Method for recovering selenium and precious metals from selenium slag

Through the combination of acid solution impregnation and activated carbon distillation, the problem of low recovery of selenium and precious metals in selenium slag is solved, efficient recycling and environmentally friendly recycling of selenium and precious metals is achieved, the process flow is simplified, and the use of oxidants and wastewater is avoided.

CN118908155AInactive Publication Date: 2024-11-08GANZHOU NONFERROUS METALLURGICAL RES INST

Patent Information

Application Number
CN202411404510.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art When recovering selenium and precious metals from selenium slag, the recovery rate is low and the use of oxidants is required, resulting in wastewater production and the process is complicated.

Method used

The selenium residue is impregnated with acid solution and distilled with activated carbon. The selenium and precious metals are collected by smelting through fire, avoiding the use of oxidants and achieving efficient recycling.

Benefits of technology

It improves the recycling rate of selenium and precious metals, simplifies the process flow, avoids the generation of wastewater, and has simple operation and obvious economic benefits.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for recovering selenium and precious metals from selenium slag, which comprises the following steps: mixing the selenium slag with an acid solution, and sequentially carrying out dipping treatment and solid-liquid separation to obtain leaching residue; the leaching residues comprise selenium and precious metal; mixing the leaching residues with activated carbon, and distilling to obtain selenium and distillation residues; the distillation residues are subjected to pyrogenic process smelting collecting, and precious metal is obtained; the precious metal comprises gold and / or silver. According to the method, selenium and precious metal in the selenium slag are recovered by combining a wet process and a pyrogenic process, the operation is simple, and the flow is short; the recovery rate of selenium and precious metals is high, the use of an oxidant is avoided, no wastewater is generated, and the economic benefit is obvious.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid waste resource utilization, and specifically relates to a method for recovering selenium and precious metals from selenium slag. Background Art

[0002] Selenium slag is the waste collected from smoke dust during the roasting process of copper sulfide concentrate or iron sulfide concentrate, which contains selenium, copper, iron, tellurium, gold, silver and other elements. The mass fraction of selenium in selenium slag is generally 10-20%. In order to recover selenium and precious metals such as gold and silver in selenium slag, the existing technology uses acid to dissolve selenium slag, and adds an oxidant (such as sodium chlorate) to dissolve the iron and selenium in the selenium slag at the same time, and then uses a reducing agent (such as iron powder, thiourea, etc.) to reduce it to form crude selenium, and then dissolves and reduces it to finally prepare refined selenium. The recovery rate of selenium obtained in this way is low (about 85%), and a large amount of oxidant is consumed, and a large amount of wastewater is generated. Summary of the invention

[0003] The object of the present invention is to provide a method for recovering selenium and precious metals from selenium slag. The method provided by the present invention has a high recovery rate of selenium and precious metals, does not require the use of oxidants, and does not generate waste water.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The present invention provides a method for recovering selenium and precious metals from selenium slag, comprising the following steps: The selenium residue is mixed with an acid solution, and then subjected to an immersion treatment and solid-liquid separation in sequence to obtain an immersion residue; the immersion residue comprises selenium and a precious metal; The leaching residue is mixed with activated carbon and distilled to obtain selenium vapor and distillation residue respectively, and the selenium vapor is condensed to obtain selenium; the distillation temperature is 400-600°C; The distillation slag is subjected to fire smelting and collection to obtain precious metals; the precious metals include gold and / or silver.

[0005] Preferably, the acid solution is hydrochloric acid or sulfuric acid; the concentration of the acid solution is 4-10 mol / L.

[0006] Preferably, the material-liquid ratio of the selenium residue to the acid solution is 1 g: 3-4 mL.

[0007] Preferably, the immersion treatment is carried out at a temperature of 60-80° C. and for a time of 2-4 hours.

[0008] Preferably, the activated carbon is coconut shell activated carbon.

