Preparation method of superfine boehmite and superfine boehmite
By adding cationic additives to the hydrothermal reaction, the problem of large particle size of boehmite is solved by hydrothermal process preparation, and high-purity and fine-grained ultrafine boehmite is prepared to meet the needs of lithium battery separator materials, realizing the Efficient preparation of boehmite.
Patent Information
- Application Number
- CN202410959878.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
Boehmite prepared by existing hydrothermal processes has large particle size and is seriously agglomerated, which cannot meet the market's demand for nano-scale boehmite, and the preparation process is uneven, affecting the application of downstream products.
By mixing aluminum hydroxide with water, grinding and diluting, forming an aluminum hydroxide slurry, hydrothermal reaction is carried out under closed conditions, and cationic additives are added when the set temperature is reached to induce the formation of aluminum hydroxide crystal nuclei. High purity and fine particle size ultrafine boehmite.
The high purity and particle size distribution of boehmite have been narrowed. The prepared boehmite has a rhombic crystal structure, with a particle size of 0.1μm to 1.0μm and a purity of more than 99.9%, meeting the demand for lithium battery separators and reducing the Particle size problem in hydrothermal process preparation.
Smart Images

Figure CN118908254A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of inorganic non-metallic materials, and in particular to a preparation method of ultrafine boehmite and the ultrafine boehmite. Background Art
[0002] Boehmite is widely used in ceramic materials, composite materials, surface protection layer materials, optical materials, catalysts and carrier materials, semiconductor materials and coatings due to its unique chemical, optical and mechanical properties. In the field of electronic substrates and potting glue, boehmite can effectively improve the heat resistance and yield rate of products, and significantly improve the flame retardant properties of materials. In the field of coatings, boehmite's plate-like crystalline particles can inhibit the intrusion of water flow into products, improve air tightness, moisture resistance, water resistance, aging resistance and flame retardancy, etc.
[0003] As the country's safety standards for power and 3C batteries are improved, the coating of power battery positive plates has become an inevitable choice for ternary batteries. The expected characteristics of future lithium batteries, high energy density, safety, and stable charging and discharging, will promote the lightweight and ultra-thin lithium battery separators, and further refine the coating material particles, with particle sizes ranging from 0.7 to 1.0um to below 0.5um. Ultra-thin separators require particles below 0.5um, with regular particle morphology and narrow particle size distribution. As the process of battery lightweighting accelerates, the demand for nano-boehmite will gradually increase. Therefore, the use of new process equipment and raw materials to efficiently prepare 200-500nm boehmite has become an urgent market demand. The prior art discloses a production process for preparing boehmite powder using ordinary industrial alumina powder as raw material, wherein the industrial alumina powder is mixed with water in a certain proportion and stirred evenly, and then transferred to a reactor, the pressure in the reactor is adjusted, and the slurry is directly released under the pressure of the pressure after the pressure is maintained for 1 hour. Although the preparation method of the patent is simple, the morphology of the obtained nano powder is uneven, and there are various morphologies such as flakes, blocks and microspheres, and the blocks are adhered to each other, and the dispersion is not good, which has an adverse effect on the application of downstream products. In order to overcome the problems of large particle size, serious agglomeration and large average particle size (D50 is 0.8-1.5um) of boehmite prepared by the traditional hydrothermal process and meet market demand, it is of great practical significance to develop a simple, fast and energy-saving method to prepare boehmite with high purity and fine particle size. Summary of the invention
[0004] The present application provides a method for preparing ultrafine boehmite and ultrafine boehmite to solve the following technical problem: how to reduce the particle size of boehmite prepared by a hydrothermal process.
[0005] In a first aspect, the present application provides a method for preparing ultrafine boehmite, the method comprising:
[0006] Aluminum hydroxide is mixed with water, and then ground and diluted to obtain an aluminum hydroxide slurry with a set solid content;
[0007] Under closed conditions, the aluminum hydroxide slurry is subjected to a hydrothermal reaction. When the temperature of the hydrothermal reaction reaches a first set temperature, a cationic additive is added to the hydrothermal reaction system to continue the hydrothermal reaction to obtain a mixed solution containing ultrafine boehmite.
[0008] Optionally, the set solid content is 80g / L to 180g / L.
[0009] Optionally, in the aluminum hydroxide slurry, the particle size D50 of aluminum hydroxide is 0.4 μm to 2.0 um.
