WS2 / graphene electrode material and preparation method and application thereof
By preparing WS2/graphene electrode materials, the problems of insufficient conductivity and selectivity of existing carbon-based electrodes and Faraday electrodes in capacitive deionization technology have been solved, achieving efficient and environmentally friendly heavy metal ion removal.
Patent Information
- Application Number
- CN202411262420.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-10
AI Technical Summary
Existing carbon-based electrode materials exhibit weak conductivity, weak capacitive adsorption capacity, and low selectivity in capacitive deionization technology. Faraday electrode materials are unstable in solution, resulting in low removal efficiency and poor regeneration performance of heavy metal ions.
The preparation method of WS2/graphene electrode material adopts the hydrothermal reaction of sodium tungstate, thiourea and graphene to form WS2/graphene composite material. The layered structure of WS2 and the high conductivity of graphene are used to improve the capacitive adsorption performance of the electrode, and selective adsorption of heavy metal ions is achieved through S2-soft Lewis base sites.
It significantly improves the selective adsorption effect of electrode materials on heavy metal ions, with a removal rate of over 99%. Moreover, the preparation method is simple and low-cost, and it has good cycle stability and environmental friendliness.
Smart Images

Figure CN118908357A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrode materials and heavy metal wastewater treatment, and specifically relates to a WS2 / graphene electrode material and a preparation method and application thereof. Background Art
[0002] With the rapid development of industry and the surge in industrial manufacturing enterprises, the problem of heavy metal industrial wastewater discharge has become increasingly prominent, seriously polluting water resources and posing a direct threat to public health. Copper, lead, zinc, cadmium, mercury, chromium, etc. are the most common and toxic heavy metal pollutants in wastewater. They have been listed as chemical pollutants of public concern by the World Health Organization. They can exist stably in the water environment and are not easily degraded naturally. Heavy metal pollutants enter the ecological water system and accumulate and amplify through the food chain, causing acute or chronic toxic effects on aquatic organisms and humans, and even death in the most dangerous cases. Therefore, efficient removal of heavy metal elements in wastewater is of great significance to the sustainable and healthy development of the heavy metal industry and environmental protection.
[0003] In recent years, domestic and foreign researchers have explored and optimized a variety of heavy metal ion removal methods, including adsorption, chemical precipitation, ion exchange and membrane separation technology, for the removal of various heavy metal pollutants. Although the above methods have shown certain heavy metal removal efficiency, their respective limitations cannot be ignored. The chemical precipitation method achieves the removal of heavy metals by forming insoluble precipitates, but the large amount of sludge produced in the process is prone to secondary environmental pollution; the ion exchange method uses exchange agents to capture heavy metals, but the oxidation sensitivity of the exchange agents limits their stability and life, and the frequent regeneration requirements significantly increase the operating cost and running cost; the membrane separation method is based on the separation characteristics of membrane materials and can effectively intercept heavy metal ions in water bodies. However, the membrane is easily blocked by pollutants or other impurities in the wastewater, resulting in decreased membrane performance and shortened service life, which in turn affects the effluent water quality; the adsorption method uses the high specific surface area or special functional groups of the material to adsorb heavy metals, but the difficulty of recycling and regeneration of the adsorbent and the limited efficiency limit its widespread promotion in practical applications. Therefore, the development of a technology that can efficiently, environmentally friendly, low-cost and selectively remove heavy metal ions from water is of great significance to the sustainable development of the environment.