[0009] Preferably, the coconut shell activated carbon has an iodine value of 800-1100 mg / g and a particle size of 0.5-1 mm.

[0010] Preferably, the distillation is vacuum distillation; the insulation time of the vacuum distillation is 2-3 hours, the pressure is 1-100 Pa, and the rate of heating to the temperature of the vacuum distillation is 8-10°C / min.

[0011] Preferably, the condensation temperature is -30~300°C.

[0012] Preferably, the temperature of the pyrometallurgical smelting capture is 1400-1650° C., and the holding time is 0.1-0.3 h.

[0013] Preferably, the selenium slag is roasted before being mixed with the acid solution; the roasting temperature is 200-300° C., and the heat preservation time is 2-3 hours.

[0014] The present invention provides a method for recovering selenium and precious metals from selenium slag, comprising the following steps: mixing the selenium slag with an acid solution, and sequentially performing an impregnation treatment and solid-liquid separation to obtain an impregnation residue; the impregnation residue comprises selenium and precious metals; mixing the impregnation residue with activated carbon, and performing distillation to obtain selenium and distillation residue; performing fire smelting and capture on the distillation residue to obtain precious metals; the precious metals comprise gold and / or silver. The present invention uses an acid solution to impregnate the selenium slag, which can dissolve metals including iron in the selenium slag and reduce the impurity content in the final product. At the same time, activated carbon, as a reducing agent, can reduce the oxidized selenium in the selenium slag to a single selenium substance, effectively improving the reduction efficiency of selenium; performing distillation under the condition of the presence of activated carbon can improve the selenium evaporation rate, and can also enrich the precious metals in the distillation residue, which is convenient for subsequent purification operations. The present invention captures the precious metals in the obtained distillation residue on the basis of distillation, which can further achieve the enrichment of precious metals and improve the capture rate of gold and silver. The invention adopts a combination of a wet process and a pyroprocess to recover selenium and precious metals in selenium slag, which has simple operation and a short process; the recovery rate of selenium and precious metals is high, and the use of oxidants is avoided, no waste water is generated, and the economic benefits are obvious.

[0015] Furthermore, the present invention adopts coconut shell activated carbon with high iodine value and loose porosity as a reducing agent in the distillation process, which has higher reducing efficiency and can quickly reduce selenate in selenium residue to selenium element, thereby improving the recovery rate of selenium and precious metals. DETAILED DESCRIPTION

[0016] The present invention provides a method for recovering selenium and precious metals from selenium slag, comprising the following steps: The selenium residue is mixed with an acid solution, and then subjected to an immersion treatment and solid-liquid separation in sequence to obtain an immersion residue; the immersion residue comprises selenium and a precious metal; The leaching residue is mixed with activated carbon and distilled to obtain selenium vapor and distillation residue respectively, and the selenium vapor is condensed to obtain selenium; the distillation temperature is 400-600°C; The distillation slag is subjected to fire smelting and collection to obtain precious metals; the precious metals include gold and / or silver.

[0017] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or are prepared by methods well known to those skilled in the art.

[0018] The selenium slag of the present invention is preferably waste generated after roasting of copper sulfide concentrate or iron sulfide concentrate. In the present invention, the selenium slag is preferably roasted before mixing with the acid solution to obtain pretreated selenium slag. In the present invention, the selenium slag is preferably mixed with activated carbon and roasted to obtain pretreated selenium slag. In the present invention, the activated carbon is preferably coconut shell activated carbon; the iodine value of the coconut shell activated carbon is 800~1100mg / g, more preferably 900~1000mg / g; the particle size is preferably 0.5~1mm, more preferably 0.8~1mm; the mass ratio of the selenium slag to the activated carbon is preferably 10~50:1~2, specifically 20:1, 25:1, 30:1, 35:1, 40:1, 45:1 or 50:1. In the present invention, the roasting temperature is preferably 200~300℃, more preferably 200~250℃; the insulation time is preferably 2~3h, specifically 2h, 2.5h or 3h. In the present invention, activated carbon is used as a reducing agent to achieve the transformation of selenium in selenium slag through a carbon reduction roasting process, thereby improving the yield of selenium in a subsequent distillation process.