[0010] Optionally, the aluminum hydroxide slurry is subjected to a hydrothermal reaction under closed conditions, and when the temperature of the hydrothermal reaction reaches a first set temperature, a cationic additive is added to the hydrothermal reaction system to continue the hydrothermal reaction to obtain a mixed solution containing ultrafine boehmite, comprising:
[0011] Transferring the aluminum hydroxide slurry into a closed reactor;
[0012] The reactor is heated to a first set temperature, and then the cationic additive is added to the reactor through a booster pump within a set time range; the set time range is 5s to 20s;
[0013] The reactor is heated to a second set temperature to perform a hydrothermal reaction at the second set temperature for a set insulation time to obtain a mixed solution containing ultrafine boehmite.
[0014] Optionally, the first set temperature is 100° C. to 200° C.; and / or the working pressure of the boost pump is 2.0 MPa to 5.0 MPa.
[0015] Optionally, the mass of the cationic additive accounts for 0.1% to 1% of the mass of the aluminum hydroxide, and the cationic additive includes one or both of organic aluminum salts and inorganic aluminum salts.
[0016] Optionally, the organic aluminum salt includes one or more of aluminum sec-butoxide, aluminum glycinate and basic aluminum acetate, and the inorganic aluminum salt includes one or more of Al(NO3)3, Al2(SO4)3, and AlCl3.
[0017] Optionally, the second set temperature is 180°C to 240°C, and the set insulation time is 0.5h to 12h.
[0018] Optionally, the method further includes:
[0019] The mixed solution containing the ultrafine boehmite is subjected to solid-liquid separation and purification to obtain the ultrafine boehmite.
[0020] In the second aspect, the present application provides an ultrafine boehmite prepared by the method described in any one of the embodiments of the first aspect, wherein the ultrafine boehmite satisfies at least one of the following properties: a diamond shape structure, a particle size D50 of 0.1 μm to 1.0 μm, a particle size D100 of 1.330 μm to 6.324 μm, and a purity of >99.9%.
[0021] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0022] The present application provides a method for preparing ultrafine boehmite, comprising: mixing aluminum hydroxide with water, then grinding and diluting to obtain an aluminum hydroxide slurry with a set solid content; under closed conditions, subjecting the aluminum hydroxide slurry to a hydrothermal reaction, and when the temperature of the hydrothermal reaction reaches a first set temperature, adding a cationic additive to the hydrothermal reaction system to continue the hydrothermal reaction to obtain a mixed solution containing ultrafine boehmite. When the hydrothermal reaction reaches the set temperature and pressure, the addition of the cationic additive can instantly induce the generation of aluminum hydroxide nuclei in large quantities and transform it into boehmite, and the prepared boehmite has high purity, good crystal form, and narrow particle size distribution. Thereby reducing the particle size of the boehmite prepared by the hydrothermal process. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0025] Figure 1 A schematic diagram of a process for preparing ultrafine boehmite provided in an embodiment of the present application;
[0026] Figure 2 A schematic diagram of a hydrothermal reaction device provided in an embodiment of the present application;
[0027] Figure 3 This is a scanning electron microscope image of the ultrafine boehmite provided in Example 1 of the present application;
[0028] Figure 4 This is a scanning electron microscope image of the ultrafine boehmite provided in Example 2 of the present application;
[0029] Figure 5 XRD diagram of the ultrafine boehmite provided in Examples 1 and 2 of the present application;
[0030] Figure 6 This is the particle size distribution diagram of the ultrafine boehmite provided in Example 1 of the present application. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0032] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0033] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0035] Figure 1 A schematic flow chart of a method for preparing ultrafine boehmite provided in an embodiment of the present application.
[0036] See also Figure 1 The present application provides a method for preparing ultrafine boehmite, the method comprising:
[0037] S1, mixing aluminum hydroxide and water, and then grinding and diluting to obtain an aluminum hydroxide slurry with a set solid content;
[0038] In some embodiments, step S1 is specifically as follows: industrial aluminum hydroxide is mixed with water, and then sand-milled for a certain period of time to prepare an aluminum hydroxide slurry with a solid content of 200 g / L to 800 g / L; the aluminum hydroxide slurry is added with water to prepare an aluminum hydroxide slurry with a set solid content;
[0039] In some embodiments, the set solid content is 80 g / L to 180 g / L.
