Method for manufacturing preform for optical fiber
By using plasma deposition and flame hydrolysis processes in the manufacturing of optical fiber prefabricated parts, the multi-layer structure of optical fiber prefabricated parts is formed, which solves the problem of strict requirements on the purity and size of the base tube, significantly reduces the attenuation of optical signals, and improves the performance of optical fibers .
Patent Information
- Application Number
- CN202410956029.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2016-03-03
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing method of manufacturing prefabricated parts for optical fibers, the purity and size of the base tube are strictly required, making it difficult to obtain sufficient quality prefabricated parts, resulting in optical signal attenuation problems.
The plasma reaction zone is generated by electromagnetic radiation, and the non-vitrified silicon oxide and vitrified silicon oxide layers are deposited on the hollow base tube through CVD process, forming an inner optical cladding and optical core layer, and glass-deposited on the outside by flame hydrolysis process Fluorine doped intermediate cladding, and then natural silicon oxide particles are deposited on the outside to melt to form an outer cladding, optimizing the layer structure to reduce attenuation.
High-quality fiber prefabricated parts are realized, reducing the attenuation of optical signals and meeting the performance requirements of optical fibers.
Smart Images

Figure CN118908559A_ABST
Abstract
Description
[0001] The present application is a divisional application of an application filed on March 3, 2016, with application number 201680085299.2 and invention name “Method for manufacturing a preform for optical fiber”. Technical Field
[0002] The present invention relates to a method for manufacturing a preform for optical fibers. Furthermore, the invention relates to a preform obtained thereby and to an optical fiber obtained from the preform. The present teaching relates to the field of manufacturing optical fibers by means of chemical vapor deposition (CVD) in which a layer of silicon oxide is deposited on a substrate; examples of said chemical vapor deposition are modified chemical vapor deposition (MDVD), plasma enhanced chemical vapor deposition (PECVD or PCVD), and outside vapor deposition (OVD). Background Art
[0003] A method for producing a primary preform precursor is known from WO 2015 / 002530 of the present applicant, wherein the method comprises the following steps: i) providing a hollow substrate tube; ii) generating a first plasma reaction zone having first reaction conditions in the interior of the hollow substrate tube by means of electromagnetic radiation to achieve deposition of non-vitrified silica layers on the inner surface of the hollow substrate tube, and subsequently; iii) generating a second plasma reaction zone having second reaction conditions in the interior of the hollow substrate tube by means of electromagnetic radiation to achieve deposition of vitrified silica layers on the non-vitrified silica layers deposited in step ii); iv) removing the hollow substrate tube from the vitrified silica layer deposited in step iii) and the non-vitrified silica layer deposited in step ii) to obtain a deposited tube.
[0004] It is difficult to obtain commercially available substrate tubes in sufficient quality due to a double constraint; first, the substrate tube must have a certain purity of the glass used, and second, the substrate tube must provide an outer diameter and an inner diameter of certain dimensions, and these dimensions must be within very narrow margins relative to the length of the substrate tube. The substrate tube becomes part of the preform and will therefore end up in the optical fiber; the purity must be sufficiently high to avoid attenuation of the optical signal. Summary of the invention
[0005] In one aspect, the present invention relates to a method for manufacturing a preform for an optical fiber, the method comprising the following steps in order:
[0006] i) depositing a non-vitrified silicon oxide layer on the inner surface of the hollow substrate tube by means of an inner plasma reaction zone having first reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation;
[0007] ii) depositing a vitrified silicon oxide layer on the inner surface of the non-vitrified silicon oxide layer deposited in step i) inside the hollow substrate tube by generating an inner plasma reaction zone having a second reaction condition inside the hollow substrate tube by means of electromagnetic radiation to form at least an inner optical cladding layer and an optical core layer from the periphery to the center;
[0008] iii) removing the hollow substrate tube from the vitrified silica layer deposited in step ii) and the non-vitrified silica layer deposited in step i) to obtain a deposited tube;
[0009] iv) optionally collapsing the deposited tube obtained in step iii) to obtain a deposited rod comprising, from the periphery to the center, at least one inner optical cladding and an optical core;
[0010] v) preparing the intermediate layer by the following steps:
[0011] * depositing a non-vitrified silicon oxide layer on the outside surface of the deposition tube obtained in step iii) or the deposition rod obtained in step iv) using glass-forming precursors in an outer reaction zone by a flame hydrolysis process, and subsequently;
[0012] * drying and consolidating the non-vitrified silica layer into a vitrified fluorine-doped silica intermediate cladding; and
[0013] *Contraction without omitting the previous step iv);
[0014] thereby providing a solid rod comprising, from the periphery to the center, an intermediate layer, at least one inner optical cladding and an optical core; wherein a fluorine-containing gas is used during deposition and / or drying and / or consolidation, and wherein the ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core is at least 3.5;
[0015] vi) depositing natural silicon oxide on the outer side surface of the intermediate cladding of the solid rod obtained in step v) by melting natural silicon oxide particles in an outer deposition zone to produce an outer cladding, thereby obtaining a preform.
[0016] Further aspects and embodiments of the invention are disclosed in the dependent claims and the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a cross section of a preform according to the present invention.
[0018] definition
[0019] The following definitions are used in this specification and claims to define the subject matter.Other terms not cited below are intended to have meanings generally accepted in the art.
[0020] - "Hollow substrate tube" as used in this specification means: preferably an elongated tube having a cavity inside. During the manufacture of the preform, the inside of the tube may be provided (or coated) with a plurality of glass layers.
[0021] - "Preform" as used in this specification refers to: a solid rod (solid composite preform) or a final preform that can be used directly to draw an optical fiber therefrom.
[0022] - "Deposition tube" as used in this specification means: a hollow tube comprising a vitrified silica layer; said silica layer is deposited on the inside of a substrate tube which is subsequently removed. In other words, the substrate tube does not form part of the deposition tube.
[0023] - "Deposition rod" as used in this specification means: a solid rod obtained by shrinking a deposition tube. The substrate tube does not form part of the deposition rod.
[0024] - "Inner surface" as used in this specification means: the inner side surface or the internal surface of the hollow substrate tube.
[0025] - "Silicon oxide" as used in this specification means: any substance in the form of SiOx, whether stoichiometric or not, and whether crystalline or amorphous.
[0026] - "Synthetic silicon oxide" as used in this specification means: amorphous silicon oxide; it is obtained by a chemical synthesis reaction in which a precursor containing silicon atoms reacts with oxygen to form silicon oxide. The purity of synthetic silicon oxide is higher than that of natural silicon oxide. The cost of synthetic silicon oxide is higher than that of natural silicon oxide. It may be known as SAS (Synthetic Amorphous Silica).