[0019] After obtaining the pretreated selenium slag, the present invention mixes the pretreated selenium slag with an acid solution, and sequentially performs an immersion treatment and solid-liquid separation to obtain an immersion residue. In the present invention, the acid solution is preferably hydrochloric acid or sulfuric acid; the concentration of the acid solution is preferably 4-10 mol / L, specifically 4 mol / L, 6 mol / L or 10 mol / L; the material-liquid ratio of the selenium slag to the acid solution is preferably 1 g: 3-4 mL, more preferably 1 g: 3-3.5 mL. In the present invention, the temperature of the immersion treatment is preferably 60-80 ° C, specifically 60 ° C, 70 ° C or 80 ° C; the time is preferably 2-4 h, specifically 2 h, 3 h or 4 h. After the immersion treatment is completed, the present invention preferably performs solid-liquid separation on the obtained feed liquid, collects solid materials and liquid materials respectively, and the liquid material is the leachate, specifically ferric sulfate solution or ferric chloride solution; the solid material is sequentially washed and dried to obtain an immersion residue. In the present invention, the solid-liquid separation is preferably filtration; the washing is preferably water washing. The function of the water washing in the present invention is to remove the acid solution remaining on the surface of the leached residue. In the present invention, the selenium residue is impregnated with hydrochloric acid and / or sulfuric acid, which can dissolve the metals including iron in the selenium residue and make them enter the solution in the form of ions or compounds, which is convenient for subsequent separation and purification; in particular, it can promote the pre-removal of iron in the selenium residue, and can increase the pre-removal efficiency of iron to more than 90%. The iron sulfate solution or iron chloride solution produced thereby can be sold as an environmentally friendly reagent; in addition, the impregnation treatment with an acid solution can also effectively reduce the content of impurities in the final product.

[0020] After obtaining the leaching residue, the present invention mixes the leaching residue with activated carbon, performs distillation, and obtains selenium vapor and distillation residue respectively, and the selenium vapor is condensed to obtain selenium. The present invention preferably covers the surface of the leaching residue with activated carbon. In the present invention, the activated carbon is preferably coconut shell activated carbon; the iodine value of the coconut shell activated carbon is 800~1100mg / g, more preferably 900~1000mg / g; the particle size is preferably 0.5~1mm, more preferably 0.8~1mm. In the present invention, the mass ratio of the leaching residue to the activated carbon is preferably 20~50:1, specifically 20:1, 30:1, 40:1 or 50:1; the coverage thickness of the activated carbon on the surface of the leaching residue is preferably 0.5~1mm, more preferably 0.8~1mm. The distillation of the present invention is preferably vacuum distillation; the temperature of the vacuum distillation is 400-600°C, preferably 450-500°C; the holding time is preferably 1-4h, more preferably 2h; the rate of heating to the temperature of the vacuum distillation is preferably 8-10°C / min, specifically 8°C / min, 9°C / min or 10°C / min; the pressure is preferably 1-100Pa, more preferably 10-70Pa. In one embodiment of the present invention, the pressure of the vacuum distillation is 14Pa; in another embodiment of the present invention, the pressure of the vacuum distillation is 40Pa; in another embodiment of the present invention, the pressure of the vacuum distillation is 70Pa. The temperature of the condensation of the present invention is preferably -30-300°C, more preferably 30-100°C. In the present invention, activated carbon is used as a reducing agent, and distillation is carried out under the condition of the presence of activated carbon. On the one hand, the selenium evaporation rate can be increased, and on the other hand, the precious metals can be enriched in the distillation residue, which is convenient for subsequent purification operations.