[0040] In the above embodiment, the solid content is controlled to be 80g / L to 180g / L, so as to ensure that the slurry can be discharged smoothly. If the solid content is lower than 80g / L, the economic cost is high. If the solid content is greater than 180g / L, the slurry will become viscous after the reaction and it will be unfavorable for discharging. For example, the solid content can be set to 80g / L, 90g / L, 100g / L, 120g / L, 140g / L, 160g / L, 180g / L, etc.
[0041] In some embodiments, in the aluminum hydroxide slurry, the particle size D50 of the aluminum hydroxide is 0.4 μm to 2.0 um.
[0042] In the above embodiment, the positive effect of the median particle size is that mechanical activation facilitates subsequent phase inversion. If the median particle size is lower than 0.4 μm, the sand milling efficiency is extremely low. If it is higher than 2 μm, the particle size of the reaction product is coarse.
[0043] S2. Under closed conditions, subjecting the aluminum hydroxide slurry to a hydrothermal reaction. When the temperature of the hydrothermal reaction reaches a first set temperature, adding a cationic additive to the hydrothermal reaction system to continue the hydrothermal reaction to obtain a mixed solution containing ultrafine boehmite.
[0044] Figure 2 Schematic diagram of the hydrothermal reaction device provided in an embodiment of the present application.
[0045] In some embodiments, see Figure 2 , the aluminum hydroxide slurry is subjected to a hydrothermal reaction under closed conditions, and when the temperature of the hydrothermal reaction reaches a first set temperature, a cationic additive is added to the hydrothermal reaction system to continue the hydrothermal reaction to obtain a mixed solution containing ultrafine boehmite, including: transferring the aluminum hydroxide slurry to a closed reactor; heating the reactor to a first set temperature, and then adding the cationic additive to the reactor through a booster pump within a set time range; the set time range is 5s to 20s; heating the reactor to a second set temperature, and performing a hydrothermal reaction at the second set temperature for a set insulation time to obtain a mixed solution containing ultrafine boehmite.
[0046] The present application can induce aluminum hydroxide to transform into boehmite in large quantities by pressing in cationic additives instantly (5s to 20s), and the prepared boehmite has high purity, good crystal form, and narrow particle size distribution. Exemplarily, the addition of cationic additives can be within a time range of 5s, a time range of 8s, a time range of 10s, a time range of 15s, a time range of 20s, etc.
[0047] In some embodiments, the first set temperature is 100° C. to 200° C.; and / or the working pressure of the boost pump is 2.0 MPa to 5.0 MPa.
[0048] In the above embodiment, when the temperature of the hydrothermal reactor is increased to 100°C to 200°C, the pressure in the reactor can reach 1 to 2MPa. At this temperature and pressure, aluminum hydroxide can be induced to transform into boehmite in large quantities by pressing in additives instantly (5s to 20s). At the same time, in order to ensure that the intermediate feeding can proceed smoothly, the pressure during the intermediate feeding must be greater than the pressure in the reactor, so the working pressure of the booster pump is controlled. Exemplarily, the first set temperature can be 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, etc., and the working pressure of the booster pump is 2.0MPa, 2.5MPa, 3.0MPa, 3.5MPa, 4.0MPa, 4.5MPa, 5.0MPa, etc.
[0049] In some embodiments, the mass of the cationic additive accounts for 0.1% to 1% of the mass of the aluminum hydroxide, and the cationic additive includes one or both of an organic aluminum salt or an inorganic aluminum salt.
[0050] In the above embodiment, the amount of cationic additive added is controlled to ensure that aluminum hydroxide can be induced to transform into boehmite in large quantities. If the cation concentration introduced is too low, it will not have an inductive effect, and if it is too high, impurities will be introduced to affect product quality. Exemplarily, the mass of the cationic additive in the mass of the aluminum hydroxide can account for 0.1%, 0.2%, 0.3%, 0.4%, 0.6%, 0.8%, 1%, etc.
[0051] In some embodiments, the organic aluminum salt includes one or more of aluminum sec-butoxide, aluminum glycinate, and basic aluminum acetate, and the inorganic aluminum salt includes one or more of Al(NO3)3, Al2(SO4)3, and AlCl3.