[0027] - "Natural silicon oxide" as used in this specification refers to crystalline silicon oxide produced in nature, such as in the form of quartz or crystal stone. For example, it is ground or milled to obtain particles of natural silicon oxide. Particles of natural silicon oxide having a particle size distribution of 95% of particles up to 400 microns measured by laser diffraction technology can be used. It is referred to as fine natural silicon oxide in this specification. The cost of natural silicon oxide is lower than that of synthetic silicon oxide.
[0028] - "Glass-forming precursor" as used in this specification refers to a reactive compound or composition used during the deposition process to react with oxygen to form an oxide that can be converted into a glass layer. Examples are silicon halides such as SiCl4, or cyclopolydimethylsiloxanes such as octamethylcyclotetrasiloxane (OMCTS).
[0029] - "Fluorine-containing gas" as used in this specification means: a gas containing fluorine and / or one or more fluorinated compounds, the fluorinated compounds being compounds including at least one bonded fluorine atom, for example, fluorinated hydrocarbons or sulfur hexafluoride (SF6).
[0030] - "doped glass layer" as used in this specification means: a glass layer comprising a dopant, which is a compound or composition present in the glass of the optical fiber and which has an influence on the refractive index of said glass. It may be, for example, a down dopant, i.e. a dopant that lowers the refractive index, such as fluorine or boron (for example introduced as a precursor in the form of F2, C2F8, SF6, C4F8 or BCl3). It may be, for example, an up dopant, i.e. a dopant that increases the refractive index, such as germanium (for example introduced as a precursor in the form of GeCl2 (germanium dichloride) or GeCl4 (germanium tetrachloride)). Dopants may be present in the glass in the form of interstices (for example in the case of F) or they may be present as oxides (for example in the case of germanium, aluminum, phosphorus or boron). Fluorine-doped silicon oxide means silicon oxide doped with a fluorine dopant.
[0031] - "Precursor of a dopant" as used in this specification means a compound or composition which, when introduced or converted into a glass, possibly after reaction with oxygen, becomes a dopant having an influence on the refractive index of the glass.
[0032] - "Non-vitrified silica" or "soot" as used in this specification means: silica that is not completely vitrified (= not vitrified or partially vitrified). It can be undoped or doped.
[0033] - "Vitrified silica" or "glass" as used in this specification means: a glassy substance produced by the vitrification of silicon oxide. It can be undoped or doped. Undoped vitrified synthetic silica is also known as fused quartz or fused silica, and has a high purity and consists mainly of amorphous SiO2; it can contain chlorine in an amount of up to 1500 ppm and still be considered undoped. Vitrified natural silica is prepared from natural silicon oxide particles or powder and contains several impurities.
[0034] - "Reaction zone" as used in this specification means: a zone or axial location where glass forming precursors react with or without precursors of dopants, and / or where deposition occurs. The zone preferably moves back and forth along the longitudinal length of the elongated tube or rod. The inner reaction zone is a reaction zone where deposition is achieved on the inside of the tube, and the outer reaction zone is a reaction zone where deposition is achieved on the outside of the tube or rod. The plasma reaction zone is a reaction zone formed by plasma. The outside deposition zone is a reaction zone for deposition on the outside of the tube or rod.
[0035] - "Intermediate layer" or intermediate cladding as used in this specification refers to: a layer of silicon oxide present between the outer cladding and the inner optical cladding.
[0036] - "Reaction conditions" as used in this specification refers to: a set of conditions such as temperature, pressure, electromagnetic radiation (eg microwaves) for achieving deposition of a silicon oxide layer (non-vitrified or vitrified).
[0037] - "Plasma" as used in this specification refers to an electrically neutral medium of a (partially) ionized gas comprising positive ions and free electrons, wherein the ionization is induced by electromagnetic radiation, for example by microwaves.
[0038] - "Drying" or dehydration as used in this specification means: removing OH-groups or H2O impurities from the deposited layer, possibly under the influence of heat, in a chlorine-containing environment.
[0039] - "Consolidation" as used in this specification means: sintering or fusing a porous layer of non-vitrified silica or dust into a vitrified layer of silica under the influence of heat.
[0040] - "Flame hydrolysis process" as used in this specification refers to: a chemical process (also known as combustion chemical vapor deposition or CCVD) by which a layer of material is deposited onto a substrate using precursor compounds added to a flame (e.g. from combustion gases). The flame moves over close to the surface to be coated, and the energy within the flame converts the precursors into reactive intermediates, which react with oxygen and are deposited on the substrate, forming an adherent layer of material.
[0041] - "Melting" as used in this specification refers to the process of heating silicon oxide particles. These particles are initially in a crystalline state, and after melting they are in a glassy state and are no longer recognizable as separate particles. DETAILED DESCRIPTION
[0042] The method according to one aspect of the present teachings comprises the step of preparing an intermediate layer of synthetic silica by depositing (multiple) non-vitrified silica layers on the outside surface of a deposition tube / rod using a flame hydrolysis process using a glass-forming precursor, and subsequently, drying and consolidating the non-vitrified silica layers into a vitrified fluorine-doped silica intermediate cladding. The presence of the intermediate layer further isolates the outer cladding from the core, resulting in a reduction in attenuation.
[0043] During the deposition and / or drying and / or consolidation of the intermediate layer, a fluorine-containing gas is used. This will ensure down-doping of the synthetic silica for obtaining a refractive index of the intermediate layer that is approximately equal to or lower than the refractive index of the outer cladding when the fiber is drawn. The absolute difference in refractive index between the intermediate cladding and the outer cladding is preferably between 0 and 2×10 -3 between 0 and 1×10 -3 between.
[0044] The preform according to the present invention may include the following layers from the center to the periphery (for example, as a cross section of the preform): Figure 1 shown):
[0045] An optical core 1 having an outer diameter (A);
[0046] an inner optical cladding 2 directly surrounding the optical core; the inner optical cladding having an inner diameter that is the same as the outer diameter (A) of the optical core and having an outer diameter (B);
[0047] an intermediate cladding 3 directly surrounding the inner optical cladding; the intermediate cladding having an inner diameter that is the same as the outer diameter (B) of the inner optical cladding and having an outer diameter (C);
[0048] an overcladding layer 4 directly surrounding the intermediate cladding; the overcladding layer having an inner diameter that is the same as the outer diameter (C) of the intermediate cladding and having an outer diameter (D);
[0049] The ratio C / A between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core is at least 3.5. This ratio ensures a sufficient distance between the optical core and the outer cladding of natural silica, and this will sufficiently reduce attenuation. In other words, the intermediate layer should have a certain thickness to ensure this ratio. Preferably, the ratio B / A between the outer diameter (B) of the inner optical cladding and the outer diameter (A) of the core is at least 1.8.
