A high nickel lithium ion battery positive electrode material with thermal safety and preparation method thereof
By using the secondary sintering process of thermally stable element MT and amphoteric element coating technology in the positive electrode material of high nickel lithium-ion battery, the problems of material structural instability and low thermal decomposition temperature are solved, and high energy density and heat are achieved The combination of stability improves safety and performance.
Patent Information
- Application Number
- CN202210191368.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-02-28
AI Technical Summary
The positive electrode material of high-nickel lithium-ion battery has problems such as structural instability and low thermal decomposition temperature during the high-nickelization process, which leads to an increase in safety hazards and limits its widespread application.
The positive electrode material of high-nickel lithium-ion battery is prepared by secondary sintering process containing thermal stability element MT. By coating the compound with uniform amphoteric elements on the surface and inside of spherical particles, the development of internal stress of the crystal lattice is suppressed and the thermal stability of the material is improved. sex.
It achieves high energy density and excellent thermal stability, improves the safety of the material, delays the occurrence of danger, and is suitable for maintaining chemical thermal stability in higher temperature ranges.
Smart Images

Figure BDA0003524566610000091 
Figure HDA0003524566620000011 
Figure HDA0003524566620000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a high-nickel lithium ion battery positive electrode material with thermal safety and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are one of the most important devices for energy storage applications. They have the advantages of high energy density and cycle efficiency, low self-discharge, and no memory effect. They have a broader application prospect in power batteries. With the progress of society, the demand for energy has gradually increased the requirements for lithium batteries. Layered lithium-ion materials composed of nickel-cobalt-manganese elements have developed rapidly in recent years due to the synergistic effect of the three elements on the materials. In particular, ternary materials with high nickel and low cobalt not only provide high energy density but also reduce the various costs brought by elemental cobalt, and have been the focus of research. However, the subsequent high nickelization brings instability in the material structure, and there will be differences in crystal structure such as Li / Ni mixing and harsh conditions in the preparation process, resulting in a large theoretical capacity difference. In addition, as the Ni content of high-nickel ternary materials increases, the thermal decomposition temperature of the material increases while the capacity continues to decrease. It has the disadvantage of being easily decomposed when heated within 350°C, which leads to increased safety hazards. High-nickel positive electrode materials can provide high capacity and are favored by people, but safety issues have always restricted the widespread application of high-nickel materials. In vehicle applications, the temperature will become uncontrolled and cause fires or even explosions. The positive electrode material is one of the core components for providing energy for lithium-ion batteries. It is very important to develop positive electrode materials with high energy density and excellent thermal stability. Summary of the invention
[0003] In view of this, the technical problem to be solved by the present invention is to provide a high-nickel lithium-ion battery positive electrode material with thermal safety and a preparation method and application thereof. The high-nickel lithium-ion battery positive electrode material provided by the present invention has high energy density and excellent thermal stability.
[0004] The present invention provides a method comprising a thermally stable element M Td And secondary sintering process high nickel lithium ion positive electrode materials and methods coated with elements of similar properties.
[0005] The present invention provides a high nickel lithium ion battery positive electrode material with thermal safety, the chemical formula of which is Li 1+ x Ni a Co b Mn c M Td O2;
[0006] Wherein, 0.01≤x≤0.03, 0.8≤a<1, 0.03≤b≤0.1, 0.5≤c / b≤1, 0.006≤d≤0.016 and a+b+c+d=1; M T One or more selected from Al, Zr, Si, Ti, Mg, W, Mo, P, Ta, Ce, Nb, Mn, Y and F;
[0007] The high nickel lithium ion battery positive electrode material is a spherical particle, and the thermally stable element M T The level of the high nickel lithium ion battery positive electrode material is reduced from the surface of the spherical particle to the interior of the spherical particle. T ;
[0008] The surface of the high-nickel lithium-ion battery positive electrode material is coated with one or more compounds of amphoteric elements.
[0009] Preferably, the material structure is loose inside, and the surface particles are arranged in a divergent manner;
[0010] The normal plane of the long diameter of the surface particles and the normal plane of the long diameter of the internal particles are in a vertical relationship in three-dimensional space.
[0011] Preferably, the molar ratio of Li to metal ions is 1.00 to 1.08;
[0012] The particle compressive strength of the positive electrode material is ≥89.8Mpa;
[0013] The particle size distribution mode of the positive electrode material is between 0.34 and 0.60 μm;
[0014] The average unit cell volume of the positive electrode material is between.
[0015] The present invention also provides a method for preparing the above-mentioned high-nickel lithium-ion battery positive electrode material with thermal safety, comprising the following steps:
[0016] A) mixing a lithium source, a high-nickel ternary precursor and a first additive and sintering them under oxygen-containing gas conditions;
[0017] The first additive contains one or more elements of Al, Zr, Si, Ti, Mg, W, Mo, P, Ta, Ce, Nb, Mn, Y and F.
[0018] Preferably, the oxygen-containing gas is an oxygen-containing atmosphere with an oxygen content of ≥ 98 vol%.
[0019] Preferably, the sintering temperature is 650-850° C., the sintering heating rate is 2° C. / min-10° C. / min, and the sintering holding time is less than 20 h.