[0052] In some embodiments, the second set temperature is 180° C. to 240° C., and the set insulation time is 0.5 h to 12 h.
[0053] In the above embodiment, it should be noted that the second set temperature is equivalent to the heating temperature of the hydrothermal reaction, and the set insulation time is equivalent to the insulation time of the hydrothermal reaction. The positive effect of this temperature and time is that the temperature is too low and the time is too short, the phase transition is incomplete, and the temperature is too high and the time is too long, the economic cost is high. Exemplarily, the second set temperature can be 180°C, 190°C, 200°C, 210°C, 230°C, 240°C, etc., and the set insulation time can be 0.5h, 1h, 3h, 4h, 6h, 8h, 10h, 12h, etc.
[0054] In some embodiments, the method further comprises: S3, performing solid-liquid separation and purification on the mixed solution containing ultrafine boehmite to obtain ultrafine boehmite.
[0055] In the above embodiment, purification includes washing and drying.
[0056] In some embodiments, the water is deionized water.
[0057] Based on a general inventive concept, the present application also provides an ultrafine boehmite prepared by the method described in any one of the above embodiments, wherein the ultrafine boehmite satisfies at least one of the following properties: a diamond shape structure, a particle size D50 of 0.1 μm to 1.0 μm, a particle size D100 of 1.330 μm to 6.324 μm, and a purity of >99.9%.
[0058] The boehmite prepared in the present application can be used as a lithium battery diaphragm material. Compared with the existing boehmite powder preparation technology, new equipment and technology are used. By instantly (5s to 20s) pressing in additives, a large amount of aluminum hydroxide can be induced to transform into boehmite. The prepared boehmite has high purity, good crystal shape, and narrow particle size distribution.
[0059] The ultrafine boehmite is realized based on the preparation method of the ultrafine boehmite mentioned above. The specific steps of the preparation method of the ultrafine boehmite can refer to the above embodiment. Since the ultrafine boehmite adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be repeated here one by one.
[0060] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0061] Example 1
[0062] This embodiment provides a method for preparing ultrafine boehmite, comprising the following steps:
[0063] (1) 450 g of aluminum hydroxide was mixed with 1000 ml of high-purity water, and the mixture was sand-milled into a slurry. Ultrapure water was added to the sand-milled slurry to prepare a 3 L aluminum hydroxide slurry with a solid content of 150 g / L;
[0064] (2) transferring the aluminum hydroxide slurry obtained in step (1) into a stainless steel hydrothermal reactor and heating it at a set temperature of 200° C.;
[0065] (3) When the temperature of the reactor in step (2) is raised to 130° C., 20 ml (10% wt) of Al(NO 3 ) 3 solution is added to the reaction system in the reactor;
[0066] (4) The reactor in step (3) was further heated to 200° C. and kept at this temperature for 2 h;
[0067] (5) Cool the reactants to below 60° C., separate the materials, and dry them to obtain boehmite.
[0068] Example 2
[0069] This embodiment provides a method for preparing ultrafine boehmite, comprising the following steps:
[0070] (1) 240 g of aluminum hydroxide was mixed with 1000 ml of high-purity water, and the mixture was sand-milled into a slurry. Ultrapure water was added to the sand-milled slurry to prepare a 3 L aluminum hydroxide slurry with a solid content of 80 g / L;
[0071] (2) transferring the aluminum hydroxide slurry obtained in step (1) to a stainless steel hydrothermal reactor and heating it at a set temperature of 240° C.;
[0072] (3) When the temperature of the reaction kettle in step (2) is raised to 170° C., 25 ml (10% wt) of aluminum sec-butoxide solution is added to the reaction system in the reaction kettle;
[0073] (4) The reactor in step (3) was further heated to 240° C. and kept warm for 1.5 h;
[0074] (5) Cool the reactants to below 60° C., separate the materials, and dry them to obtain boehmite.
[0075] Example 3
[0076] This embodiment provides a method for preparing ultrafine boehmite, comprising the following steps:
[0077] (1) 360 g of aluminum hydroxide was mixed with 1000 ml of high-purity water, and the mixture was sand-milled into a slurry. Ultrapure water was added to the sand-milled slurry to prepare a 3 L aluminum hydroxide slurry with a solid content of 120 g / L;
[0078] (2) transferring the aluminum hydroxide slurry obtained in step (1) into a stainless steel hydrothermal reactor and heating it at a set temperature of 220° C.;
[0079] (3) When the temperature of the reactor in step (2) is raised to 160° C., 30 ml (10% wt) of aluminum glycinate solution is added to the reaction system in the reactor;
[0080] (4) The reactor in step (3) was further heated to 220° C. and kept warm for 1.8 h;
[0081] (5) Cool the reactants to below 60° C., separate the materials, and dry them to obtain boehmite.