[0050] Several method steps will be discussed below.
[0051] Step i)
[0052] Step i) involves depositing a non-vitrified silicon oxide layer on the inner surface of the hollow substrate tube by means of an inner plasma reaction zone having first reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation.
[0053] First, a hollow substrate tube is provided with an inner surface on which deposition will occur. The substrate tube used in accordance with the present invention may be a quartz substrate tube, such as a relatively low purity quartz tube. It may also be a non-quartz substrate tube. The substrate tube should be able to withstand the temperatures used in the deposition process without melting or liquefying. In addition, when a plasma inside deposition method is used to prepare the inside deposition, the substrate tube should be transparent to electromagnetic radiation so that a plasma is formed inside the substrate tube. The dimensions of the substrate tube used in the present invention may be selected based on the requirements of the process equipment, the size of the preform, and the type of optical fiber to be formed. It may be required to subject the substrate tubes to a pretreatment process to make them more suitable for use in the plasma deposition equipment used in the present invention.
[0054] A gas stream is supplied to the interior of the substrate tube. In one embodiment, a gas stream is introduced via a supply side of the substrate tube, such as via a pipeline connected to the supply side; the gas stream comprises at least one glass-forming gas (such as silicon tetrachloride in combination with oxygen).
[0055] The removal of the substrate tube is facilitated by the presence of a soot (non-vitrified silica) layer between the inner surface of the substrate tube and the deposited glass layer. This soot layer (non-vitrified silica layer) is sacrificed during the process. The soot layer is a fine, dust-like material that enables the removal of the substrate tube.
[0056] The silica dust (non-vitrified silica layer) has a certain (although limited) adhesion to the glass layer to be deposited, and has a certain (although limited) adhesion to the substrate tube. The dust is used as a barrier between two solid parts, firstly the substrate tube, and on the other hand the vitrified silica layer deposited in step ii). This barrier or sacrificial layer will serve as a non-sticky layer or buffer layer that separates the two vitrified silica layers on either side. The dust layer can be regarded as a buffer layer between the two tubes of the substrate tube on the outside and the deposition tube on the inside. On the one hand, the adhesion of the dust layer to the substrate tube should be sufficient to allow the formation of a layer (e.g., a continuous layer and / or a layer with a substantially constant coverage of the inner surface of the substrate tube, and / or a layer with a substantially constant thickness relative to the length of the substrate tube). On the other hand, the adhesion of the dust layer to the substrate tube should not be too high so that the substrate tube is subsequently separated from the dust layer. On the one hand, the adhesion of the dust layer to the vitrified silica layer to be deposited should be sufficient to allow the formation of a vitrified silica layer. On the other hand, the adhesion of the soot layer to the vitrified silica layer to be deposited should not be too high so that the vitrified silica layer separates from the soot layer when the substrate tube is removed so that the vitrified silica layer forming the deposition tube is not damaged during substrate tube removal.
[0057] During step i), so-called first reaction conditions are applied. These first reaction conditions are effective for the production of non-vitrified silicon oxide layers, in other words, these conditions are selected to prevent the deposition of vitrified silicon oxide. The first reaction conditions may require the use of electromagnetic radiation to obtain plasma (see PCVD section below). During this step, there is a gas flow of more than one glass-forming gas. In one embodiment, a high pressure (relative to vacuum, such as>30mbar, or>50mbar) is maintained inside the substrate tube to prevent vitrification; the pressure determines the amount of silicon oxide formed in the gas phase. If the pressure is higher than, for example, 30mbar, a large amount of dust will be generated by the aggregation of silicon oxide particles in the gas phase before being deposited on the inner diameter of the substrate tube. The dust will adhere to the inner surface of the substrate tube. When the plasma deposition process is carried out under a higher pressure state (>50mbar or even>60mbar), the deposition includes even a larger portion of dust material.
[0058] In one embodiment, the non-vitrified silica is supplied over a large portion of the inner surface of the substrate tube, for example between the reversal point near the supply side and the reversal point near the discharge side. This allows for optimal use of the substrate tube.
[0059] In one embodiment, the area of the inner surface covered by the vitrified silica layer is also previously covered by a non-vitrified silica layer. This will facilitate the later removal of the substrate tube without damaging the vitrified silica layer, ie the deposited layer.
[0060] In one embodiment, the non-vitrified silica is applied as a continuous layer. This will prevent any damage to the vitrified silica layer when the substrate tube is removed.
[0061] In one embodiment, the non-vitrified silica is applied as a layer having a substantially constant thickness relative to the length of the substrate tube. This will ensure uniform deposition of the vitrified silica layer.
[0062] Step ii)
[0063] Step ii) involves depositing a vitrified silica layer on the inner surface of the non-vitrified silica layer deposited in step i) inside the hollow substrate tube by an inner plasma reaction zone having second reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation to form at least an inner optical cladding and an optical core layer from the periphery to the center.
[0064] Step ii) requires the generation of an inner plasma reaction zone with a second reaction condition different from the first reaction condition inside the hollow substrate tube. The substrate tube already comprises a deposited non-vitrified glass layer on its inner surface. The second reaction condition is generated with the aid of electromagnetic radiation. Thus during step ii), the deposition of a vitrified silicon oxide layer on the non-vitrified silicon oxide layer deposited in the previous step is achieved. The second reaction condition should be suitable for the deposition of glass and is known in the art, it may require the use of electromagnetic radiation to obtain a plasma (e.g. for a PCVD process as described below).
[0065] At the end of this deposition step, a substrate tube is obtained having the desired number of doped or undoped vitrified silicon oxide layers deposited on the inner surface. At this point, the deposition process is stopped. Thus, in the case of a plasma deposition process, the electromagnetic radiation is stopped and the gas flow, including the glass-forming gas, is also stopped.
[0066] A gas stream is supplied to the interior of the hollow substrate tube. In one embodiment, the gas stream is introduced via a supply side of the substrate tube; the gas stream comprises at least one glass-forming precursor (e.g., silicon tetrachloride in combination with oxygen). Optionally, during at least a portion of the deposition, the gas stream further comprises a precursor for at least one dopant, such as germanium (e.g., in the form of germanium tetrachloride or germanium dichloride) and / or fluorine (e.g., in the form of a fluorine-containing gas such as C2F6).