[0020] Preferably, after the sintering step in step A), the sintered product is crushed, screened, washed and dried to obtain a washed material;
[0021] Then the washed material is mixed with a second additive and sintered for a second time, and then sieved to obtain a high-nickel lithium-ion battery positive electrode material.
[0022] Preferably, the water washing temperature is <40°C, and the water-to-material mass ratio is (0.5-3):1;
[0023] The free lithium content in the water-washed material needs to be ≤1400ppm.
[0024] Preferably, the second additive is selected from one or more amphoteric compounds;
[0025] The atmosphere condition of the second sintering is an oxygen-containing atmosphere, the sintering temperature is ≤600° C., the sintering time is <15h, and the sintering heating rate is 2° C. / min to 10° C. / min.
[0026] Preferably, the surface of the water-washed material is coated with amphoteric elements, and the coating amount is less than 5000 ppm.
[0027] Compared with the prior art, the present invention provides a high nickel lithium ion battery positive electrode material with thermal safety, the chemical formula of which is Li 1+x Ni a Co b Mn c M Td O2; where 0.01≤x≤0.03, 0.8≤a<1, 0.03≤b≤0.1, 0.5≤c / b≤1, 0.006≤d≤0.016 and a+b+c+d=1; M T One or more selected from Al, Zr, Si, Ti, Mg, W, Mo, P, Ta, Ce, Nb, Mn, Y and F; the high nickel lithium ion battery positive electrode material is spherical particles, the thermally stable element M T The level of M is reduced from the surface of the spherical particles to the inside of the spherical particles; the surface of the high nickel lithium ion battery positive electrode material is coated with one or more compounds of amphoteric elements. In the present invention, the surface and internal M of the positive electrode material particles T It has the characteristics of being non-uniform. The material particles are essentially high-nickel NCM ternary materials inside, while the rest of the material is NCMM. T High nickel quaternary material. Particle surface cation M T The addition of O 2-, this effect inhibits the escape of [O] during the charging process, and replaces part of the framework ions and fills the lattice gaps, which effectively inhibits the development of internal stress in the lattice, thereby improving the stability of the crystal structure of the high-nickel positive electrode material; this structure is beneficial to inhibit the surface side reactions of the primary particles and effectively improve the stress release during the lithium ion insertion and extraction process on the basis of maintaining the capacity. The high-nickel lithium-ion battery positive electrode material provided by the present invention has a high thermal decomposition temperature, the harmful effect of the doping elements on the internal crystal structure of the spherical particles is low, and the discharge capacity is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A process flow chart of the preparation of the high nickel lithium ion battery positive electrode material provided by the present invention;
[0029] Figure 2 For the high nickel ternary precursor Ni 0.86 Co 0.06 Mn 0.08 Cross-section of (OH)2;
[0030] Figure 3 This is a cross-sectional view of the high-nickel lithium-ion battery positive electrode material prepared by the present invention;
[0031] Figure 4 This is a SEM photo of the high-nickel lithium-ion battery positive electrode material prepared by the present invention;
[0032] Figure 5 for Figure 4 The diameter width distribution histogram of visible primary particles of medium- and high-nickel lithium-ion battery cathode materials;
[0033] Figure 6 It is the single value diagram of Example 1 and Comparative Example 1;
[0034] Figure 7 It is a box plot of Example 1 and Comparative Example 1;
[0035] Figure 8 It is the charge and discharge curve of Example 1;
[0036] Fig. 9 is the DSC curve of Example 1;
[0037] Fig.10 is the DSC curve of Example 2;
[0038] Fig.11 It is the charge and discharge curve of comparative example 1;
[0039] Fig.12 It is the DSC curve of Comparative Example 1;
[0040] Fig.13 It is the SEM picture of comparative example 6;
[0041] Fig.14 This is the histogram of the primary particles of Comparative Example 6. DETAILED DESCRIPTION
[0042] The present invention provides a high nickel lithium ion battery positive electrode material with thermal safety, the chemical general formula of which is Li 1+ x Ni a Co b Mn c M Td O2;
[0043] Wherein, 0.01≤x≤0.08, preferably 0.03, 0.05, 0.06, or any value between 0.01 and 0.08;
[0044] 0.8≤a<1, preferably 0.83, 0.86, 0.9, 0.95, 0.99, or any value between 0.8 and 1 but not 1;
[0045] 0.03≤b≤0.1, preferably 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, or any value between 0.03 and 0.1;
[0046] 0.5≤c / b≤1, preferably 0.5, 0.6, 0.7, 0.8, 0.9, 1, or any value between 0.5 and 1;
[0047] 0.006≤d≤0.016, preferably 0.006, 0.008, 0.010, 0.012, 0.014, 0.016, or any value between 0.006 and 0.016;
[0048] a+b+c+d=1;
[0049] M T One or more selected from Al, Zr, Si, Ti, Mg, W, Mo, P, Ta, Ce, Nb, Mn, Y and F, preferably one or two of Al and Zr.