[0021] After obtaining the distillation slag, the present invention performs fire smelting and capture on the distillation slag to obtain precious metals; the precious metals include gold and / or silver. In the present invention, the temperature of the fire smelting and capture is preferably 1400~1650℃, more preferably 1550℃; the insulation time is preferably 0.1~0.3h, more preferably 0.2h. In an embodiment of the present invention, the distillation slag is specifically mixed with iron powder and then eutectic, and fire smelting and capture are performed to obtain a mixture containing precious metals and iron, wherein the mass ratio of the distillation slag to the iron powder is 1~10:1~2, specifically 2:1, 4:1, 6:1, 8:1 or 10:1. The present invention captures the precious metals in the distillation slag by fire smelting, which can further achieve the enrichment of precious metals and improve the capture rate of gold and silver.

[0022] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The selenium slag used in the embodiment is the waste generated after the iron sulfide concentrate is roasted; The activated carbon used in the embodiment is coconut shell activated carbon, with an iodine value of 800-1100 mg / g and a particle size of 0.5-1 mm.

[0024] Example 1 Selenium slag and activated carbon are mixed in a mass ratio of 30:1, and calcined at 250°C for 2h to obtain pretreated selenium slag. Take 100g of pretreated selenium slag, add 300mL of sulfuric acid with a concentration of 4mol / L to the pretreated selenium slag, and immerse for 2h at 60°C; after the immersion, filter the obtained liquid, collect the solid material and liquid material respectively, and the liquid material (i.e., the leachate) is a ferric sulfate solution (which can be sold as an environmentally friendly reagent). The solid material leaching residue is washed and dried in turn to obtain the leaching residue.

[0025] The leaching residue is placed in a vacuum furnace connected to a condensation tank, a layer of activated carbon with a thickness of 1 mm is covered on the surface of the leaching residue (the mass ratio of the leaching residue to the activated carbon is 50:1), the vacuum furnace is evacuated to 14 Pa, the temperature of the vacuum furnace is uniformly increased from room temperature to 450° C. at a rate of 10° C. / min, and the temperature is kept at 450° C. for 2 hours. During the distillation process, selenium volatilizes into the condensation tank, and the obtained selenium vapor is condensed at 60° C. After the distillation, selenium and distillation residue are obtained, wherein the recovery rate of selenium is 92.3%, and the purity of selenium is ≥98%.

[0026] The distillation slag was mixed with iron powder in a mass ratio of 6:1, and the resulting mixture was smelted at 1550° C. for 0.2 h to achieve fire smelting capture, and a gold-silver-iron mixture was obtained after the completion, wherein the capture rates of gold and silver were 95.2% in total.

[0027] Example 2 Selenium slag and activated carbon are mixed in a mass ratio of 35:1, and calcined at 250°C for 2h to obtain pretreated selenium slag. Take 100g of pretreated selenium slag, add 300mL of 10mol / L sulfuric acid to the pretreated selenium slag, and immerse for 2h at 60°C; after the immersion, filter the obtained liquid, collect the solid material and liquid material respectively, and the liquid material (i.e., the leachate) is a ferric sulfate solution (which can be sold as an environmentally friendly reagent). The solid material is washed and dried in turn to obtain the leached residue.

[0028] The leaching residue is placed in a vacuum furnace connected to a condensation tank, a layer of activated carbon with a thickness of 1 mm is covered on the surface of the leaching residue (the mass ratio of the leaching residue to the activated carbon is 40:1), the vacuum furnace is evacuated to 14 Pa, the temperature of the vacuum furnace is uniformly increased from room temperature to 450° C. at a rate of 10° C. / min, and the temperature is kept at 450° C. for 2 hours. During the distillation process, selenium volatilizes into the condensation tank, and the obtained selenium vapor is condensed at 60° C. After the distillation is completed, selenium and distillation residue are obtained, wherein the recovery rate of selenium is 97.3%, and the purity of selenium is ≥98%.