[0067] During this step, multiple layers of vitrified silica are formed. In one embodiment, the successive silica layers are doped or undoped and determine the refractive index profile of the optical fiber to be made from the preform. For example, a series of layers forming an optical cladding may include a region having multiple layers of vitrified fluorine-doped silica having a refractive index difference of -1×10 -3and -10×10 -3 The subsequent series of layers forms an optical core comprising a region of multiple layers of glassy GeO2-doped silicon oxide having a refractive index difference of 3×10 -3 and 10×10 -3 between.
[0068] It is within the capabilities of the PCVD process to form any series of vitrified silica layers having different or gradually varying refractive indices, including vitrified silica layers having more than one dopant, such as fluorine and GeO2 co-doped layers.
[0069] PCVD
[0070] PCVD is one or more processes that can be used to deposit a non-vitrified silicon oxide layer during step i) of the process and / or to deposit a vitrified silicon oxide layer during step ii) of the process. This technique is used to deposit a thin film on a substrate, usually on the inside of a substrate tube, from a gaseous state (vapor) to a solid state. In this process, a chemical reaction is involved, which occurs after the generation of a plasma that reacts the glass-forming gases introduced into the interior of the substrate tube. They can be added from one end, called the "supply side" of the substrate tube. A doped or undoped glass layer (depending on the use of reactive gases with or without precursors of one or more dopants, respectively) is deposited onto the inner surface of the substrate tube. For example, the remaining gas is exhausted or removed from the other or opposite end of the substrate tube, called the "exhaust side" of the substrate tube. The remaining gas (unreacted starting gas and reaction products) is removed, for example, with the aid of a vacuum pump; the vacuum pump has the effect of generating a reduced pressure (for example between 5 and 50 mbar) inside the substrate tube.
[0071] In one embodiment, the plasma is induced by using electromagnetic radiation (e.g., microwaves), which can be generated in a generator and guided to an applicator via a waveguide. The applicator preferably surrounds a portion of the substrate tube. The plasma reaction zone is a three-dimensional space occupied by the plasma inside the substrate tube. The applicator couples electromagnetic energy into the plasma generated inside the substrate tube. The applicator can move back and forth in the longitudinal direction of the substrate tube; then, the formed plasma (called the "inner plasma reaction zone") also moves back and forth. As a result of this movement, a thin silicon oxide layer is deposited on the inside of the substrate tube during each stroke or pass. Depending on the reaction conditions, the layer can be non-vitrified silicon oxide or vitrified silicon oxide. The applicator and the substrate tube can be surrounded by a heating furnace to maintain the substrate tube at a temperature between 900°C and 1300°C during the plasma deposition process.
[0072] The applicator can translate over the length of the substrate tube within the boundaries of a furnace that surrounds the substrate tube and the applicator that reciprocates within the furnace; the plasma has the same translation. In this embodiment, when the applicator reaches the inner wall of the furnace near one end of the substrate tube, the movement of the applicator is reversed so that it moves toward the other inner wall of the furnace to the other end of the substrate tube. The applicator and therefore the plasma travels in a reciprocating motion along the length of the substrate tube. Each reciprocating motion is referred to as a "stroke" or "stroke". With each stroke, a thin layer of silicon oxide material is deposited on the inside of the substrate tube.
[0073] The plasma causes a chemical reaction of the glass-forming gas (e.g., O2, SiCl4, and a precursor of a dopant such as GeCl4 or other gases) supplied to the inside of the substrate tube. The chemical reaction of the glass-forming gas causes Si (silicon), O (oxygen) to react with, for example, a dopant Ge (germanium), so that direct deposition of, for example, Ge-doped SiOx on the inner surface of the substrate tube is achieved. Only at the location of the plasma, the reactive gas is converted into solid glass and deposited on the inner surface of the substrate tube.
[0074] The plasma may be generated in only a portion of the substrate tube, ie the portion surrounded by the applicator.
[0075] As the number of strokes increases, the accumulated thickness of these films, ie the deposited material, increases; thus resulting in a reduction in the remaining inner diameter of the substrate tube. In other words, with each stroke, the hollow space inside the substrate tube remains progressively smaller.
[0076] Step iii)
[0077] Step iii) involves the removal of the substrate tube.
[0078] The substrate tube is removed from the vitrified silicon oxide layer deposited in step ii) and the non-vitrified silicon oxide layer deposited in step i). After this step, a deposited tube is obtained.
[0079] After the deposition of the vitrified silicon oxide layer in step ii) onto the interior of the substrate tube (on top of the already existing non-vitrified layer deposited in step i), the substrate tube is removed. The substrate tube can be considered a temporary substrate tube in the sense that it does not form part of the material constituting the preform. The substrate tube can be considered a hollow mandrel which is removed after its task has been fulfilled.
[0080] The removal of the substrate tube may be mechanical. Mechanical removal may be performed manually or by machine. There are several ways in which the substrate tube may be removed. In the first, the substrate tube will remain intact after removal. In the second, the substrate tube will not remain intact after removal.
[0081] For example, near the two longitudinal ends of the substrate tube, an annular (radial) cut is made, preferably through the thickness of the substrate tube, optionally extending into the soot layer. After this radial cut, the substrate tube is in principle present coaxially around the deposited glass layer in a non-connected (loose) manner. The soot layer is brittle and by rotation or forced sliding of the "loose" substrate tube, this soot layer can be broken or shattered to provide a movement between the substrate tube and the glass layer. However, it should be noted that this movement is in practice very limited, since the limited space between the substrate tube and the glass layer is filled with the (broken or shattered) soot layer. The soot layer can also be removed first.
[0082] In one embodiment, before removing the substrate tube, the (sacrificial) non-vitrified silica layer is removed by using a liquid, such as water or other aqueous solution. The brittle particles of the non-vitrified silica are broken so that a fine, dust-like material is obtained dispersed in the liquid, which can be removed by removing the liquid. This will then free up the space between the substrate tube and the vitrified silica layer, allowing the substrate tube to slide off the deposition tube formed by the vitrified silica layer. After removing the liquid and particles, a hollow space is obtained between the two coaxial tubes, facilitating the removal of the outer substrate tube.