[0050] Through comparison of physical and chemical test data, it is known that when the molar ratio of Li to metal elements in the positive electrode material of high-nickel lithium-ion batteries is between 1.01 and 1.08, it is called a lithium-rich state, and the DSC thermal decomposition temperature of the material is relatively high.
[0051] The high nickel lithium ion battery positive electrode material is a spherical particle, and the thermally stable element M T The level of M decreases from the surface of the spherical particles to the inside of the spherical particles. T The level gradually decreases from the surface to the inside in the longitudinal section of the spherical particles;
[0052] The surface of the high-nickel lithium-ion battery positive electrode material is coated with one or more compounds of amphoteric elements.
[0053] In the high nickel positive electrode material of the present invention, the element M which can improve the thermal stability of the material is added. T After being mixed with NCM precursor particles and sintered at high temperature, M T Elements gradually penetrate from high-concentration areas into low-concentration areas, and are doped on the surface of the polycrystalline nickel-cobalt-manganese ternary cathode matrix to achieve the M T The material particles are essentially high-nickel NCM ternary materials inside, while the surface part of the material is NCMM T High nickel quaternary material. Particle surface cation M T The addition of O 2- This effect inhibits the escape of [O] during the charging process, replaces part of the framework ions and fills the lattice voids, which effectively inhibits the development of internal stress in the lattice, thereby improving the crystal structure stability of the high-nickel positive electrode material; this structure is beneficial to inhibit the surface side reactions of primary particles and effectively improve the stress release in the process of lithium ion insertion and extraction while maintaining the capacity.
[0054] The material structure is irregularly arranged inside, and the surface particles are arranged in a divergent manner;
[0055] The normal plane of the particle length diameter on the surface layer and the normal plane of the particle length diameter inside the surface layer are in a vertical relationship in three-dimensional space.
[0056] The particle compressive strength of the positive electrode material is ≥89.8Mpa;
[0057] The particle size distribution mode of the positive electrode material is between 0.34 and 0.60 μm; wherein the particle size distribution mode refers to the width of the primary particle size on the length, width and height measurement scale in three-dimensional space. If it is not in this range, it cannot maintain the thermal stability of the crystal structure. Smaller particles are more likely to transfer heat after being heated, and more primary particle size distributions are greater than the upper limit of this range, which is more likely to cause spherical particle collapse.
[0058] The average unit cell volume of the positive electrode material is Preferably, the unit cell volume after surface doping is
[0059] The present invention also provides a method for preparing the above-mentioned high-nickel lithium-ion battery positive electrode material with thermal safety, comprising the following steps:
[0060] A) mixing a lithium source, a high-nickel precursor and a first additive and sintering them under oxygen-containing gas conditions to obtain a high-nickel lithium-ion battery positive electrode material.
[0061] Wherein, the lithium source is selected from one or any combination of lithium hydroxide, hydrated hydroxide and carbonate;
[0062] The high-nickel ternary precursor is selected from nickel-cobalt-manganese hydroxide and nickel-cobalt-manganese coprecipitated hydroxide;
[0063] The first additive contains one or more elements selected from the group consisting of Al, Zr, Si, Ti, Mg, W, Mo, P, Ta, Ce, Nb, Mn, Y and F. In some specific embodiments of the present invention, the additive contains at least one doping ion, Mg 2+ 、Ti 4 + 、Zr 4+ 、Si 4+ 、、W 6+ 、Al 3+ 、Mo 6+ , P 5+ 、 5+ 、Ce 3+ , Nb 5+ , Mn 4+ , Y 3+ and F - The first additive is preferably a compound containing one or more of the above elements.
[0064] Wherein, when the ingredients are prepared before mixing, the molar ratio of Li to the metal elements other than lithium is in the range of 1.00 to 1.15.
[0065] After the mixed material is obtained, the mixed material is sintered under oxygen-containing gas conditions, wherein the oxygen-containing gas is an oxygen-containing atmosphere with an oxygen content of ≥ 98 vol%.
[0066] Specifically, the obtained mixed material is loaded into a sagger after being tested for uniformity, and the mixed material is sintered in an oxygen-containing atmosphere with an oxygen content of ≥98 vol%.
[0067] The sintering temperature is 650-850°C, preferably 650, 700, 750, 800, 850, preferably any value between 650 and 850°C, the sintering heating rate is 2°C / min-10°C / min, preferably 2, 4, 6, 8, 10, or any value between 2°C / min and 10°C / min, and the sintering holding time is <20h.
[0068] In a specific embodiment of the present invention, after the sintering step, the sintered product is crushed, screened, washed and dried to obtain a washed material;
[0069] Then the washed material is mixed with a second additive and sintered for a second time, and then sieved to obtain a high-nickel lithium-ion battery positive electrode material.
[0070] The crushing is carried out by first using a jaw crusher and then mechanically crushing. The specific method of screening is a method known to those skilled in the art.
[0071] The powder obtained by screening is washed and dried to obtain a washed material. The washing conditions are as follows: the washing temperature is <40°C, the water-to-material mass ratio is (0.5-3):1, the washing speed is 300-400r / min, and the washing time is 10-20min; after washing, the powder is filtered and then placed in an atmosphere vacuum drying oven for drying at a vacuum drying temperature of 120°C for not less than 4h, oxygen is passed through, and the powder is sieved to ensure that the free lithium content in the dried material is ≤1400ppm.
