Preparation method of copper-doped porous nano-silicon negative electrode material
By using copper-doped nanoporous silicon materials in lithium-ion batteries, combined with ion exchange and molten salt-assisted magnesium thermal reaction technology, the problem of nano-silicon material collapse after charging and discharge is solved, and better cycle stability is achieved and Electrochemical performance improves the overall performance of lithium batteries.
Patent Information
- Application Number
- CN202410971964.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The structural collapse effect of nano-silicon materials in existing lithium-ion batteries after multiple charges and discharges leads to poor circulation performance, making it difficult to effectively alleviate the volume expansion effect, affecting the long cycle stability and rateability of the battery.
Inexpensive montmorillonite is used as the silicon source, combined with ion exchange technology and molten salt-assisted magnesium thermal reaction method, to prepare copper-doped nanoporous silicon material, through copper ions embedded in the internal structure of montmorillonite, lithium ions react with copper silicon alloy phase, This slows down volume expansion and stabilizes the structure by heat treatment, improving conductivity and electrochemical properties.
Effectively inhibit nanostructure collapse, enhance crystal structure stability, improve lithium storage, rate performance and circulation performance of lithium batteries, and extend battery life.
Smart Images

Figure CN118908220A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery negative electrode materials, and in particular relates to a method for preparing a copper-doped porous nano-silicon negative electrode material. Background Art
[0002] Lithium batteries have the characteristics of high energy density, long life, high safety, low self-discharge rate and no memory effect. They are one of the most commonly used energy storage devices. Silicon materials have a large lithium storage capacity, so silicon negative electrodes can greatly improve the energy density of lithium batteries, but the pulverization effect caused by the large volume expansion rate during charging brings difficulties to practical applications. Nano-sizing is an effective means to overcome the pulverization of silicon negative electrodes, and its shorter lithium ion diffusion distance is conducive to improving the lithium storage capacity of silicon negative electrodes at high current density, but the structural collapse effect of nano-silicon materials after multiple charge and discharge processes has an adverse effect on their long-cycle stability.
[0003] Montmorillonite is a two-dimensional layered mineral of hydrous aluminum silicate, which has the characteristics of abundant resources, low price, large specific surface area, and exchangeable interlayer cations. Currently, magnesium thermal reduction using montmorillonite as raw material has become a cheap and efficient means of preparing nano-silicon materials. For example, patent CN110034296A discloses a method for preparing convex mirror-shaped silicon nanosheet materials by using intercalation separation of montmorillonite and combining magnesium thermal reduction technology. This method destroys the interlayer bonding force of montmorillonite, separates the silicon layer and the aluminum layer, increases the contact area between silicon oxide and magnesium powder, and ensures that a very thin silicon nanosheet is obtained after magnesium thermal reduction. It has excellent electrochemical performance in the field of lithium-ion battery negative electrode materials; patent CN117303370A discloses a method for preparing silicon nanosheet negative electrode materials by molten salt-assisted magnesium thermal reduction of montmorillonite. This method can realize the formation of nanosheet structure of montmorillonite, which is conducive to the silicon particles to maintain a complete structure during the charging and discharging process, slow down the volume expansion, and improve the cycle life and rate performance of lithium-ion batteries. At the same time, the preparation method is adapted to the needs of different scale production and has high scalability. Even though montmorillonite magnesium thermal reduction silicon has nanoporous characteristics and can effectively alleviate the volume expansion effect of silicon charging and discharging process, the nano silicon material prepared by the above method still has the disadvantage of poor cycle performance due to the collapse of the porous structure after multiple charging and discharging processes. Summary of the invention
[0004] In view of the shortcomings of the above-mentioned prior art, the present invention proposes a method for preparing a copper-doped porous nano-silicon negative electrode material. Using cheap montmorillonite as a silicon source, combined with ion exchange technology and molten salt-assisted magnesium thermal reaction method, a copper-doped nano-porous silicon material with excellent cycle performance and good structural stability is prepared in one step.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a copper-doped porous nano-silicon negative electrode material, comprising the following steps:
[0006] (1) mixing a copper salt solution and montmorillonite and allowing the mixture to stand, then filtering, collecting and vacuum drying the mixture to obtain copper ion-doped montmorillonite;
[0007] (2) mixing copper ion-doped montmorillonite, magnesium powder and metal chloride evenly under anhydrous and oxygen-free conditions to obtain a molten salt-assisted magnesium thermal reduction raw material;
[0008] (3) subjecting the raw material to magnesium thermal reduction reaction under anhydrous and oxygen-free atmosphere with the assistance of molten salt to obtain a mixture containing copper-doped nano-silicon material;
[0009] (4) washing the copper-doped nano-silicon material mixture with water and an acid solution in sequence and filtering the mixture, and vacuum drying the filtered product to obtain a copper-doped porous nano-silicon material preform;
[0010] (5) The copper-doped porous nano-silicon material preform is heat-treated in a protective gas to obtain a copper-doped porous nano-silicon negative electrode material.