[0029] The distillation slag was mixed with iron powder in a mass ratio of 6:1, and the resulting mixture was smelted at 1550° C. for 0.2 h to achieve fire smelting capture, and a gold-silver-iron mixture was obtained after the completion, wherein the capture rates of gold and silver were 96.2% in total.

[0030] Example 3 Selenium slag and activated carbon were mixed in a mass ratio of 50:1, and calcined at 250°C for 2h to obtain pretreated selenium slag. 300g of pretreated selenium slag was taken, 1000mL of 5mol / L sulfuric acid was added to the pretreated selenium slag, and the pretreated selenium slag was immersed at 70°C for 3h; after the immersion, the obtained liquid was filtered, and the solid material and liquid material were collected respectively, and the liquid material (i.e., the leachate) was an iron sulfate solution (which can be sold as an environmentally friendly reagent). The solid material was washed and dried in turn to obtain the leached residue.

[0031] The leaching residue is placed in a vacuum furnace connected to a condensation tank, a layer of activated carbon with a thickness of 2 mm is covered on the surface of the leaching residue (the mass ratio of the leaching residue to the activated carbon is 20:1), the vacuum furnace is evacuated to 40 Pa, the temperature of the vacuum furnace is uniformly increased from room temperature to 500° C. at a rate of 10° C. / min, and the temperature is kept at 500° C. for 2 hours. During the distillation process, selenium volatilizes into the condensation tank, and the obtained selenium vapor is condensed at 60° C. After the distillation, selenium and distillation residue are obtained, wherein the recovery rate of selenium is 94.3%, and the purity of selenium is ≥98%.

[0032] The distillation slag was mixed with iron powder in a mass ratio of 6:1, and the resulting mixture was smelted at 1550° C. for 0.2 h to achieve fire smelting capture, and a gold-silver-iron mixture was obtained after the completion, wherein the capture rates of gold and silver were 96.2% in total.

[0033] Example 4 Selenium slag and activated carbon are mixed in a mass ratio of 50:1, and calcined at 250°C for 2h to obtain pretreated selenium slag. Take 100g of pretreated selenium slag, add 300mL of 10mol / L sulfuric acid to the pretreated selenium slag, and immerse for 4h at 80°C; after the immersion, filter the obtained liquid, collect the solid material and liquid material respectively, and the liquid material (i.e., the leachate) is a ferric sulfate solution (which can be sold as an environmentally friendly reagent). The solid material is washed and dried in turn to obtain the leached residue.

[0034] The leaching residue is placed in a vacuum furnace connected to a condensation tank, a layer of activated carbon with a thickness of 3 mm is covered on the surface of the leaching residue (the mass ratio of the leaching residue to the activated carbon is 20:1), the vacuum furnace is evacuated to 70 Pa, the temperature of the vacuum furnace is uniformly increased from room temperature to 490° C. at a rate of 10° C. / min, and the temperature is kept at 490° C. for 2 hours. During the distillation process, selenium volatilizes into the condensation tank, and the obtained selenium vapor is condensed at 60° C. After the distillation is completed, selenium and distillation residue are obtained, wherein the recovery rate of selenium is 91.5%, and the purity of selenium is ≥98%.

[0035] The distillation slag was mixed with iron powder in a mass ratio of 6:1, and the obtained mixture was eutectic at 1550° C. for 0.2 h, and smelted and captured by fire method to obtain a gold-silver-iron mixture, wherein the capture rates of gold and silver were 90.2% in total.

[0036] Example 5 Selenium slag and activated carbon are mixed in a mass ratio of 45:1, and calcined at 250°C for 2 hours to obtain pretreated selenium slag. Take 100g of pretreated selenium slag, add 300mL of 10mol / L sulfuric acid to the pretreated selenium slag, and immerse for 4 hours at 80°C; after the immersion, filter the obtained liquid, collect the solid material and liquid material respectively, and the liquid material (i.e., the leachate) is a ferric sulfate solution (which can be sold as an environmentally friendly reagent). The solid material is washed and dried in turn to obtain the leached residue.