[0072] In the present invention, the water washing is carried out in a weakened water washing manner. That is, a certain mass of lithium hydroxide is first dissolved in pure water, and then the material is added to the solution, which reduces the structural remodeling of the surface of the washed particles and reduces the loss of residual lithium on the surface, which has a positive effect on the subsequent thermal safety.
[0073] Next, the washed material is mixed with a second additive for a second sintering. The second additive is selected from the group consisting of but not limited to M T The amount of the second additive added is ≤5000ppm.
[0074] The atmosphere condition of the second sintering is an oxygen-containing atmosphere, the sintering temperature is 350-600°C, preferably Al2O3 and B(OH)3; the sintering time is <15h, and the sintering heating rate is 2°C / min-10°C / min, preferably 2, 4, 6, 8, 10, or any value between 2°C / min and 10°C / min.
[0075] After the second sintering is completed, the sintering product is naturally cooled to obtain a sintered product, and the sintered product is sieved to obtain a high-nickel lithium-ion battery positive electrode material with thermal safety.
[0076] See also Figure 1 , Figure 1 This is a process flow chart for preparing the high-nickel lithium-ion battery positive electrode material provided by the present invention.
[0077] In the present invention, by controlling the additive M T The type and quantity of primary particles with a specific diameter and width, and spherical particles with different arrangements of the surface and the interior, are used to obtain a high-nickel lithium-ion battery positive electrode material, which has a high energy density and excellent thermal stability.
[0078] The method of the present invention has low requirements on equipment, is easy to industrialize, has easy conditions to achieve, and has low processing costs;
[0079] The high nickel material prepared by the method has a high thermal decomposition temperature, the harmful effect of the doping elements on the internal crystal structure of the spherical particles is relatively low, and the discharge capacity is high;
[0080] The present invention has low requirements on precursors, is easy to implement and has low raw material costs.
[0081] In the "a high nickel lithium ion battery positive electrode material with thermal safety and its preparation method" described in the present invention, "thermal safety" means: the DSC decomposition temperature of the positive electrode material is increased, that is, the positive electrode material can maintain chemical thermal stability in a higher temperature range, delaying the occurrence of danger to a certain extent, after disassembling the fully charged half-battery, the dried positive electrode sheet is matched with a considerable amount of electrolyte and then subjected to DSC detection, and the peak temperature of the heat absorption / release peak is above 230.50°C; "high nickel" means: the molar content of Ni element in the polycrystalline nickel cobalt manganese oxide matrix accounts for more than 80% of the molar amount of all metal elements. DSC uses a differential scanning calorimeter to characterize the phase safety temperature of the positive electrode material; the lithium-rich state is a state in which the number of lithium elements is greater than 1 compared to the number of metal elements.
[0082] In order to further understand the present invention, the high-nickel lithium-ion battery positive electrode material with thermal safety provided by the present invention, its preparation method and application are described below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0083] Example 1
[0084] Ni 0.86 Co 0.06 Mn 0.08 (OH)2 and LiOH·H2O are added into a 10L high-speed mixer at a molar ratio of 1:1.08, aluminum hydroxide at a stoichiometric ratio of 0.01 with transition metal ions, and 5000ppm ZrO2 for mixing at a rate of 1000r / min for 10 to 30min; the mixture is first sintered at 850°C for 15h with a heating rate of 2°C / min, sieved through a 325-mesh sieve, and mechanically crushed; then washed with water under the conditions of a water-to-material ratio of 1:0.5, a rotation speed of 360r / min, and a washing time of 30min, and then placed in a vacuum oven for drying at 120°C for 4h. After being taken out, 2000ppm of boric acid is first added, and then 2000ppm of aluminum oxide is added. After being mixed evenly, the mixture is sintered for a second time at a sintering temperature of 380°C for 10h with a heating rate of 2°C / min. After being taken out, the mixture is sieved and crushed to obtain a high-nickel lithium-ion battery positive electrode material. The particle compressive strength of the prepared positive electrode material is 90.8Mpa; the average unit cell volume is
[0085] See also Figure 2 and Figure 3 , Figure 2 For the high nickel ternary precursor Ni 0.86 Co 0.06 Mn 0.08 Cross-section of (OH)2; Figure 3 This is a cross-sectional view of the high-nickel lithium-ion battery positive electrode material prepared by the present invention.
[0086] from Figure 3 It can be found that the normal plane of the distribution direction of the particles in the dotted part is perpendicular to the normal plane of the surface particle distribution. Such uneven spatial distribution of microstrain effectively curbs the expansion of stress stripes of material decomposition, thereby significantly increasing the temperature of its thermal decomposition. It successfully improves its thermal stability without reducing the proportion of Ni element in the high-nickel ternary positive electrode material, that is, without reducing its specific capacity.