[0004] Capacitive deionization technology is a new type of electrochemical water treatment technology that is environmentally friendly, pollution-free, low in energy consumption, and has great development potential. It has attracted more and more attention from researchers in recent years. The electrochemical method uses the redox reaction on the electrode surface to reduce heavy metal ions in water to a more stable and less toxic form, or directly reduce metal ions to metal elements on the electrode surface to achieve efficient removal of metal ions in the aqueous phase. Therefore, electrochemical methods are a more effective way to remove ions in the solution. The principle of capacitive deionization technology is similar to the mechanism of double-layer capacitance. By applying a certain voltage between the two electrodes to establish an electric field, the anions and cations in the solution move to the corresponding electrodes under the action of the electric field force, and finally adsorb on the surface of the electrode or precipitate on the surface of the electrode, thereby reducing the ion concentration in the solution. When the ions on the electrode surface reach saturation, the two electrodes are connected in reverse, and the ions adsorbed on the electrodes are released into the solution due to the loss of the electric field, so that the ions in the solution are enriched again and the electrodes are regenerated. The electrode is an important component of the capacitive deionization system and is the key to determining the effect of capacitive deionization. Commonly used electrodes are carbon-based electrodes. Carbon-based electrode materials, such as activated carbon, have rich pore structures and good adsorption properties. They mainly capture charged ions through the Coulomb force at the double-layer interface. However, most carbon-based materials have reached a development bottleneck due to their weak conductivity, weak capacitive adsorption capacity, and low selectivity. The development of new electrode materials has become a development need. For example, patent CN 114988537 A discloses a composite electrode that uses nZVI and Fe3O4 to be composited and then loaded on ACF. It is used in capacitive deionization technology to remove heavy metals from water and can effectively adsorb and remove heavy metal ions. Patent CN 117427610 A discloses a nickel-manganese-carbon ternary composite material and its preparation method, electrode, and capacitive deionization treatment method for heavy metal wastewater. It mainly verifies that the electrode has good adsorption performance for Cd 2+ , Pb 2+ and Zn 2+ The removal effect of the three ions at a voltage of 1.5V is 95.56%, 97.83% and 94.54% respectively. Patent CN116395650 A discloses a FeP-doped polytriazine carbon material and its preparation method and application in selective capacitive deionization electrode. The electrode material prepared by FeP-doped polytriazine carbon material can separate Cu with high content in wastewater with low consumption and high efficiency. 2+ Patent CN 115536112A discloses a capacitor electrode for selectively removing heavy metal lead ions from drinking water by electrosorption. The electrode achieves selective removal of lead ions and has high adsorption capacity and good stability.
[0005] The addition of Faraday materials can provide the Faraday effect to increase the capacitive deionization capacity of the electrode. However, some Faraday electrodes are limited by the conductivity and specific surface area of the material itself and are unstable in the solution, resulting in poor regeneration performance and low removal efficiency. In addition, due to the lack of affinity sites for the target ions, its selective recovery performance for metal ions is severely limited. Therefore, how to construct a highly selective, recyclable and stable Faraday electrode is the key to capacitive enrichment and extraction of heavy metal ions.
[0006] WS2 has a typical layered structure similar to graphite. The structure of WS2 is a sandwich-like layered structure, in which the inner layer (SWS) is strongly covalently bonded, and the interlayer is weaker van der Waals force, and the layers are easily peeled off. With WS2 as the main material, through insertion reaction, guest atoms or molecules can be inserted between the main layers to form intercalation compounds. Since the layers of WS2 layered compounds are bound by weak van der Waals forces, it is possible to introduce foreign ions, atoms or molecules between the layers. The above characteristics have made WS2 widely studied for its application in electrochemical lithium storage electrode materials. For example, patents CN 102694172A and CN 104091947 A both disclose a WS2 and graphene composite nanomaterial, but the preparation method is to use ammonium thiotungstate and graphene oxide to simultaneously reduce WS2 and graphene, respectively, and then prepare them by high-temperature heat treatment in a nitrogen / hydrogen mixed atmosphere. The preparation method is relatively complicated, and it is mainly used for electrocatalysis of hydrogen evolution reaction and enhancing electrochemical lithium storage performance. It is not disclosed that it has the performance of selective capacitive adsorption to remove heavy metal ions. Summary of the invention
[0007] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide a method for preparing WS2 / graphene electrode material.
[0008] Another object of the present invention is to provide a WS2 / graphene electrode material prepared by the above method.
[0009] Another object of the present invention is to provide the application of the above-mentioned WS2 / graphene electrode material in capacitive adsorption and removal of heavy metal ions.