[0083] According to the first aspect, the implementation is as follows. First, radial cuts are made near the two longitudinal ends, as described above. Second, one (or both) ends of the substrate tube are removed (e.g., by making a deeper radial cut through the entire substrate tube and deposition tube) so that the substrate tube can slide off the deposited glass layer on its inside. This allows the substrate tube to be used again for another deposition process. In one embodiment, the total thickness of the non-vitrified layer (soot layer) is between 200 and 1000 microns, with, for example, between 100 and 500 layers of non-vitrified silica. This allows the distance between the two coaxial tubes (i.e., the outer substrate tube and the inner deposition tube) to be sufficient to achieve removal.
[0084] For the second aspect, where the substrate pipe is not left intact, several, non-limiting embodiments perform longitudinal cuts and removal or fragmentation of the substrate pipe by manual hammers and chisels.
[0085] In one embodiment, more than one (e.g. two opposite) longitudinal cuts (e.g. by a machine-operated saw blade) may be made to the substrate pipe. For example, these longitudinal cuts (or one-shot cuts) are made over the entire length of the substrate pipe. These cuts (or one-shot cuts) preferably pass through the thickness of the substrate pipe, optionally extending into the dust layer. After making these cuts (or one-shot cuts), the two halves (or more parts) of the substrate pipe may be removed. This makes the substrate pipe unusable.
[0086] In another embodiment, the substrate pipe may be subjected to a manual hammer and chisel to form a crack (or more cracks). These cracks will develop in the longitudinal direction. This will fragment the substrate pipe, which is removed in multiple parts. This makes the substrate pipe unusable again.
[0087] In another embodiment, the substrate tube is provided with one or more longitudinal or spiral grooves made with a glazier's diamond knife, followed by fragmentation of the substrate tube. This can be done by machine or by manual operation. This renders the substrate tube unusable.
[0088] In order to reduce manufacturing time and costs, in this case, the total thickness of the non-vitrified layers is preferably between 1 and 100 micrometers, more preferably a maximum of 40 micrometers, even more preferably a maximum of 20 micrometers. The number of non-vitrified silicon oxide layers is preferably between 1 and 50 layers, more preferably a maximum of 20 layers, even more preferably a maximum of 10 layers.
[0089] In another aspect of these embodiments, the ends of the substrate tube (welded ends) can be maintained in place. This allows the deposited tube (after removal of the substrate tube) to be easily transferred to the next step of the process, such as a shrinking device or a plasma deposition device. In this case, the step of radial cutting near both longitudinal ends can be performed as a first step to remove the substrate tube.
[0090] Step iv)
[0091] Step iv) involves shrinking the deposited tube obtained in step iii) to obtain a deposited rod comprising from the periphery to the center at least one inner optical cladding and an optical core. This step is optional at this point in the process.
[0092] The deposited tube obtained after removal of the substrate tube can subsequently be compacted by heating into a solid rod ("shrinking") or a deposited rod.
[0093] For shrinking, the deposition tube can be mounted on a lathe, for example, by fixing the two ends of the deposition tube by means of a clamp. The deposition tube can be heated locally (for example, by the hot zone of a reciprocating furnace or burner) until a sufficiently high temperature is reached to soften the glass. When the glass begins to soften, the deposition tube assumes a smaller diameter and closes the central cavity. On the one hand, the process is carried out until the deposition tube is completely closed, that is, until the cavity no longer exists; several strokes can be performed to achieve this. The temperature during shrinking can be at least 1700° C., for example at least 1800° C., or at least 1900° C.
[0094] The deposited tube may be subjected to a shrinking process to form a solid rod (performing step iv)). However, it is conceivable to carry out the shrinking step only after the deposition of the intermediate layer (without performing step iv)).
[0095] Step v)
[0096] Step v) involves the preparation of the intermediate layer.
[0097] In one embodiment, the step of adding the intermediate layer is carried out directly on the deposition tube after removal of the substrate tube, or on a deposition rod obtained from shrinking the deposition tube; no sleeve is applied on the deposition tube or rod.
[0098] The solid rod obtained after this step can be considered as a primary preform.
[0099] The intermediate layer is preferably obtained by an external vapor deposition (OVD) process. During this process, a non-vitrified silicon oxide layer is deposited and subsequently consolidated (vitrified). During this step, synthetic silicon oxide is deposited. Vitrified synthetic silicon oxide is also known as fused quartz or fused silicon oxide, and has a high purity and mainly comprises amorphous SiO2. The refractive index of vitrified synthetic silicon oxide at 632.8nm can be 1.4585. Even if synthetic silicon oxide may have, for example, chlorine contaminants, synthetic silicon oxide is also referred to as pure silicon oxide. It can be obtained by using high-purity raw materials, such as gaseous silicon precursors such as silicon tetrahalide SiX4 (wherein X is a halogen) (e.g. SiCl4), or siloxane precursors such as having the formula [(CH3)2SiO] y Cyclomethicone (cyclopolydimethylsiloxane) (for example, octamethylcyclotetrasiloxane where y is 4, also known as OMCTS or D4) can be used to prepare synthetic silica. y wherein y is 5 or 6. Preferred precursors for synthetic silicon oxide used during this step are SiCl4 and D4.
[0100] This step may include several sub-steps discussed in more detail below.
[0101] Sub-step a) :
[0102] * A non-vitrified silicon oxide layer is deposited on the outer surface of the deposition tube obtained in step iii) or the deposition rod obtained in step iv) by a flame hydrolysis process in an outer reaction zone using a glass-forming precursor.
[0103] Preferably, the deposition of the non-vitrified interlayer is achieved by a flame hydrolysis process of a silicon oxide based dust on a deposition tube or a deposition rod. In one embodiment, the tube or rod is mounted on an OVD horizontal lathe and the silicon oxide dust is deposited on the outside of a rotating tube or rod used as a target in a standard OVD process.
[0104] Flame hydrolysis deposition of silicon oxide produces porous (non-vitrified) glass or dust. A vapor-fed burner can be used, in which a precursor such as SiCl4 or OMCTS is added in gaseous form to the burner flame to produce oxide-dust particles that are deposited on the surface of the substrate. The gas stream provides vapor of at least one material that will hydrolyze in the burner flame to form the oxide.
[0105] In one embodiment, the glass-forming precursor used is a gaseous silicon precursor.
[0106] In one embodiment, the gaseous silicon precursor is a silicon tetrahalide or a silicon tetrahalide having the formula [(CH3)2SiO] y wherein y is 4, 5 or 6.
[0107] In one embodiment, the gaseous silicon precursor is SiCl4 or octamethylcyclotetrasiloxane (OMCTS). OMCTS is an environmentally friendly chlorine-free precursor. OMCTS can be supplied to the lathe in liquid form and converted into vapor form in an evaporator using nitrogen as a carrier.