[0087] The obtained positive electrode material was charged to 4.3V at 0.2C and a cut-off current of 0.05C. The battery was disassembled and the corresponding electrode pieces were cut. The corresponding mass of electrolyte was placed in a crucible to simulate the environment of the material under the working voltage and perform a DSC test.
[0088] The half capacity was measured to be 204.3 mAh / g and the DSC thermal decomposition temperature was 246.50°C.
[0089] After testing with a particle pressure tester, it was found that the average compressive strength of the secondary spherical particles in the material was 125.3Mpa, and the compressive strength of the minimum particle was 89.8Mpa.
[0090] See also Figure 4 and Figure 5 , Figure 4 This is a SEM photo of the high-nickel lithium-ion battery positive electrode material prepared by the present invention. Figure 5 for Figure 4 The diameter width distribution histogram of visible primary particles of medium- and high-nickel lithium-ion battery cathode materials. Figure 5 It can be seen that the widest distribution of particle size is between 0.3 and 0.6 μm.
[0091] Comparative Example 1
[0092] Ni 0.86 Co 0.06 Mn 0.08(OH)2 and LiOH·H2O were added to a 10L high-speed mixer at a molar ratio of 1:1.08 and mixed at 1000r / min for 10 to 30min; after the first sintering at 850℃ for 15h, the heating rate was 8℃ / min, sieved through a 325-mesh sieve, and mechanically crushed, wherein the molar ratio of lithium element to transition metal element in the precursor was 1.04; then washed with water, the washing conditions were a water-to-material ratio of 1:0.5, a rotation speed of 360r / min, and a washing time of 30 minutes, placed in a vacuum oven and dried at 120℃ for 4h, taken out and added with 600ppm boric acid, mixed evenly, and then sintered for the second time, the sintering temperature was 380℃, 10h, the heating rate was 2℃ / min, taken out, sieved, and crushed. The half-capacity was measured to be 208.1mAh / g and the DSC temperature was 220.32℃
[0093] A two-sample t-test was performed on Example 1 and Comparative Example 1 to verify whether the primary particle diameter width distribution on the surface of the spherical particles is related to the DSC thermal decomposition temperature. Figures 6-7 and Table 1. Among them, Figure 6 is the single value graph of sample 1 and sample 2, Figure 7 : It is the wire box diagram of sample 1 and sample 2. Sample 1 is the high nickel positive electrode material prepared in Example 1, and sample 2 is the high nickel material described in the comparative example; in the figure, C2 represents Example 1, and C5 represents comparative example 1.
[0094] Table 1
[0095]
[0096] The above statistical results show that different particle size distributions have an impact on the DSC thermal decomposition temperature. The thermal safety performance of high nickel positive electrode material sample 1 prepared by the preparation process of the present invention is better than that of sample 2.
[0097] Based on this, the particle compressive strength of the positive electrode material is 85.9 MPa and the particle size distribution mode of the positive electrode material is between 0.34 and 0.6 μm.
[0098] Comparative Example 2
[0099] Ni 0.86 Co 0.06 Mn 0.08(OH)2 and LiOH·H2O were added to a 10L high-speed mixer at a molar ratio of 1:1.04, alumina with a stoichiometric ratio of 0.01 to transition metal ions, and 5000ppm ZrO2 for 10-30min at 1000r / min; sintered for the first time at 850℃ for 12h, with a heating rate of 2℃ / min, sieved through a 325-mesh sieve, and mechanically crushed, wherein the molar ratio of lithium element to transition metal element in the precursor was 1.04; then washed with water, the washing conditions were a water-to-material ratio of 1:0.5, a rotation speed of 360r / min, and a washing time of 20 minutes, placed in a vacuum oven at 120℃ for 4h, taken out and added with 3000ppm of boric acid, mixed evenly, and sintered for the second time, the sintering temperature was 380℃, 5h, and the heating rate was 2℃ / min, taken out, sieved, and crushed. The DSC result was 222.48℃.
[0100] Comparative Example 3
[0101] The quaternary Ni 0.85 Co 0.06 Mn 0.08 Al 0.01 (OH)2 high nickel precursor, LiOH·H2O at a molar ratio of 1:1.08 and 5000ppm ZrO2 were added to a 10L high speed mixer and mixed at 1000r / min for 10-30min; sintered for the first time at 850℃ for 12h; the subsequent steps were the same as in the example, and the obtained positive electrode material had a particle compressive strength of 82.8Mpa. The 0.2C discharge capacity was 200.2mAh / g and the DSC peak temperature was 220.6℃
[0102] Comparative Example 4
[0103] Ni 0.9 Co 0.05 Mn 0.05(OH)2 and LiOH·H2O in a molar ratio of 1:1.04, alumina with a stoichiometric ratio of 0.01 to transition metal ions, and 5000ppm ZrO2 are added to a 10L high-speed mixer and mixed at 1000r / min for 10 to 30min; after the first sintering at 850°C for 12h and a heating rate of 2°C / min, the mixture is sieved through a 325-mesh sieve and mechanically crushed, wherein the molar ratio of lithium element to transition metal element in the precursor is 1.04; then washed with water, the washing conditions are a water-to-material ratio of 1:0.5, a rotation speed of 360r / min, and a washing time of 20 minutes, and then placed in a vacuum oven and dried at 120°C for 4h. After taking out, the same coating agent as in Example 1 is added, and after mixing evenly, a second sintering is carried out, the sintering temperature is 380°C for 5h, the heating rate is 2°C / min, and after taking out, the mixture is sieved and crushed. It was measured that the particle compressive strength of the positive electrode material is 78.6Mpa and the average unit cell volume is The 0.2C discharge capacity is 211.2 mAh / g and the DSC peak temperature is 208.6°C.