[0010] The purpose of the present invention is achieved through the following technical solutions:
[0011] A method for preparing a WS2 / graphene electrode material comprises the following preparation steps:
[0012] (1) dispersing sodium tungstate, thiourea and hydroxylamine hydrochloride uniformly in deionized water, adjusting the pH, adding graphene and a surfactant and mixing uniformly to obtain a mixed solution;
[0013] (2) transferring the mixed solution of step (1) into a pressure-resistant reactor and sealing it for hydrothermal reaction;
[0014] (3) The reaction product obtained in step (2) is separated, washed and dried to obtain WS2 / graphene electrode material.
[0015] Furthermore, in step (1), the molar ratio of sodium tungstate, thiourea and hydroxylamine hydrochloride is 0.5-0.6:2:1.
[0016] The above preparation method involves the following reaction:
[0017] Na2WO4+4CH4N2S+4H2O——4CO2+Na2WS4+8NH3,
[0018] Na2WS4+2NH2OH·HCl——WS2+N2+2H2O+2H2S+2NaCl.
[0019] Furthermore, the amount of deionized water added in step (1) is 5 to 10 times the total mass of sodium tungstate, thiourea and hydroxylamine hydrochloride.
[0020] Furthermore, the amount of graphene added in step (1) is 0.1% to 1% of the mass of sodium tungstate.
[0021] Furthermore, the surfactant in step (1) is CTAB (cetyltrimethylammonium bromide), and the amount of CTAB added is 0.5% to 2% (based on the mass percentage in the mixed solution).
[0022] Furthermore, the pH adjustment in step (1) refers to adjusting the pH value to 5-7 with hydrochloric acid or ammonia water.
[0023] Furthermore, the pressure-resistant reactor in step (2) is a polytetrafluoroethylene-lined stainless steel autoclave.
[0024] Furthermore, the reaction temperature of the hydrothermal reaction in step (2) is 160-200° C., and the reaction time is 12-48 hours.
[0025] Furthermore, in step (3), the separation refers to filtering and separating the solid phase product; the washing refers to washing with deionized water and anhydrous ethanol; and the drying refers to drying at a temperature of 50 to 70° C. for 8 to 12 hours.
[0026] A WS2 / graphene electrode material is prepared by the above method.
[0027] Preferably, the WS2 / graphene electrode material is composed of flat and smooth nanosheets, wherein the mass ratio of tungsten, sulfur and carbon is 1-20:1-10:1-90.
[0028] The application of the above-mentioned WS2 / graphene electrode material in the removal of heavy metal ions by capacitive adsorption.
[0029] Furthermore, the application method is: using the WS2 / graphene electrode material as the negative electrode of the capacitive deionization device, and the activated carbon material as the positive electrode, and then removing heavy metal ions through capacitive adsorption.
[0030] Preferably, the voltage adsorbed by the capacitor is 0.1-5V.
[0031] Preferably, the heavy metal ions include at least one of Cr, Cd, Pb, Ni, Co, and Cu heavy metal ions.
[0032] The principle of the invention is that WS2 is a lamellar hollow sphere with a hexagonal crystal system, which has a unique SWS layered structure that can promote the insertion of ions into the interlayer space. In the WS2 layered structure, two layers of sulfur atoms are sandwiched between metal atoms, making more soft Lewis base sites S 2- The group is exposed on the surface. 2- Soft Lewis base sites have a high affinity for soft Lewis acid heavy metal ions and can be used for the selective removal of heavy metal ions. In addition, the central W atom of WS2 exhibits good pseudocapacitive properties due to its rich oxidation valence states (from +2 to +6). However, the lower electronic / ionic conductivity between adjacent SWSs leads to poor conductivity of WS2, resulting in low capacitive adsorption performance. Graphene is a two-dimensional material with a large specific surface area, good hydrophilicity and good conductivity. The combination of graphene and WS2 can not only improve the conductivity of the electrode material, but also facilitate the entry of the electrolyte and the rapid transfer of ions, thereby improving the removal rate of heavy metal ions by capacitive adsorption.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The present invention obtains pseudocapacitor-sulfur site interface material WS2 / graphene by hydrothermal reaction of sodium tungstate, thiourea and graphene, which has binding sites with affinity for heavy metal ions and can significantly improve the selective adsorption effect of electrode materials on heavy metal ions. The obtained WS2 / graphene electrode material has a high adsorption capacity for Cr at a voltage of 1.2V. 3+ 、Cd 2+ , Pb 2+ 、Ni 2 + 、Co 2+ , Cu 2+ The selective recovery efficiency of heavy metal ions can reach over 99%.