[0108] In one embodiment, a fluorine-containing gas is used during the deposition of the non-vitrified silicon oxide layer deposited in step v) to obtain a fluorine-doped non-vitrified silicon oxide layer. In one embodiment, the fluorine-containing gas is selected from the group consisting of SiF4, SF6, CF4, and C2F6, preferably SF6 and C2F6.
[0109] Sub-step b) :
[0110] * Drying and consolidating the non-vitrified silica layer into a vitrified fluorine-doped silica intermediate cladding.
[0111] Drying and consolidation of the non-vitrified silica layer can be performed by placing the deposited tube / rod with the non-vitrified silica layer on the outer surface in a heated environment, such as a heating furnace, wherein the temperature of the first zone is, for example, above 900°C, for example above 1000°C, such as between 1000°C and 1300°C, and the temperature of the preferably continuous second zone is, for example, above 1400°C, or above 1500°C, such as between 1500°C and 1650°C.
[0112] The heating furnace may be supplied with helium at a flow rate of 10 to 20 l / min, thereby creating a helium atmosphere inside.
[0113] The (entire) deposition tube or deposition rod (comprising a non-vitrified glass layer on its outer surface) is maintained in the first zone for a first drying time which may be between 60 and 180 minutes, such as between 100 and 140 minutes.
[0114] In one embodiment, a fluorine-containing gas is used during the drying of the non-vitrified silicon oxide layer deposited in step v); in other words, simultaneous drying and doping. In one embodiment, the fluorine-containing gas is selected from the group consisting of SiF4, SF6, CF4, and C2F6, preferably SF6 and C2F6.
[0115] In one embodiment, simultaneous drying and doping of the non-vitrified glass layer with fluorine occurs by heating the entire deposition tube or deposition rod (including the non-vitrified glass layer on its outer surface) at a temperature of 1000° C. to 1350° C. and by exposing it to an atmosphere containing a chlorine-containing gas and a fluorine-containing gas (preferably a helium atmosphere), the content of fluorine-containing gas in the atmosphere is preferably 0.01% by volume to 0.50% by volume, and the content of chlorine-containing gas in the atmosphere is preferably between 2% by volume and 10% by volume.
[0116] In one embodiment, the content of chlorine-containing gas in the atmosphere is between 2 volume % and 10 volume %. In one embodiment, the content of fluorine-containing gas in the atmosphere is between 0.01 volume % and 0.50 volume %. In one embodiment, the atmosphere is a helium atmosphere.
[0117] Consolidation of the non-vitrified silica layer can be performed by moving the deposited tube / rod having the dry non-vitrified silica layer on the outer surface into the second zone at a speed of 5 mm / min to 10 mm / min until all parts of the tube / rod (including the non-vitrified glass layer as its outer surface) have been subjected to a heating environment with a temperature of, for example, above 1400°C, for example above 1500°C, such as between 1500°C and 1650°C.
[0118] In one embodiment, the chlorine-containing gas is maintained during consolidation of the non-vitrified layer in step v), in other words, simultaneous consolidation and further drying.
[0119] The consolidation time may be between 100 and 400 minutes, for example between 200 and 300 minutes.
[0120] The optimum fluorine doping level depends on the tension used to draw the fiber from the preform. In one embodiment, when the fiber is drawn with a drawing tension of 80 grams, the F doping of the intermediate layer is at least 1100 ppm, 1800 ppm is required for a drawing tension of 140 grams, and 2400 ppm is required for a drawing tension of 190 grams. If the fluorine doping is too low, an intermediate ring with a positive refractive index will appear in the refractive index profile, which will significantly increase the bending losses at longer wavelengths, making the fiber very sensitive to bending and less suitable for use.
[0121] Sub-step c) :
[0122] *Shrinkage in case the previous step iv) is omitted.
[0123] When deposition tubes are used instead of deposition rods for the addition of the intermediate layer, a shrinking step needs to be performed at this stage of the process. This can be a separate shrinking step as described above, or alternatively shrinking of the rods occurring during consolidation.
[0124] The result of process step v) is a solid rod comprising, from the periphery to the centre, an intermediate layer, at least one inner optical cladding and an optical core.
[0125] The solid rod obtained has a certain amount of fluorine doping obtained by using a fluorine-containing gas d during deposition and / or drying and / or consolidation.
[0126] The intermediate layer has a ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core of at least 3.5. In the case of a C / A ratio of 3.5, native silica with up to 0.1 ppm iron can be used without significant increase in attenuation at 1550 nm.
[0127] In one embodiment, the intermediate layer has a ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core of at least 4.0. In the case of a C / A ratio of 4.0, native silica with up to 0.3 ppm iron and 10 ppm OH can be used without significant increase in attenuation at 1550 nm.
[0128] In one embodiment, the intermediate layer has a ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core of at least 4.2. In the case of a C / A ratio of 4.2, native silica with up to 0.5 ppm iron can be used without a significant increase in attenuation at 1550 nm.
[0129] It should be noted that the ratio between C / A in the preform corresponds to the ratio between C / A in the optical fiber drawn therefrom.
[0130] The ratio between B / A is preferably between 1.8 and 3.0. It should be noted that the ratio between B / A in the preform corresponds to the ratio between B / A of the optical fiber drawn therefrom.
[0131] The thickness of the intermediate layer in the resulting optical fiber is preferably between 10 and 20 microns.
[0132] Step vi)
[0133] Step vi) involves depositing native silicon oxide on the outer surface of the intermediate cladding of the solid rod obtained in step v). This deposition occurs by melting particles or grains of native silicon oxide in an outer deposition zone to produce an outer cladding, thereby obtaining a preform.
[0134] The outer cladding is applied by depositing native silica on the outer surface of the intermediate cladding by melting fine native silica particles. The solid rod is further provided with an additional amount of glass on the outside, for example by means of an external vapor deposition process or direct glass overcladding (so-called "overcladding"), thereby obtaining a composite preform called final preform. From the final preform thus produced, one end of which is heated, an optical fiber is obtained by drawing on a drawing tower. The refractive index profile of the consolidated (final) preform corresponds to the refractive index profile of the optical fiber drawn from such a preform.
[0135] Outsourcing can be carried out using the so-called APVD process or axial (external) plasma vapor deposition, in which grains of native silicon oxide are deposited by gravity from a feed tube translated parallel to a solid rod, wherein the silicon oxide grains are fused with the aid of an atmospheric plasma flame at a temperature of, for example, 2300°C and then vitrified.