[0011] As a preferred embodiment of the present invention, the copper salt is at least one of copper chloride, copper sulfate, and copper nitrate; the metal chloride is at least one of sodium chloride, potassium chloride, magnesium chloride, and calcium chloride.
[0012] As a preferred embodiment of the present invention, the mass volume ratio of the montmorillonite to the copper salt solution is (0.1-1):(1-10); the concentration of the copper salt solution is 0.1-10 mol / L.
[0013] As a preferred embodiment of the present invention, the mass ratio of the copper ion-doped montmorillonite, magnesium powder and metal chloride is 1:(0.1-5):(1-10).
[0014] As a preferred embodiment of the present invention, the temperature of the magnesium thermal reduction reaction is 400-1000° C. and the time is 1-36 hours.
[0015] As a preferred embodiment of the present invention, in the step (4), the acid solution cleaning includes first cleaning with acid A and then cleaning with acid B; acid A is at least one of hydrochloric acid, sulfuric acid, and nitric acid, and acid B is at least one of hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid.
[0016] As a preferred embodiment of the present invention, the concentration of the A acid is 0.01-5 mol / L, and the cleaning time is 1 min-10 h; the mass percentage concentration of the B acid is 0.01%-10%, and the cleaning time is 1 min-10 h.
[0017] As a preferred embodiment of the present invention, the temperature of the vacuum drying treatment is 40 to 80° C., and the time is 1 min to 24 h.
[0018] As a preferred embodiment of the present invention, the heat treatment temperature is 300-1000° C. and the time is 1 min-24 h.
[0019] As a preferred embodiment of the present invention, the anhydrous and oxygen-free gas atmosphere is one or more of nitrogen, argon, hydrogen and helium.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention uses cheap montmorillonite as a raw material, utilizes the property that montmorillonite interlayers can be used for ion exchange, embeds copper ions into the internal structure of montmorillonite by ion exchange, and obtains a copper-silicon alloy phase by molten salt-assisted magnesium thermal reduction reaction. Lithium ions can enter the montmorillonite interlayers to react with the copper-silicon alloy phase, thereby slowing down the volume expansion from the inside, and the process requires fewer control factors. The present invention can not only effectively inhibit the nanostructure collapse effect after multiple charge and discharge processes of the nanostructure, but also enhance the crystal structure stability of montmorillonite to a certain extent. The metal copper precipitated after the copper-silicon alloy reacts with lithium ions can also improve the conductivity of montmorillonite, promote the migration of electrons, and improve the electrochemical performance. Therefore, the present invention can greatly improve the lithium storage performance, rate performance and cycle performance of the lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the SEM image of the copper-doped porous nano-silicon negative electrode material prepared in Example 1.
[0023] Figure 2 This is the elemental energy spectrum of the copper-doped porous nano-silicon negative electrode material prepared in Example 1.
[0024] Figure 3 This is the XRD pattern of the copper-doped porous nano-silicon negative electrode material prepared in Example 1.
[0025] Figure 4 This is a diagram of the lithium storage cycle performance of the copper-doped porous nano-silicon negative electrode material prepared in Example 1.