[0035] (2) The preparation method of the WS2 / graphene electrode material of the present invention is simple, the reaction conditions are mild, and the cost is low; the obtained product has good morphology and high activity.
[0036] (3) Compared with conventional adsorption, chemical precipitation, ion exchange and membrane separation methods, the application method of the present invention in heavy metal removal has the advantages of high energy efficiency, environmental friendliness and no pollution, and has better cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a scanning electron microscope image of the WS2 / graphene electrode material prepared in Example 1;
[0038] Figure 2 This is a transmission electron microscopy image of the WS2 / graphene electrode material prepared in Example 1;
[0039] Figure 3 XPS and element content distribution diagram of the WS2 / graphene electrode material prepared in Example 1;
[0040] Figure 4 This is a diagram showing the removal efficiency of heavy metal ions by the WS2 / graphene electrode material prepared in Example 1;
[0041] Figure 5 This is a diagram showing the removal efficiency of heavy metal ions by the WS2 / graphene electrode material prepared in Example 1 at different cycle times;
[0042] Figure 6 This is a scanning electron microscope image of the WS2 pseudocapacitive interface material prepared in Comparative Example 1;
[0043] Figure 7 This is a diagram showing the removal efficiency of heavy metal ions by the WS2 pseudocapacitive interface material prepared in Comparative Example 1. DETAILED DESCRIPTION
[0044] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0045] Example 1
[0046] A method for preparing a WS2 / graphene electrode material in this embodiment, the specific preparation steps are as follows:
[0047] (1) 1.6493 g of sodium tungstate, 1.5224 g of thiourea and 0.6949 g of hydroxylamine hydrochloride were uniformly dispersed in 30 mL of deionized water, 2 mol / L hydrochloric acid or ammonia water was added dropwise under magnetic stirring to adjust the pH to 6.0, and 10 mg of graphene and 0.24 g of surfactant CTAB were added and mixed to obtain a mixed solution.
[0048] (2) The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and subjected to a hydrothermal reaction in a digital constant temperature oven at a temperature of 180° C. for 24 h.
[0049] (3) The solid phase product was separated by suction filtration, washed with deionized water and anhydrous ethanol for multiple times, and dried at 60° C. for 10 h to obtain the WS2 / graphene electrode material of this embodiment.
[0050] The scanning electron microscope images and transmission electron microscope images of the WS2 / graphene electrode material obtained in this example are shown in Figure 2. Figure 1 and Figure 2 As shown, the element distribution diagram of WS2 / graphene electrode material is as follows Figure 3 It can be seen that the WS2 / graphene electrode material obtained by the present invention is composed of flat and smooth nanosheets, wherein the mass ratio of tungsten, sulfur and carbon is 16.45:1.34:82.21.