[0136] The melting of the silicon oxide particles that occurs during the APVD process can occur at a melting temperature at which the natural silicon oxide changes from a crystalline state to an amorphous state. The melting temperature can be higher than 1800°C, such as higher than 2000°C. The melting temperature can be lower than 2500°C, such as lower than 2200°C. In one embodiment, the melting temperature is between 1800°C and 2200°C. After melting, the resulting solid rod can be cooled to a temperature lower than 300°C, thereby forming a silicon oxide layer (SiO2). The melting can be performed using a plasma flame or a torch. The duration of the melting is between 12 and 24 hours. The flow rate of the natural silicon oxide during this process is between 30 and 150 g / min.
[0137] In one embodiment, fine natural silicon oxide particles, such as silicon oxide powder, are used during the final overcoating step, wherein "fine" means that the median particle size of the powder is less than 400 microns, preferably less than 200 microns.
[0138] Natural silica particles can be used as the material for the coating. However, natural silica contains impurities (e.g. hydroxyl groups or Fe). Typical residual contaminants of natural silica used for the manufacture of optical fibers - although the present invention is not limited to the use of natural silica with these values - are: between 5 and 25 ppm aluminum (Al), between 0.1 and 0.7 ppm lithium (Li), between 0 and 0.5 ppm iron (Fe), between 0 and 0.5 ppm potassium (K), between 0 and 0.5 ppm sodium (Na), between 0 and 1 ppm calcium (Ca), between 1 and 2 ppm titanium (Ti).
[0139] In one aspect, a preform obtained or obtainable by the above method is provided.
[0140] In one embodiment, the outer diameter of the optical core of an optical fiber drawn from such a preform is between 8 and 10 microns. In one embodiment, the outer diameter of the optical core is 8.5 microns.
[0141] In one embodiment, the outer diameter of the inner optical cladding of an optical fiber drawn from such a preform is between 16 and 24 microns. In one embodiment, the outer diameter of the inner optical cladding is between 19 and 21 microns. In one embodiment, the outer diameter of the inner optical cladding is 20 microns.
[0142] In one embodiment, the outer diameter of the intermediate layer of an optical fiber drawn from such a preform is between 28 and 40 microns. In one embodiment, the outer diameter of the intermediate layer is between 32 and 36 microns. In one embodiment, the outer diameter of the intermediate layer is 34 microns.
[0143] In one embodiment, the outer cladding of an optical fiber drawn from such a preform has a diameter between 100 and 150 microns. In one embodiment, the outer cladding has a diameter between 115 and 135 microns. In one embodiment, the outer cladding has a diameter of 125 microns.
[0144] In one aspect, an optical fiber obtained by the process of drawing the above preform is provided. In one embodiment, the optical fiber is a single-mode optical fiber. The final preform prepared using the method according to the present invention can be used to draw an optical fiber.
[0145] From the final preform thus produced, one end of which is heated, an optical fiber is obtained by drawing on a drawing tower. The refractive index profile of the consolidated (shrinked) preform corresponds to that of the optical fiber drawn from such a preform.
[0146] The present teachings do not require major changes to instrumentation or equipment already in use.
[0147] Terms
[0148] The following clauses define several aspects and embodiments of the teachings herein.
[0149] 1. A method for manufacturing a preform for an optical fiber, the method comprising the following (sequential) steps:
[0150] i) depositing a non-vitrified silicon oxide layer on the inner surface of the hollow substrate tube by means of an inner plasma reaction zone having first reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation;
[0151] ii) depositing a vitrified silica layer on the inner surface of the non-vitrified silica layer deposited in step i) inside the hollow substrate tube by means of an inner plasma reaction zone having second reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation to form at least an inner optical cladding layer and an optical core layer from the periphery to the center;
[0152] iii) removing the hollow substrate tube from the vitrified silica layer deposited in step ii) and the non-vitrified silica layer deposited in step i) to obtain a deposited tube;
[0153] iv) optionally, shrinking the deposited tube obtained in step iii) to obtain a deposited rod comprising at least one inner optical cladding and an optical core from the periphery to the center;
[0154] v) preparing the intermediate layer by the following steps:
[0155] * depositing a non-vitrified silicon oxide layer on the outer side surface of the deposition tube obtained in step iii) or the deposition rod obtained in step iv) by a flame hydrolysis process in an outer reaction zone using a glass-forming precursor, and subsequently;
[0156] * drying and consolidating the non-vitrified silica layer into a vitrified fluorine-doped silica intermediate cladding; and
[0157] *Contraction without the previous step iv);
[0158] thereby providing a solid rod comprising, from the periphery to the center, an intermediate layer, at least one inner optical cladding and an optical core; wherein a fluorine-containing gas is used during deposition and / or drying and / or consolidation, and wherein the intermediate layer has a ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core of at least 3.5;
[0159] vi) depositing natural silicon oxide on the outer side surface of the intermediate cladding of the solid rod obtained in step v) by melting natural silicon oxide particles in an outer deposition zone to produce an outer cladding, thereby obtaining a preform.
[0160] 2. The method according to clause 1, wherein the intermediate layer is doped with at least 1100 ppm of fluorine.
[0161] 3. The method according to clause 1, wherein the intermediate layer is doped with at least 1800 ppm of fluorine.
[0162] 4. The method according to clause 1, wherein the intermediate layer is doped with at least 2400 ppm of fluorine.
[0163] 5. The method according to clause 1, wherein the fluorine-containing gas is used during consolidation of the non-vitrified silicon oxide layer in step v).
[0164] 6. The method of clause 1, wherein the fluorine-containing gas is selected from the group consisting of SiF4, SF6, CF4, and C2F6.
[0165] 7. The method according to clause 1, wherein the fluorine-containing gas is SF6.
[0166] 8. The method according to clause 1, wherein the fluorine-containing gas is C2F6.
[0167] 9. The method of clause 1, wherein the C / A ratio is at least 4.0.
[0168] 10. The method of clause 1, wherein the C / A ratio is at least 4.2.
[0169] 11. The method according to clause 1, wherein the glass-forming precursor used in step v) is a gaseous silicon precursor.
[0170] 12. The method according to clause 1, wherein the glass forming precursor used in step v) is silicon tetrahalide.
[0171] 13. A method according to clause 1, wherein the glass-forming precursor used in step v) is a precursor having the formula [(CH3)2SiO] y wherein y is 4, 5 or 6.
[0172] 14. The method according to clause 1, wherein the glass forming precursor used in step v) is SiCl4.
[0173] 15. The method according to clause 1, wherein the glass forming precursor used in step v) is octamethylcyclotetrasiloxane (OMCTS).
