectively, filtered and vacuum dried; finally, silicene nanosheets are obtained by supercritical drying.
7. A method for preparing a 3D printed silicene-based composite structural material according to claim 6, characterized in that: The concentration of the NaOH solution is 2 mol / L, the CaSi2 is allowed to stand in the NaOH solution for 10 min, the temperature of the constant temperature water bath is set to 60°C, the reaction time is 24 h, the product B is centrifugally washed 3 times with methanol and 5 wt% hydrogen chloride methanol solution respectively, filtered and vacuum dried at 80°C for 24 h, and finally supercritically dried for 4 h.
8. A method for preparing a 3D printed silicene-based composite structural material according to claim 1 or 6, characterized in that: In step (1), the graphene oxide is prepared by a modified Hummers method, comprising the following steps: Pour sodium nitrate, flake graphite powder and concentrated sulfuric acid into a container, force stirring in an ice water bath, then add KMnO4 and stir, increase the water bath temperature twice in sequence to react respectively, after the reaction is completed, add hydrogen peroxide and let it stand, use deionized water to centrifuge and wash it to near neutrality, then perform ultrasonic and centrifugal treatment to obtain a thick slurry at the bottom, freeze-dry the thick slurry at the bottom in a vacuum freeze dryer to obtain graphene oxide dry powder, and store it in a vacuum for later use.
9. The method for preparing a 3D printed silicene-based composite structural material according to claim 8, characterized in that: The water bath temperature was first raised to 35° C. for reaction for 45 min, and then raised to 90° C. for reaction for 15 min. The ultrasonic dispersion was performed for 30 min, and the centrifugal treatment was performed for 15 min.
10. The use of the 3D printed silicene-based composite structural material according to any one of claims 1 to 9, characterized in that: The 3D printed silicene-based composite structural material is used in the preparation of hydrogen storage products, capacitors and batteries.
Citation Information
Patent Citations
Cobalt-sulfur hydrogen storage composite material containing porous polyaniline / reduced graphene oxide and preparation method thereof
CN113054181A
A platinum-loaded nitrogen / sulfur co-doped porous carbon nanofiber material and its preparation and application
CN113089136B
Silylene / graphene composite material, and preparation method and applications thereof
CN106532047A
3D-printed graphene oxide / cellulose composite material, and preparation method and application of same
CN107501612A
Hydrogen storage fiber paper loaded with silylene-doped polyaniline
CN114045707A
Cited By
Preparation method of silylene / graphene composite material
CN119503782A
A method for preparing a silicene / graphene composite
CN119503782B
Industrial acetylene impurity removal device and impurity removal method thereof
CN121944707A