[0026] Figure 5 The material morphology and structure SEM images of the undoped copper porous nano-silicon negative electrode material electrode film prepared in Comparative Example 1 before and after 2000 cycles; (a) is the material morphology and structure SEM image of the undoped copper porous nano-silicon negative electrode material electrode film prepared in Comparative Example 1 before 2000 cycles; (b) is the material morphology and structure SEM image of the undoped copper porous nano-silicon negative electrode material electrode film prepared in Comparative Example 1 after 2000 cycles.
[0027] Figure 6 The SEM comparison diagram of the material morphology and structure of the copper-doped porous nano-silicon negative electrode material electrode membrane prepared in Example 1 before and after 2000 cycles; (a) is the SEM comparison diagram of the material morphology and structure of the copper-doped porous nano-silicon negative electrode material electrode membrane prepared in Example 1 before 2000 cycles; (b) is the SEM comparison diagram of the material morphology and structure of the copper-doped porous nano-silicon negative electrode material electrode membrane prepared in Example 1 after 2000 cycles.
[0028] Figure 7 This is the SEM image of the copper-doped porous nano-silicon negative electrode material prepared in Example 2.
[0029] Figure 8 This is a diagram of the lithium storage cycle performance of the copper-doped porous nano-silicon negative electrode material prepared in Example 2. DETAILED DESCRIPTION
[0030] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0031] Example 1
[0032] A method for preparing a copper-doped porous nano-silicon negative electrode material comprises the following steps:
[0033] (1) preparing a cupric chloride solution, fully stirring the cupric chloride solution and montmorillonite, and then standing for a certain period of time to allow metal ions between montmorillonite layers to exchange ions with copper ions in the cupric chloride solution. After the ion exchange is completed, filtering and collecting, and vacuum drying are performed to obtain copper ion-doped montmorillonite.
[0034] (2) Copper ion-doped montmorillonite, magnesium powder and anhydrous sodium chloride were mixed in a glove box at a weight ratio of 10:8:40 and ground in a mortar to obtain a molten salt-assisted magnesium thermal reduction raw material.
[0035] (3) The molten salt-assisted magnesium thermal reduction raw material is placed in a stainless steel crucible, transferred to a tubular furnace filled with argon gas, and heated to 650° C. to carry out a molten salt-assisted magnesium thermal reduction reaction of montmorillonite and magnesium powder. The reaction time is 6 hours to obtain a mixture containing copper-doped nano-silicon material.
[0036] (4) Grinding the mixture of copper-doped nano-silicon materials, adding deionized water to the ground powder and slowly stirring for 2 hours, filtering to obtain a solid powder product I; adding the solid powder product I to 0.5 mol / L hydrochloric acid and stirring at room temperature for 4 hours, filtering to obtain a solid powder product II; dispersing the solid powder product II in a 0.5% HF solution and stirring for 4 hours to extract, filtering and rinsing with deionized water for multiple times to obtain a solid powder III; placing the solid powder III in a vacuum drying oven at 60° C. for vacuum drying for 10 hours to obtain a copper-doped porous nano-silicon material preform.
[0037] (5) The copper-doped porous nano-silicon material preform is annealed and heat-treated in an argon atmosphere at a temperature of 400° C. for a heat treatment time of 2 h to obtain a copper-doped porous nano-silicon negative electrode material.
[0038] An application of a copper-doped porous nano-silicon negative electrode material as a battery material, specifically:
[0039] according to Figure 1 It can be seen that the copper-doped porous nano-silicon negative electrode material prepared in this embodiment has a porous structure. Figure 2 It can be seen that the copper-doped porous nano-silicon negative electrode material only contains copper, silicon and oxygen elements. From the XRD diagram ( Figure 3 ) It can be seen that the copper-doped porous nano-silicon negative electrode material has a single silicon crystal phase. The porous nano-silicon negative electrode material prepared in this embodiment is used as the positive electrode, the metal lithium sheet is used as the negative electrode, the Celgard membrane is used as the separator, the electrolyte is composed of LiPF6 in ethylene carbonate (EC) / diethyl carbonate (DEC) (volume ratio of 3:7) with 10wt% fluoroethylene carbonate (FEC), the binder is composed of polyacrylic acid (PAA) and sodium carboxymethyl cellulose (CMC, 6wt%) (PAA / CMC volume ratio of 1:1), the working electrode is prepared by silicon nanosheets, conductive carbon black Super-P, and binder in a weight ratio of 7:1.5:1.5, the battery is assembled in a glove box filled with argon, and constant current charge and discharge tests are carried out. Figure 4 It can be seen that the reversible capacity of the copper-doped porous nano-silicon negative electrode material is 1400 mAh / g after 2000 cycles at a current density of 200 mA / g.