[0051] The application of the WS2 / graphene electrode material obtained in this embodiment in heavy metal removal is as follows:
[0052] The obtained WS2 / graphene electrode material was used as the negative electrode of the capacitive deionization device, and the activated carbon was used as the positive electrode of the capacitive deionization device. The capacitive adsorption of heavy metal solutions (containing Cr, Cr2+, Cr3+, Cr4+, Cr6+, Cr7+, Cr8+, Cr8+, Cr9+, Cr10+, Cr11+, Cr12+, Cr13+, Cr14+, Cr15+, Cr16+, Cr17+, Cr18+, Cr19+, Cr22+, Cr19+, Cr18+, Cr19+, Cr1 ... 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ ) in the heavy metal ions. The solution adsorbed by the capacitor was tested by ICP-OES to calculate the removal rate of heavy metal ions. The test results are as follows Figure 4 As shown. Figure 4 The results show that the WS2 / graphene electrode material obtained in this example has a good stability to Cr with a solubility of 10 ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions is 99.34%, 99.84%, 99.02%, 99.02%, 99.32% and 99.30% respectively, and the solubility of Cr is 30ppm. 3+ 、Cd 2 + , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+The removal efficiency of heavy metal ions is 98.91%, 98.14%, 98.88%, 95.68%, 97.70% and 98.02% respectively, and the solubility of Cr is 50ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions was 96.10%, 93.71%, 96.35%, 94.97%, 96.32% and 97.86% respectively, and the solubility of Cr was 70ppm. 3+ 、Cd 2+ , Pb 2 + 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions is 93.99%, 92.36%, 95.14%, 91.80%, 95.26% and 96.29% respectively. The solubility of Cr is 90ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiencies of heavy metal ions were 90.64%, 90.38%, 89.89%, 90.03%, 93.51% and 93.57% respectively.
[0053] At the same time, the obtained WS2 / graphene electrode material was used as the negative electrode of the capacitive deionization device, and the activated carbon was used as the positive electrode of the capacitive deionization device. The multi-component mixed solution containing six heavy metal ions (10 mg / L for each heavy metal) and NaCl (100 mg / L) was capacitively adsorbed under a voltage of 1.2 V. The capacitively adsorbed solution at different cycle times was tested by ICP-OES to calculate the heavy metal ion removal rate. The test results are shown in Figure 5 As shown. Figure 5 The results show that the WS2 / graphene electrode material obtained in this example has a good stability to Cr with a solubility of 10 ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ Heavy metal ions have high and stable selective removal efficiency.
[0054] Example 2
[0055] A method for preparing a WS2 / graphene electrode material in this embodiment, the specific preparation steps are as follows:
[0056] (1) 1.6493 g of sodium tungstate, 1.5224 g of thiourea and 0.6949 g of hydroxylamine hydrochloride were uniformly dispersed in 35 mL of deionized water, 2 mol / L hydrochloric acid or ammonia water was added dropwise under magnetic stirring to adjust the pH to 5.0, and 1.65 mg of graphene and 0.18 g of surfactant CTAB were added and mixed to obtain a mixed solution.
[0057] (2) The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and subjected to a hydrothermal reaction in a digital constant temperature oven at a temperature of 160° C. for 48 h.
[0058] (3) The obtained solid phase product was separated by suction filtration, washed with deionized water and anhydrous ethanol for multiple times, and dried at 50° C. for 12 h to obtain the WS2 / graphene electrode material of this embodiment.
[0059] The application of the WS2 / graphene electrode material obtained in this example in the removal of heavy metals (the specific application method is the same as in Example 1) shows that the Cr with a solubility of 10 ppm 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions is 98.23%, 97.88%, 97.37%, 97.47%, 97.13% and 98.49% respectively, and the solubility of Cr is 30ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions was 95.48%, 93.26%, 94.13%, 92.97%, 94.14% and 96.81% respectively, and the solubility of Cr was 50ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions was 92.89%, 89.10%, 90.35%, 90.99%, 91.04% and 94.44% respectively, and the solubility of Cr was 70ppm. 3+ 、Cd 2+ , Pb 2 + 、Ni 2+ 、Co 2+ , Cu 2+The removal efficiencies of heavy metal ions were 90.03%, 84.43%, 86.21%, 85.85%, 82.77% and 91.33% respectively, and the solubility of Cr was 90ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiencies of heavy metal ions were 86.37%, 79.20%, 81.56%, 82.66%, 83.20% and 84.66% respectively.
[0060] Example 3
[0061] A method for preparing a WS2 / graphene electrode material in this embodiment, the specific preparation steps are as follows:
[0062] (1) 1.6493 g of sodium tungstate, 1.5224 g of thiourea and 0.6949 g of hydroxylamine hydrochloride were uniformly dispersed in 20 mL of deionized water, 2 mol / L hydrochloric acid or ammonia water was added dropwise under magnetic stirring to adjust the pH to 7.0, and 16.5 mg of graphene and 0.40 g of surfactant CTAB were added and mixed to obtain a mixed solution.