[0104] Comparative Example 5
[0105] Ni 0.83 Co 0.06 Mn 0.11 (OH)2 and LiOH·H2O were added into a 10L high-speed mixer at a molar ratio of 1:1.08 for mixing at a rate of 1000r / min for 10 to 30min; the mixture was first sintered at 850℃ for 15h, with a heating rate of 2℃ / min, passed through a 325-mesh sieve, and mechanically crushed; and then washed with water under the conditions of a water-to-material ratio of 1:0.5, a rotation speed of 360r / min, and a washing time of 10 minutes. The DSC peak temperature was 225.5℃
[0106] Comparative Example 6
[0107] The same raw materials as in Example 1 were mixed, sintered for the first time at 750°C for 15 h, washed with water, and sintered for the same second time to obtain the following material: The primary particle diameter mode was 0.2-0.3 μm, and the DSC decomposition temperature was 220.35°C. Fig.13 and Fig.14 The morphology and distribution of primary particles are listed
[0108] Example 2
[0109] Ni 0.90 Co 0.05 Mn 0.05(OH)2 and LiOH·H2O in a molar ratio of 1:1.08, Al(OH)3 and 5000ppm ZrO2 of the corresponding amount were added to a 10L high-speed mixer for mixing at a rate of 1000r / min for 10 to 30min; the first sintering was performed at 850℃ for 15h, and the subsequent steps were the same as in Example 1. The average unit cell volume was obtained by testing. The particle strength is 91Mpa, the primary particle diameter is about 0.42μm, the 0.2C capacity is 202.8mAh / g, and the DSC peak temperature is 238.6℃
[0110] Example 3
[0111] Ni 0.86 Co 0.06 Mn 0.08 (OH)2 and LiOH·H2O in a molar ratio of 1:1.15, 0.05mol% MgO and 5000ppm ZrO2 were added to a 10L high-speed mixer for mixing at a rate of 1000r / min for 10 to 30min; the first sintering was performed at 850℃ for 15h, and the subsequent steps were the same as in Example 1. The DSC peak temperature was measured to be 238.2℃
[0112] Example 4
[0113] Ni 0.86 Co 0.06 Mn 0.08 (OH)2 and LiOH·H2O were added into a 10L high-speed mixer at a molar ratio of 1:1.08, along with 1mol% (NH4)2MoO4 and 5000ppm ZrO2 for mixing at a rate of 1000r / min for 10 to 30min. After the first sintering at 850℃ for 15h, the subsequent steps were the same as those in Example 1. The average unit cell volume was measured to be The particle strength is 90.5 MPa and the DSC result is 240.2°C.
[0114] Example 5
[0115] Ni 0.86 Co 0.06 Mn 0.08 (OH)2 and LiOH·H2O in a molar ratio of 1:1.08, 1 mol% Al(OH)3 and 5000ppm ZrO2 were added into a 10L high-speed mixer for mixing at a rate of 1000r / min for 10 to 30min; after the first sintering at 850℃ for 15h, water washing and secondary sintering coating with 2000ppm boric acid and 1000ppm MnO2, the DSC result was measured to be 245.2℃.
[0116] Example 6
[0117] Ni 0.86 Co 0.06 Mn 0.08 (OH)2 and LiOH·H2O in a molar ratio of 1:1.08, 1 mol% Al(OH)3 and 5000ppm ZrO2 were added to a 10L high-speed mixer for mixing at a rate of 1000r / min for 10 to 30min; the first sintering was performed at 850℃ for 15h, the heating rate was 6℃ / min, and the water washing and secondary sintering were coated with 2000ppm of boric acid. The average unit cell volume was measured to be The DSC result was 238.0°C.
[0118] Example 7
[0119] Ni 0.83 Co 0.06 Mn 0.11 (OH)2 and LiOH·H2O in a molar ratio of 1:1.08 were added to a 10L high-speed mixer with 1mol% Al(OH)3 and 5000ppm ZrO2 for mixing at a rate of 1000r / min for 10 to 30min; the first sintering was performed at 850℃ for 15h, and the water washing and second sintering coating were the same as in Example 1. The average unit cell volume of the obtained positive electrode material was The particle strength is 103.5Mpa, the 0.2C discharge capacity is 207.1mAh / g, and the DSC peak temperature is 253.5℃
[0120] Example 8
[0121] Ni 0.86 Co 0.06 Mn 0.08 (OH)2 and LiOH·H2O are added into a 10L high-speed mixer at a molar ratio of 1:1.08, and W2O5, 500ppm MgO and 3500ppm ZrO2, which account for 500ppm of transition metal ions, are mixed at a rate of 1000r / min for 10 to 30min; the mixture is first sintered at 850℃ for 15h, with a heating rate of 2℃ / min, passed through a 325-mesh sieve and mechanically crushed; the mixture is then washed with water, with the washing conditions being a water-to-material ratio of 1:0.5, a rotation speed of 360r / min and a washing time of 30min, and then placed in a vacuum oven and dried at 120℃ for 4h. After being taken out, 2000ppm of boric acid is first added, and then 2000ppm of alumina is added. After being mixed evenly, the mixture is sintered for a second time, with a sintering temperature of 380℃ for 10h and a heating rate of 2℃ / min. After being taken out, the mixture is sieved and crushed to obtain a high-nickel lithium-ion battery positive electrode material.