[0040] according to Figure 6 It can be seen that only some tiny cracks are formed on the electrode surface of the copper-doped porous nano-silicon negative electrode material electrode film prepared in this embodiment before and after cycling, indicating that the cross-sectional expansion of the silicon electrode is significantly improved under the synergistic effect of nano-porosity and copper doping, and the electrochemical performance is also improved.
[0041] Example 2
[0042] A method for preparing a copper-doped porous nano-silicon negative electrode material comprises the following steps:
[0043] (1) preparing a copper sulfate solution, fully stirring the copper sulfate solution and montmorillonite, and then standing for a certain period of time to allow metal ions between montmorillonite layers to exchange ions with copper ions in the copper sulfate solution. After the ion exchange is completed, filtering and collecting, and vacuum drying are performed to obtain copper ion-doped montmorillonite.
[0044] (2) Copper ion-doped montmorillonite, magnesium powder, anhydrous lithium chloride and anhydrous magnesium chloride were mixed in a glove box at a weight ratio of 10:8:30:10 and ground in a mortar to obtain a molten salt-assisted magnesium thermal reduction raw material.
[0045] (3) The molten salt-assisted magnesium thermal reduction raw material is placed in a stainless steel crucible, transferred to a tubular furnace filled with argon gas, and heated to 800° C. to carry out a molten salt-assisted magnesium thermal reduction reaction of montmorillonite and magnesium powder. The reaction time is 3 hours to obtain a mixture containing copper-doped nano-silicon material.
[0046] (4) Grinding the mixture of copper-doped nano-silicon materials, adding deionized water to the ground powder and slowly stirring for 2 hours, filtering to obtain a solid powder product I; adding the solid powder product I to 0.5 mol / L hydrochloric acid and stirring at room temperature for 4 hours, filtering to obtain a solid powder product II; dispersing the solid powder product II in a 0.5% HF solution and stirring for 4 hours to extract, filtering and rinsing with deionized water for multiple times to obtain a solid powder III; placing the solid powder III in a vacuum drying oven at 60° C. for vacuum drying for 10 hours to obtain a copper-doped porous nano-silicon material preform.
[0047] (5) The copper-doped porous nano-silicon material preform is annealed and heat-treated in an argon atmosphere at a temperature of 400° C. for a heat treatment time of 2 h to obtain a copper-doped porous nano-silicon negative electrode material.
[0048] An application of a copper-doped porous nano-silicon negative electrode material as a battery material, specifically:
[0049] according to Figure 7It can be seen that the copper-doped porous nano-silicon negative electrode material prepared in this embodiment has a porous structure, and the copper-doped porous nano-silicon negative electrode material contains only copper, silicon and oxygen elements, and has a single silicon crystal phase. The porous nano-silicon negative electrode material prepared in this embodiment is used as the positive electrode, the metal lithium sheet is used as the negative electrode, the Celgard membrane is used as the separator, the electrolyte is composed of LiPF6 in ethylene carbonate (EC) / diethyl carbonate (DEC) (volume ratio of 3:7) with 10wt% fluoroethylene carbonate (FEC) added, the binder is composed of polyacrylic acid (PAA) and sodium carboxymethyl cellulose (CMC, 6wt%) (PAA / CMC volume ratio of 1:1), the silicon nanosheet, conductive carbon black Super-P, and the binder weight ratio of 7:1.5:1.5 are used to prepare the working electrode, and the battery is assembled in a glove box filled with argon gas, and a constant current charge and discharge test is performed. Figure 8 It can be seen that the reversible capacity of the copper-doped porous nano-silicon negative electrode material is 1370 mAh / g after 2000 cycles at a current density of 200 mA / g.