[0082] Example 4
[0083] This embodiment provides a method for preparing ultrafine boehmite, comprising the following steps:
[0084] (1) 600 g of aluminum hydroxide was mixed with 1000 ml of high-purity water, and the mixture was sand-milled into a slurry. Ultrapure water was added to the sand-milled slurry to prepare a 3 L aluminum hydroxide slurry with a solid content of 180 g / L;
[0085] (2) transferring the aluminum hydroxide slurry obtained in step (1) into a stainless steel hydrothermal reactor and heating it at a set temperature of 220° C.;
[0086] (3) When the temperature of the reaction kettle in step (2) is raised to 190° C., 50 ml (10% wt) of basic aluminum acetate solution is added to the reaction system in the reaction kettle;
[0087] (4) The reactor in step (3) was further heated to 220° C. and kept warm for 1.8 h;
[0088] (5) Cool the reactants to below 60° C., separate the materials, and dry them to obtain boehmite.
[0089] Example 5
[0090] This embodiment provides a method for preparing ultrafine boehmite, comprising the following steps:
[0091] (1) 600 g of aluminum hydroxide was mixed with 1000 ml of high-purity water, and the mixture was sand-milled into a slurry. Ultrapure water was added to the sand-milled slurry to prepare 3 L of slurry aluminum hydroxide with a solid content of 180 g / L;
[0092] (2) transferring the aluminum hydroxide slurry obtained in step (1) into a stainless steel hydrothermal reactor and heating it at a set temperature of 220° C.;
[0093] (3) When the temperature of the reaction kettle in step (2) is raised to 190° C., 50 ml (8% wt) of basic aluminum acetate + (4% wt) Al(NO 3 ) 3 mixed solution is added to the reaction system in the reaction kettle;
[0094] (4) The reactor in step (3) was further heated to 220° C. and kept warm for 1.8 h;
[0095] (5) Cool the reactants to below 60° C., separate the materials, and dry them to obtain boehmite.
[0096] Comparative Example 1
[0097] This comparative example provides a method for preparing ultrafine boehmite, comprising the following steps:
[0098] (1) 450 g of aluminum hydroxide was mixed with 1000 ml of high-purity water, and the mixture was sand-milled into a slurry. Ultrapure water was added to the sand-milled slurry to prepare a 3 L slurry of aluminum hydroxide with a solid content of 150 g / L;
[0099] (2) The aluminum hydroxide slurry obtained in step (1) was transferred to a stainless steel hydrothermal reactor, heated at 200° C., and kept warm for 2 h;
[0100] (3) Cooling the reactants to below 60° C., separating the materials, and drying them to obtain boehmite.
[0101] Comparative Example 2
[0102] This comparative example provides a method for preparing ultrafine boehmite, comprising the following steps:
[0103] (1) 240 g of aluminum hydroxide was mixed with 1000 ml of high-purity water, and the mixture was sand-milled into a slurry. Ultrapure water was added to the sand-milled slurry to prepare a 3 L aluminum hydroxide slurry with a solid content of 80 g / L;
[0104] (2) The aluminum hydroxide slurry obtained in step (1) was transferred to a stainless steel hydrothermal reactor, heated at 240° C., and kept warm for 1.5 h;
[0105] (3) Cooling the reactants to below 60° C., separating the materials, and drying them to obtain boehmite.
[0106] The particle size of aluminum hydroxide in the aluminum hydroxide slurry of the embodiment and the comparative example was measured, and the particle size and purity of the boehmite obtained in the embodiment and the comparative example were measured. The results are shown in Table 1.
[0107] Table 1 Aluminum hydroxide particle size in aluminum hydroxide slurry and boehmite particle size and purity
[0108]
[0109]
[0110] Figure 3 This is a scanning electron microscope image of the ultrafine boehmite provided in Example 1 of the present application; Figure 4 This is a scanning electron microscope image of the ultrafine boehmite provided in Example 2 of the present application. Figure 3 and Figure 4 It can be seen that the prepared boehmite has good rhombus crystallization, uniform particle size distribution and good dispersibility.