[0063] (2) The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and subjected to a hydrothermal reaction in a digital constant temperature oven at a temperature of 200° C. for 12 h.
[0064] (3) The obtained solid phase product was separated by suction filtration, washed with deionized water and anhydrous ethanol for multiple times, and dried at 70° C. for 8 h to obtain the WS2 / graphene electrode material of this embodiment.
[0065] The application of the WS2 / graphene electrode material obtained in this example in the removal of heavy metals (the specific application method is the same as in Example 1) shows that the Cr with a solubility of 10 ppm 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions is 99.20%, 99.65%, 99.77%, 99.00%, 99.40%, 99.44% respectively, and the solubility of Cr is 30ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+The removal efficiency of heavy metal ions is 99.37%, 99.00%, 98.50%, 97.21%, 97.32% and 98.73% respectively, and the solubility of Cr is 50ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions was 97.23%, 95.17%, 96.48%, 96.06%, 97.46% and 98.44% respectively, and the solubility of Cr was 70ppm. 3+ 、Cd 2+ , Pb 2 + 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions is 95.63%, 93.68%, 96.35%, 94.72%, 95.69% and 96.53% respectively. The solubility of Cr is 90ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiencies of heavy metal ions were 92.26%, 91.15%, 90.66%, 92.85%, 93.38% and 94.53% respectively.
[0066] Comparative Example 1
[0067] In this comparative example, a preparation method based on WS2 pseudocapacitive interface material is described. Compared with Example 1, graphene is not added during the preparation process. The specific preparation steps are as follows:
[0068] (1) 1.6493 g of sodium tungstate, 1.5224 g of thiourea, 0.6949 g of hydroxylamine hydrochloride and 0.24 g of surfactant CTAB were dispersed in 30 mL of deionized water, and the pH was adjusted to 6.0 by dropping 2 mol / L hydrochloric acid or ammonia water under magnetic stirring to obtain a mixed solution.
[0069] (2) The mixed solution was transferred into a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and reacted at 180 °C in a digital constant temperature oven for 24 h.
[0070] (3) The obtained solid phase product was separated by suction filtration, washed with deionized water and anhydrous ethanol for multiple times, and then placed in an oven for drying at 60° C. for 10 h to obtain the pseudocapacitive interface material (WS2) of this comparative example.
[0071] The scanning electron microscope image of the WS2 pseudocapacitor interface material obtained in this comparative example is as follows: Figure 6 It can be seen that the pseudocapacitor interface material WS2 obtained in this comparative example is composed of irregular blocks, which is quite different from the morphology of the pseudocapacitor-sulfur site interface material WS2 / graphene.
[0072] The WS2 pseudocapacitive interface material obtained in this comparative example is used in heavy metal removal, and the specific application method is the same as in Example 1. The solution adsorbed by the capacitor is tested by ICP-OES, and the test results are as follows: Figure 7 As shown. Figure 7 The results show that the WS2 pseudocapacitive interface material obtained in this comparative example has a high affinity to Cr with a solubility of 10 ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions was 94.45%, 94.92%, 90.98%, 93.67%, 89.69% and 93.61% respectively, and the solubility of Cr was 30ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiency of heavy metal ions was 92.72%, 84.48%, 88.22%, 87.91%, 89.31% and 92.85% respectively, and the solubility of Cr was 50ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiencies of heavy metal ions were 85.52%, 78.64%, 82.60%, 79.45%, 87.57% and 92.26% respectively, and the solubility of Cr was 70ppm. 3+ 、Cd 2+ , Pb 2 + 、Ni 2+ 、Co 2+ , Cu 2+ The removal efficiencies of heavy metal ions were 84.20%, 67.38%, 75.67%, 74.74%, 72.61% and 86.71% respectively, and the solubility of Cr was 90ppm. 3+ 、Cd 2+ , Pb 2+ 、Ni 2+ 、Co 2+ , Cu 2+The removal efficiencies of heavy metal ions were 82.79%, 59.76%, 71.53%, 71.89%, 69.08% and 72.10% respectively.