[0050] Example 3
[0051] A method for preparing a copper-doped porous nano-silicon negative electrode material comprises the following steps:
[0052] (1) preparing a copper sulfate solution, fully stirring the copper sulfate solution and montmorillonite, and then standing for a certain period of time to allow metal ions between montmorillonite layers to exchange ions with copper ions in the copper sulfate solution. After the ion exchange is completed, filtering and collecting, and vacuum drying are performed to obtain copper ion-doped montmorillonite.
[0053] (2) Copper ion-doped montmorillonite, magnesium powder and anhydrous magnesium chloride were mixed in a glove box at a weight ratio of 10:1:100 and ground in a mortar to obtain a molten salt-assisted magnesium thermal reduction raw material.
[0054] (3) The molten salt-assisted magnesium thermal reduction raw material is placed in a stainless steel crucible, transferred to a tubular furnace filled with argon gas, and heated to 1000° C. to carry out a molten salt-assisted magnesium thermal reduction reaction of montmorillonite and magnesium powder. The reaction time is 1 hour to obtain a mixture containing copper-doped nano-silicon material.
[0055] (4) Grinding the mixture of copper-doped nano-silicon materials, adding deionized water to the ground powder and slowly stirring for 10 hours, filtering to obtain solid powder product I; adding the solid powder product I to 0.01 mol / L hydrochloric acid and stirring at room temperature for 10 hours, filtering to obtain solid powder product II; dispersing the solid powder product II into 0.01% HF solution and stirring for 10 hours to extract, filtering and rinsing with deionized water for multiple times to obtain solid powder III; placing the solid powder III in a vacuum drying oven at 40° C. for vacuum drying for 24 hours to obtain a copper-doped porous nano-silicon material preform.
[0056] (5) The copper-doped porous nano-silicon material preform is annealed and heat-treated in an argon atmosphere at a temperature of 1000° C. for a heat treatment time of 1 min to obtain a copper-doped porous nano-silicon negative electrode material.
[0057] An application of a copper-doped porous nano-silicon negative electrode material as a battery material, specifically:
[0058] The copper-doped porous nano-silicon negative electrode material prepared in this embodiment has a porous structure, and the copper-doped porous nano-silicon negative electrode material contains only copper, silicon and oxygen elements and has a single-substance silicon crystal phase. The porous nano-silicon negative electrode material prepared in this embodiment is used as the positive electrode, the metal lithium sheet is used as the negative electrode, the Celgard membrane is used as the separator, the electrolyte is composed of LiPF6 in ethylene carbonate (EC) / diethyl carbonate (DEC) (volume ratio of 3:7) with 10wt% fluoroethylene carbonate (FEC), the binder is composed of polyacrylic acid (PAA) and sodium carboxymethyl cellulose (CMC, 6wt%) (PAA / CMC volume ratio of 1:1), the silicon nanosheet, conductive carbon black Super-P, and the binder weight ratio of 7:1.5:1.5 are used to prepare the working electrode, the battery is assembled in an argon-filled glove box, and the constant current charge and discharge test is carried out. The copper-doped porous nano-silicon negative electrode material has a reversible capacity of 1500mAh / g after 2000 cycles at a current density of 200mA / g.
[0059] Example 4
[0060] A method for preparing a copper-doped porous nano-silicon negative electrode material comprises the following steps:
[0061] (1) preparing a copper sulfate solution, fully stirring the copper sulfate solution and montmorillonite, and then standing for a certain period of time to allow metal ions between montmorillonite layers to exchange ions with copper ions in the copper sulfate solution. After the ion exchange is completed, filtering and collecting, and vacuum drying are performed to obtain copper ion-doped montmorillonite.
[0062] (2) Copper ion-doped montmorillonite, magnesium powder and anhydrous magnesium chloride were mixed in a glove box at a weight ratio of 10:50:10 and ground in a mortar to obtain a molten salt-assisted magnesium thermal reduction raw material.
[0063] (3) The molten salt-assisted magnesium thermal reduction raw material is placed in a stainless steel crucible, transferred to a tubular furnace filled with argon gas, and heated to 400° C. to carry out a molten salt-assisted magnesium thermal reduction reaction of montmorillonite and magnesium powder. The reaction time is 36 hours to obtain a mixture containing copper-doped nano-silicon material.