[0111] Figure 5 The XRD diagram of the ultrafine boehmite provided in Examples 1 and 2 of the present application. Figure 5It can be seen that the diffraction peaks in the XRD graph are all specific diffraction peaks of boehmite, without diffraction peaks of impurities, and the surface reaction product is pure phase boehmite.
[0112] Figure 6 This is the particle size distribution diagram of the ultrafine boehmite provided in Example 1 of the present application. It should be noted that: Figure 6 The horizontal axis is marked as particle size μm, and the vertical axis is marked as cumulative %. Figure 6 It can be seen that the prepared boehmite has a narrow particle size distribution and no agglomeration.
[0113] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0114] (1) In the embodiments of the present invention, the prepared boehmite has good uniformity and narrow particle size distribution, does not require high-speed pulverizer or air flow mill for deagglomeration, and has a complete morphology.
[0115] (2) In the embodiment of the present invention, the prepared boehmite has a narrow particle size distribution D50 of 0.1 μm to 1.0 μm, D100 of 1.330 μm to 6.324 μm, high purity and good crystal form.
[0116] (3) In the embodiment of the present invention, the prepared near-nano boehmite has low cost and cheap raw materials, and can be used in the field of lithium battery separator film coating.
[0117] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing ultrafine boehmite, characterized in that: The method comprises: Aluminum hydroxide is mixed with water, and then ground and diluted to obtain an aluminum hydroxide slurry with a set solid content; Under closed conditions, the aluminum hydroxide slurry is subjected to a hydrothermal reaction. When the temperature of the hydrothermal reaction reaches a first set temperature, a cationic additive is added to the hydrothermal reaction system to continue the hydrothermal reaction to obtain a mixed solution containing ultrafine boehmite.
2. The method according to claim 1, characterized in that The set solid content is 80g / L to 180g / L.
3. The method according to claim 1, characterized in that In the aluminum hydroxide slurry, the particle size D50 of aluminum hydroxide is 0.4 μm to 2.0 μm.
4. The method according to claim 1, characterized in that: The aluminum hydroxide slurry is subjected to a hydrothermal reaction under a closed condition, and when the temperature of the hydrothermal reaction reaches a first set temperature, a cationic additive is added to the hydrothermal reaction system to continue the hydrothermal reaction to obtain a mixed solution containing ultrafine boehmite, comprising: Transferring the aluminum hydroxide slurry into a closed reactor; The reactor is heated to a first set temperature, and then the cationic additive is added to the reactor through a booster pump within a set time range; the set time range is 5s to 20s; The reactor is heated to a second set temperature to perform a hydrothermal reaction at the second set temperature for a set insulation time to obtain a mixed solution containing ultrafine boehmite.
5. The method according to claim 4, characterized in that The first set temperature is 100° C. to 200° C.; and / or the working pressure of the booster pump is 2.0 MPa to 5.0 MPa.
6. The method according to claim 4, characterized in that The mass of the cationic additive accounts for 0.1% to 1% of the mass of the aluminum hydroxide, and the cationic additive includes one or both of an organic aluminum salt or an inorganic aluminum salt.
7. The method according to claim 6, characterized in that The organic aluminum salt includes one or more of aluminum sec-butoxide, aluminum glycinate and basic aluminum acetate, and the inorganic aluminum salt includes one or more of Al(NO3)3, Al2(SO4)3 and AlCl3.
8. The method according to claim 4, characterized in that The second set temperature is 180° C. to 240° C., and the set insulation time is 0.5 h to 12 h.
9. The method according to claim 1, characterized in that: The method further comprises: The mixed solution containing the ultrafine boehmite is subjected to solid-liquid separation and purification to obtain the ultrafine boehmite.
10. An ultrafine boehmite prepared by the method according to any one of claims 1 to 9, characterized in that: The ultrafine boehmite meets at least one of the following properties: a rhombus-shaped structure, a particle size D50 of 0.1 μm to 1.0 μm, a particle size D100 of 1.330 μm to 6.324 μm, and a purity of more than 99.9%.
Citation Information
Cited By
Preparation method of boehmite
CN120793981A