[0037] The leaching residue is placed in a vacuum furnace connected to a condensation tank, a layer of activated carbon with a thickness of 3 mm is covered on the surface of the leaching residue (the mass ratio of the leaching residue to the activated carbon is 20:1), the vacuum furnace is evacuated to 70 Pa, the temperature of the vacuum furnace is uniformly increased from room temperature to 550° C. at a rate of 10° C. / min, and the temperature is kept at 550° C. for 2 hours. During the distillation process, selenium volatilizes into the condensation tank, and the obtained selenium vapor is condensed at 60° C. After the distillation, selenium and distillation residue are obtained, wherein the recovery rate of selenium is 95.5%, and the purity of selenium is ≥98%.

[0038] The distillation slag was mixed with iron powder in a mass ratio of 6:1, and the resulting mixture was smelted at 1550° C. for 0.2 h, and smelted and captured by fire method to obtain a gold-silver-iron mixture, wherein the capture rates of gold and silver were 93.7% in total.

[0039] Therefore, the method provided by the present invention is simple to operate, does not require the use of an oxidant, does not generate wastewater, and has high recovery rates of selenium and precious metals, wherein the recovery rate of selenium is 91.5-97.3%, and the recovery rate of precious metals is 90.2-96.2%.

[0040] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for recovering selenium and precious metals from selenium slag, characterized in that: The following steps are involved: The selenium residue is mixed with an acid solution, and then subjected to an immersion treatment and solid-liquid separation in sequence to obtain an immersion residue; the immersion residue comprises selenium and a precious metal; The leaching residue is mixed with activated carbon and distilled to obtain selenium vapor and distillation residue respectively, and the selenium vapor is condensed to obtain selenium; the distillation temperature is 400-600°C; The distillation slag is subjected to fire smelting and collection to obtain precious metals; the precious metals include gold and / or silver.

2. The method according to claim 1, characterized in that The acid solution is hydrochloric acid or sulfuric acid; the concentration of the acid solution is 4-10 mol / L.

3. The method according to claim 1 or 2, characterized in that: The material-liquid ratio of the selenium residue to the acid solution is 1 g: 3-4 mL.

4. The method according to claim 1, characterized in that: The immersion treatment is carried out at a temperature of 60-80° C. and for a time of 2-4 hours.

5. The method according to claim 1, characterized in that The activated carbon is coconut shell activated carbon.

6. The method according to claim 5, characterized in that The iodine value of the coconut shell activated carbon is 800-1100 mg / g, and the particle size is 0.5-1 mm.

7. The method according to claim 1, characterized in that The distillation is vacuum distillation; the temperature of the vacuum distillation is 400-600°C, the insulation time is 2-3h, the pressure is 1-100Pa, and the rate of heating to the vacuum distillation temperature is 8-10°C / min.

8. The method according to claim 1 or 7, characterized in that: The condensation temperature is -30~300℃.

9. The method according to claim 1, characterized in that: The temperature of the fire smelting capture is 1400-1650°C, and the insulation time is 0.1-0.3h.

10. The method according to claim 1, characterized in that The selenium slag is roasted before being mixed with the acid solution; the roasting temperature is 200-300° C., and the heat preservation time is 2-3 hours.

Citation Information

Patent Citations

  • Method for recovering rare noble metal from waste water slag of process of producing silver and selenium

    CN102978400A

  • Method for removing lead, antimony, bismuth, selenium, tellurium and arsenic from copper anode slime by vacuum reduction

    CN107217145A

  • Method for enriching low-grade precious metal through fire-wet method

    CN107460338A

  • Method for recovering selenium, tellurium, copper and precious metal from copper anode slime

    CN109371228A

  • High selenium and high silver flue dust treatment process

    CN112831665A

Cited By

  • Smelting equipment for extracting valuable metals in 3N selenium slag

    CN224480018U