[0064] (4) Grinding the mixture of copper-doped nano-silicon materials, adding deionized water to the ground powder and slowly stirring for 1 min, filtering to obtain solid powder product I; adding the solid powder product I to 5 mol / L hydrochloric acid and stirring at room temperature for 1 min, filtering to obtain solid powder product II; dispersing the solid powder product II in a 5% HF solution and stirring for 1 min to extract, filtering and rinsing with deionized water for multiple times to obtain solid powder III; placing the solid powder III in a vacuum drying oven at 80° C. for vacuum drying for 1 min to obtain a copper-doped porous nano-silicon material preform.
[0065] (5) The copper-doped porous nano-silicon material preform is annealed and heat-treated in an argon atmosphere at a temperature of 300° C. for 24 h to obtain a copper-doped porous nano-silicon negative electrode material.
[0066] An application of a copper-doped porous nano-silicon negative electrode material as a battery material, specifically:
[0067] The copper-doped porous nano-silicon negative electrode material prepared in this embodiment has a porous structure, and the copper-doped porous nano-silicon negative electrode material contains only copper, silicon and oxygen elements and has a single-substance silicon crystal phase. The porous nano-silicon negative electrode material prepared in this embodiment is used as the positive electrode, the metal lithium sheet is used as the negative electrode, the Celgard membrane is used as the separator, the electrolyte is composed of LiPF6 in ethylene carbonate (EC) / diethyl carbonate (DEC) (volume ratio of 3:7) with 10wt% fluoroethylene carbonate (FEC), the binder is composed of polyacrylic acid (PAA) and sodium carboxymethyl cellulose (CMC, 6wt%) (PAA / CMC volume ratio of 1:1), the silicon nanosheet, conductive carbon black Super-P, and the binder weight ratio is 7:1.5:1.5 to prepare the working electrode, the battery is assembled in an argon-filled glove box, and the constant current charge and discharge test is carried out. The copper-doped porous nano-silicon negative electrode material has a reversible capacity of 1450mAh / g after 2000 cycles at a current density of 200mA / g.
[0068] Comparative Example 1
[0069] A method for preparing a porous nano-silicon negative electrode material comprises the following steps:
[0070] (1) Montmorillonite, magnesium powder and anhydrous sodium chloride were mixed in a glove box at a weight ratio of 10:8:40 and ground in a mortar to obtain a molten salt-assisted magnesium thermal reduction raw material.
[0071] (3) The molten salt-assisted magnesium thermal reduction raw material is placed in a stainless steel crucible, transferred to a tubular furnace filled with argon gas, and heated to 650° C. to carry out a molten salt-assisted magnesium thermal reduction reaction of montmorillonite and magnesium powder. The reaction time is 6 hours to obtain a mixture containing nano-silicon material.
[0072] (4) Grinding the mixture of nano-silicon materials, adding deionized water to the ground powder and slowly stirring for 2 hours, filtering to obtain solid powder product I; adding the solid powder product I to 0.5 mol / L hydrochloric acid and stirring at room temperature for 4 hours, filtering to obtain solid powder product II; dispersing the solid powder product II in a 0.5% HF solution and stirring for 4 hours to extract, filtering and rinsing with deionized water for multiple times to obtain solid powder III; placing the solid powder III in a vacuum drying oven at 60° C. for vacuum drying for 10 hours to obtain a porous nano-silicon material preform.
[0073] (5) The porous nano-silicon material preform is annealed and heat-treated in an argon atmosphere at a temperature of 700° C. for a heat treatment time of 4 h to obtain a porous nano-silicon negative electrode material.
[0074] An application of a porous nano-silicon negative electrode material as a battery material, specifically:
[0075] The porous nano-silicon negative electrode material prepared in this comparative example has a nano-sheet structure and a single silicon crystal phase. The porous nano-silicon negative electrode material prepared in this comparative example is used as the positive electrode, the metal lithium sheet is used as the negative electrode, the Celgard membrane is used as the diaphragm, the electrolyte is composed of LiPF6 in ethylene carbonate (EC) / diethyl carbonate (DEC) (volume ratio of 3:7) with 10wt% fluoroethylene carbonate (FEC), the binder is composed of polyacrylic acid (PAA) and sodium carboxymethyl cellulose (CMC, 6wt%) (PAA / CMC volume ratio of 1:1), the silicon nanosheet, the conductive carbon black Super-P, and the binder weight ratio are 7:1.5:1.5 to prepare the working electrode, the battery is assembled in a glove box filled with argon, and the constant current charge and discharge test is performed. The reversible capacity of the porous nano-silicon negative electrode material is 900mAh / g after 2000 cycles at a current density of 200mA / g.