[0122] Example 9
[0123] Ni 0.86 Co 0.06 Mn 0.08 (OH)2 and LiOH·H2O are added into a 10L high-speed mixer at a molar ratio of 1:1.08, aluminum hydroxide with a stoichiometric ratio of 0.15 to transition metal ions, Si(TEOS) with a mass concentration of 1000ppm of transition metal ions and 2500ppm of ZrO2 to mix at a rate of 1000r / min for 10 to 30min; the mixture is first sintered at 850°C for 15h with a heating rate of 2°C / min, sieved through a 325-mesh sieve and mechanically crushed; then washed with water under the conditions of a water-to-material ratio of 1:0.5, a rotation speed of 360r / min and a washing time of 30min, placed in a vacuum oven and dried at 120°C for 4h, taken out and added with 2000ppm of boric acid, mixed evenly and then sintered for a second time at a sintering temperature of 380°C for 10h with a heating rate of 2°C / min, taken out, sieved and crushed to obtain a high-nickel lithium-ion battery positive electrode material.
[0124] Example 10
[0125] Ni 0.86 Co 0.06 Mn 0.08 (OH)2 and LiOH·H2O are added into a 10L high-speed mixer at a molar ratio of 1:1.08, aluminum hydroxide at a stoichiometric ratio of 0.1 to transition metal ions, MnO2 with a mass concentration of 1000ppm of transition metal ions, 500ppm of Si and 3000ppm of ZrO2 at a mass concentration of 1000ppm of transition metal ions, at a rate of 1000r / min for 10 to 30min; the mixture is first sintered at 850°C for 15h with a heating rate of 2°C / min, sieved through a 325-mesh sieve and mechanically crushed; the mixture is then washed with water under the conditions of a water-to-material ratio of 1:0.5, a rotation speed of 360r / min and a washing time of 30min, and then placed in a vacuum oven and dried at 120°C for 4h. After being taken out, 2000ppm of boric acid is added, and after being evenly mixed, the mixture is sintered for a second time at a sintering temperature of 380°C for 10h with a heating rate of 2°C / min. After being taken out, the mixture is sieved and crushed to obtain a high-nickel lithium-ion battery positive electrode material.
[0126] Embodiment 11
[0127] Ni 0.86 Co 0.06 Mn 0.08(OH)2 and LiOH·H2O in a molar ratio of 1:1.08 are added to a 10L high-speed mixer for mixing with P2O5, 1000ppm NbO2 and 2800ppm ZrO2 with a mass concentration of transition metal ions of 1000ppm at a rate of 1000r / min for 10 to 30min; the mixture is first sintered at 850°C for 15h with a heating rate of 2°C / min, sieved through a 325-mesh sieve and mechanically crushed; then washed with water under the conditions of a water-to-material ratio of 1:0.5, a rotation speed of 360r / min and a washing time of 30min, placed in a vacuum oven and dried at 120°C for 4h, 2000ppm of boric acid is added after taking out, and then 2000ppm of alumina is added, and the mixture is evenly mixed and then sintered for a second time at a sintering temperature of 380°C for 10h with a heating rate of 2°C / min. After taking out, the mixture is sieved and crushed to obtain a high-nickel lithium-ion battery positive electrode material.
[0128] Example 12
[0129] Ni 0.86 Co 0.06 Mn 0.08 (OH)2 and LiOH·H2O are added into a 10L high-speed mixer at a molar ratio of 1:1.08, and CeO4, 100ppm Ti(TBOT) and 3500ppm ZrO2, which account for 400ppm of transition metal ions, are mixed at a rate of 1000r / min for 10 to 30min; the mixture is first sintered at 850℃ for 15h, with a heating rate of 2℃ / min, passed through a 325-mesh sieve and mechanically crushed; the mixture is then washed with water, with the washing conditions being a water-to-material ratio of 1:0.5, a rotation speed of 360r / min and a washing time of 30min, and then placed in a vacuum oven and dried at 120℃ for 4h. After being taken out, 2000ppm of boric acid is first added, and then 2000ppm of alumina is added. After being mixed evenly, the mixture is sintered for a second time, with a sintering temperature of 380℃ for 10h and a heating rate of 2℃ / min. After being taken out, the mixture is sieved and crushed to obtain a high-nickel lithium-ion battery positive electrode material.