[0073] By comparing the results of this comparative example with Examples 1 to 3, it can be seen that the present invention can further improve the removal rate of heavy metal ions by the electrode material by compounding with graphene to increase the specific surface area and conductivity of the material.
[0074] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a WS2 / graphene electrode material, characterized in that: The method comprises the following preparation steps: (1) dispersing sodium tungstate, thiourea and hydroxylamine hydrochloride uniformly in deionized water, adjusting the pH, adding graphene and a surfactant and mixing uniformly to obtain a mixed solution; (2) transferring the mixed solution of step (1) into a pressure-resistant reactor and sealing it for hydrothermal reaction; (3) The reaction product obtained in step (2) is separated, washed and dried to obtain WS2 / graphene electrode material.
2. The method for preparing a WS2 / graphene electrode material according to claim 1, characterized in that: The molar ratio of sodium tungstate, thiourea and hydroxylamine hydrochloride in step (1) is 0.5-0.6:2:
1.
3. The method for preparing a WS2 / graphene electrode material according to claim 2, characterized in that: The amount of deionized water added in step (1) is 5 to 10 times the total mass of sodium tungstate, thiourea and hydroxylamine hydrochloride; the amount of graphene added is 0.1% to 1% of the mass of sodium tungstate.
4. The method for preparing a WS2 / graphene electrode material according to claim 1, characterized in that: In step (1), the surfactant is CTAB, and the amount of CTAB added is 0.5% to 2% of the mass of the mixed solution; and the pH adjustment refers to adjusting the pH value to 5 to 7 with hydrochloric acid or ammonia water.
5. The method for preparing a WS2 / graphene electrode material according to claim 1, characterized in that: The pressure-resistant reactor in step (2) is a polytetrafluoroethylene-lined stainless steel autoclave; the reaction temperature of the hydrothermal reaction is 160 to 200° C., and the reaction time is 12 to 48 hours.
6. The method for preparing a WS2 / graphene electrode material according to claim 1, characterized in that: The separation in step (3) refers to filtering and separating the solid phase product; the washing refers to washing with deionized water and anhydrous ethanol; and the drying refers to drying at a temperature of 50 to 70° C. for 8 to 12 hours.
7. A WS2 / graphene electrode material, characterized in that: It is prepared by the method described in any one of claims 1 to 6; the WS2 / graphene electrode material is composed of flat and smooth nanosheets, wherein the mass ratio of tungsten, sulfur and carbon is 1-20:1-10:1-90.
8. Use of the WS2 / graphene electrode material described in claim 7 in removing heavy metal ions by capacitive adsorption.
9. The use of a WS2 / graphene electrode material according to claim 8 in capacitive adsorption to remove heavy metal ions, characterized in that: The application method is: using the WS2 / graphene electrode material as the negative electrode of a capacitive deionization device, using the activated carbon material as the positive electrode, and then removing heavy metal ions through capacitive adsorption.
10. The use of a WS2 / graphene electrode material according to claim 9 in capacitive adsorption to remove heavy metal ions, characterized in that: The voltage adsorbed by the capacitor is 0.1-5V; the heavy metal ions include at least one of Cr, Cd, Pb, Ni, Co, and Cu heavy metal ions.
Citation Information
Patent Citations
Hydrothermal preparation method for composite material of single-layer WS2 and graphene
CN102694171A
Preparation method of tungsten disulfide nanorod
CN105502502A
Preparation method of graphene doped WS2 and application of graphene doped WS2 in lithium / sodium ion battery
CN108899496A
Preparation method of GO / MoS2 electrode for removing lead ions in water by electrochemical method
CN111302445A
A system for evaluating the amount of carbon dioxide emissions per unit of building.
KR1020230055490A
Cited By
Sewage autotrophic denitrification treatment process and system and filler thereof
CN120117747A