[0076] according to Figure 5 It can be seen that the electrode surface cracks of the undoped copper porous nano-silicon negative electrode material electrode film are more numerous before and after cycling, the silicon electrode expands more severely, and the electrochemical performance is poor.
[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a copper-doped porous nano-silicon negative electrode material, characterized in that: The steps include: (1) mixing a copper salt solution and montmorillonite and allowing the mixture to stand, then filtering, collecting and vacuum drying the mixture to obtain copper ion-doped montmorillonite; (2) mixing copper ion-doped montmorillonite, magnesium powder and metal chloride evenly under anhydrous and oxygen-free conditions to obtain a molten salt-assisted magnesium thermal reduction raw material; (3) subjecting the raw material to magnesium thermal reduction reaction under anhydrous and oxygen-free atmosphere with the assistance of molten salt to obtain a mixture containing copper-doped nano-silicon material; (4) washing the copper-doped nano-silicon material mixture with water and an acid solution in sequence and filtering the mixture, and vacuum drying the filtered product to obtain a copper-doped porous nano-silicon material preform; (5) The copper-doped porous nano-silicon material preform is heat-treated in a protective gas to obtain a copper-doped porous nano-silicon negative electrode material.
2. The method for preparing the copper-doped porous nano-silicon negative electrode material according to claim 1, characterized in that: The copper salt is at least one of copper chloride, copper sulfate and copper nitrate; the metal chloride is at least one of sodium chloride, potassium chloride, magnesium chloride and calcium chloride.
3. The method for preparing the copper-doped porous nano-silicon negative electrode material according to claim 1, characterized in that: The mass volume ratio of the montmorillonite to the copper salt solution is (0.1-1):(1-10); the concentration of the copper salt solution is 0.1-10 mol / L.
4. The method for preparing the copper-doped porous nano-silicon negative electrode material according to claim 1, characterized in that: The mass ratio of the copper ion-doped montmorillonite, magnesium powder and metal chloride is 1:(0.1-5):(1-10).
5. The method for preparing the copper-doped porous nano-silicon negative electrode material according to claim 1, characterized in that: The temperature of the magnesium thermal reduction reaction is 400-1000° C. and the time is 1-36 hours.
6. The method for preparing the copper-doped porous nano-silicon negative electrode material according to claim 1, characterized in that: In the step (4), the acid solution cleaning includes first cleaning with acid A and then cleaning with acid B; the acid A is at least one of hydrochloric acid, sulfuric acid, and nitric acid, and the acid B is at least one of hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid.
7. The method for preparing the copper-doped porous nano-silicon negative electrode material according to claim 1, characterized in that: The concentration of the A acid is 0.01-5 mol / L, and the cleaning time is 1 min-10 h; the mass percentage concentration of the B acid is 0.01%-10%, and the cleaning time is 1 min-10 h.
8. The method for preparing the copper-doped porous nano-silicon negative electrode material according to claim 1, characterized in that: The vacuum drying process is performed at a temperature of 40 to 80° C. and for a time of 1 minute to 24 hours.
9. The method for preparing the copper-doped porous nano-silicon negative electrode material according to claim 1, characterized in that: The heat treatment temperature is 300-1000° C. and the time is 1 min-24 h.
10. The method for preparing the copper-doped porous nano-silicon negative electrode material according to claim 1, characterized in that: The anhydrous and oxygen-free gas atmosphere is one or more of nitrogen, argon, hydrogen and helium.
Citation Information
Patent Citations
Porous silicon-copper composite material and preparation method and application thereof
CN105826528A
Method for preparing silicon nanosheet negative electrode material by reducing montmorillonite based on fused salt
CN117303370A