[0130] Example 13
[0131] Ni 0.86 Co 0.06 Mn 0.08(OH)2 and LiOH·H2O in a molar ratio of 1:1.08 were added into a 10L high-speed mixer with 600ppm of Ta2O5, 400ppm of LiF, 800ppm of Y2O3 and 2500ppm of ZrO2 as transition metal ions at a mass concentration of 1000r / min for 10 to 30min; the mixture was first sintered at 850℃ for 15h with a heating rate of 2℃ / min and passed through a 325-mesh sieve. , mechanical crushing; then washed with water, the washing conditions are a water-to-material ratio of 1:0.5, a rotation speed of 360r / min, and a washing time of 30 minutes, put into a vacuum oven and bake at 120°C for 4h, take out and first add 2000ppm of boric acid, then add 2000ppm of alumina, mix well and then carry out a second sintering, the sintering temperature is 380°C, 10h, the heating rate is 2°C / min, after taking out, sieve and crush to obtain a high-nickel lithium-ion battery positive electrode material.
[0132] The performance of the positive electrode materials of Examples 8 to 13 was measured according to the test method of Example 1. The results are shown in Table 2.
[0133] Table 2 Performance test results of positive electrode materials
[0134] Example Capacity (mAh / g) DSC performance (℃) 8 203.6 238.6 9 202.4 244.3 10 203.2 245.2 11 202.1 240.2 12 202.4 240.7 13 202.3 238.5
[0135] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high nickel lithium ion battery positive electrode material with thermal safety, characterized in that: The chemical formula is Li 1+ x Ni a Co b Mn c M Td O2; Among them, 0.01≤x≤0.03, 0.8≤a<1, 0.03≤b≤0.1, 0.5≤c / b≤1, 0.006≤d≤0.016 and a+b+c+d=1; M T One or more selected from Al, Zr, Si, Ti, Mg, W, Mo, P, Ta, Ce, Nb, Mn, Y and F; The high nickel lithium ion battery positive electrode material is a spherical particle, and the thermally stable element M T It shows a decreasing level from the surface of the spherical particles to the inside of the spherical particles; The surface of the high-nickel lithium-ion battery positive electrode material is coated with one or more compounds of amphoteric elements, and the amphoteric elements are Al and / or B; The particles of the high-nickel lithium-ion battery positive electrode material are composed of high-nickel NCM ternary materials inside and NCMM on the surface. T For high-nickel quaternary materials, the normal plane of the particle length diameter on the surface and the normal plane of the particle length diameter inside are perpendicular to each other in three-dimensional space; The particle size distribution mode of the positive electrode material is between 0.34 and 0.60 μm.
2. The high nickel lithium ion battery positive electrode material according to claim 1, characterized in that: The material structure is loose inside, and the surface particles are arranged in a divergent manner.
3. The high nickel lithium ion battery positive electrode material according to claim 1, characterized in that: The particle compressive strength of the positive electrode material is ≥89.8Mpa; The average unit cell volume of the positive electrode material is 95.0~110.0Å 3 between.
4. A method for preparing a high nickel lithium ion battery positive electrode material with thermal safety as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: A) mixing a lithium source, a high-nickel ternary precursor and a first additive, sintering the mixture at 850° C. in an oxygen-containing gas, crushing and sieving the sintered product, washing the mixture with water and drying the mixture to obtain a washed material; Then the washed material is mixed with a second additive and sintered for a second time, and after screening, a high-nickel lithium-ion battery positive electrode material is obtained; The first additive contains one or more elements selected from Al, Zr, Si, Ti, Mg, W, Mo, P, Ta, Ce, Nb, Mn, Y and F; the second additive is selected from Al2O3 and / or B(OH)3; The water washing temperature is <40°C, and the water-to-material mass ratio is (0.5-3):1; The free lithium content in the water-washed material needs to be ≤1400 ppm.
5. The preparation method according to claim 4, characterized in that: The oxygen-containing gas is an oxygen-containing atmosphere with an oxygen content of ≥98 vol%.
6. The preparation method according to claim 4, characterized in that: The heating rate of the sintering is 2°C / min~10°C / min, and the sintering holding time is less than 20h.
7. The preparation method according to claim 4, characterized in that: The second additive is selected from one or more amphoteric compounds; The atmosphere condition of the second sintering is an oxygen-containing atmosphere, the sintering temperature is ≤600°C, the sintering time is <15h, and the sintering heating rate is 2°C / min~10°C / min.
8. The preparation method according to claim 4, characterized in that: The surface of the water-washed material is coated with amphoteric elements, and the coating amount is less than 5000 ppm.
Citation Information
Patent Citations
Core-shell polynary lithium ion battery anode material distributed in all-concentration gradient way and preparation method thereof
CN104852026A
Novel lithium-ion-battery gradient anode material and preparing method thereof
CN108269970A
Magnesium ion doped gradient nickel cobalt lithium manganate anode material and preparation method thereof
CN109686938A
Low-free-lithium aluminum oxide-coated high-nickel positive electrode material as well as preparation method and application thereof
CN109742344A
Nickel-cobalt-lithium manganate ternary cathode material and preparation method thereof
CN110474026A