[0174] 16. The method according to clause 1, wherein step ii) comprises depositing one or more layers of vitrified fluorine-doped silicon oxide, wherein the difference in refractive index between the vitrified fluorine-doped silicon oxide and the undoped silicon oxide is within -1×10 -3 and -10×10 -3 between.
[0175] 17. The method according to clause 1, wherein a plasma flame is used for the deposition of native silicon oxide in step vi).
[0176] 18. The method according to clause 1, wherein a fluorine-containing gas is used during drying of the non-vitrified silicon oxide layer deposited in step v).
[0177] 19. A method according to clause 18, wherein simultaneous drying and doping of the non-vitrified glass layer with fluorine occurs by heating the entire deposition tube or deposition rod (comprising the non-vitrified glass layer on its outer surface) at a temperature of 1000° C. to 1350° C. and by exposing it to an atmosphere comprising a chlorine-containing gas and a fluorine-containing gas, the content of the fluorine-containing gas in the atmosphere being 0.01% to 0.50% by volume.
[0178] 20. The method according to clause 19, wherein after simultaneous drying and doping of the non-vitrified glass layer with fluorine, the non-vitrified glass layer is consolidated at a consolidation temperature of 1500° C. to 1650° C.
[0179] 21. A preform obtained or obtainable by a method according to any one of the preceding clauses.
[0180] 22. An optical fiber obtained by the process of drawing the preform according to clause 21.
[0181] 23. A single-mode optical fiber obtained by the process of drawing the preform according to clause 21.
[0182] 24. An optical fiber according to clause 22 or 23, wherein the outer diameter of the optical core is between 8 and 10 microns.
[0183] 25. An optical fiber according to clause 22 or 23, wherein the outer diameter of the optical core is 8.5 microns.
[0184] 26. An optical fiber according to clause 22 or 23, wherein the outer diameter of the inner optical cladding is between 16 and 24 microns.
[0185] 27. An optical fiber according to clause 22 or 23, wherein the outer diameter of the inner optical cladding is between 19 and 21 microns.
[0186] 28. An optical fiber according to clause 22 or 23, wherein the outer diameter of the inner optical cladding is, for example, 20 microns.
[0187] 29. An optical fiber according to clause 22 or 23, wherein the outer diameter of the intermediate layer is between 28 and 40 microns.
[0188] 30. An optical fiber according to clause 22 or 23, wherein the outer diameter of the intermediate layer is between 32 and 36 microns.
[0189] 32. An optical fiber according to clause 22 or 23, wherein the outer diameter of the intermediate layer is 34 microns.
[0190] 33. An optical fiber according to clause 22 or 23, wherein the diameter of the outer cladding is between 100 and 150 microns.
[0191] 34. An optical fiber according to clause 22 or 23, wherein the diameter of the outer cladding is between 115 and 135 microns.
[0192] 35. An optical fiber according to clause 22 or 23, wherein the diameter of the outer cladding is 125 microns.
[0193] 36. A method for manufacturing a preform for an optical fiber, the method comprising depositing a non-vitrified silica layer by flame hydrolysis of a glass-forming precursor, adding an intermediate layer to the outer surface of a deposition tube or a deposition rod, and drying and consolidating, depositing the native silica on the outer surface of the intermediate cladding by melting the native silica particles.
[0194] 37. A method according to clause 36, wherein a fluorine-containing gas is used during deposition and / or drying and / or consolidation, and wherein the intermediate layer has a ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core of at least 3.5.
[0195] 38. A method for manufacturing a preform for optical fiber, the method comprising the following steps in order:
[0196] i) depositing a non-vitrified silicon oxide layer on the inner surface of the hollow substrate tube by means of an inner plasma reaction zone having first reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation;
[0197] ii) depositing a vitrified silica layer on the inner surface of the non-vitrified silica layer deposited in step i) inside the hollow substrate tube by means of an inner plasma reaction zone having second reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation to form at least an inner optical cladding layer and an optical core layer from the periphery to the center;
[0198] iii) removing the hollow substrate tube from the vitrified silica layer deposited in step ii) and the non-vitrified silica layer deposited in step i) to obtain a deposited tube;
[0199] iv) shrinking the deposited tube obtained in step iii) to obtain a deposited rod including at least one inner optical cladding and an optical core from the periphery to the center;
[0200] v) preparing the intermediate layer by: * depositing a non-vitrified silica layer on the outer side surface of the deposited rod obtained in step iv) by a flame hydrolysis process in an outer reaction zone using a glass-forming precursor, and subsequently; * drying and consolidating the non-vitrified silica layer into a vitrified fluorine-doped silica intermediate cladding; thereby providing a solid rod comprising, from the periphery to the center, an intermediate layer, at least one inner optical cladding and an optical core; wherein a fluorine-containing gas is used during deposition and / or drying and / or consolidation, and wherein the intermediate layer has a ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core of at least 3.5;
[0201] vi) depositing natural silicon oxide on the outer side surface of the intermediate cladding of the solid rod obtained in step v) by melting natural silicon oxide particles in an outer deposition zone to produce an outer cladding, thereby obtaining a preform.
[0202] 39. A method for manufacturing a preform for optical fiber, the method comprising the following steps in order:
[0203] a) depositing a non-vitrified silicon oxide layer on the inner surface of the hollow substrate tube by means of an inner plasma reaction zone having first reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation;
[0204] b) depositing a vitrified silica layer on the inner surface of the non-vitrified silica layer deposited in step a) inside the hollow substrate tube by means of an inner plasma reaction zone having second reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation to form at least an inner optical cladding layer and an optical core layer from the periphery to the center;
[0205] c) removing the hollow substrate tube from the vitrified silica layer deposited in step b) and the non-vitrified silica layer deposited in step a) to obtain a deposited tube;
[0206] d) preparing the intermediate layer by the following steps: * depositing a non-vitrified silica layer on the outer side surface of the deposition tube obtained in step c) by flame hydrolysis process in an outer reaction zone using a glass forming precursor, and subsequently; * drying and consolidating the non-vitrified silica layer into a vitrified fluorine-doped silica intermediate cladding; and * shrinking; thereby providing a solid rod comprising the intermediate layer, at least one inner optical cladding and an optical core from the periphery to the center; wherein a fluorine-containing gas is used during deposition and / or drying and / or consolidation, and wherein the intermediate layer has a ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core of at least 3.5;
[0207] e) depositing natural silicon oxide on the outer side surface of the intermediate cladding of the solid rod obtained in step d) by melting natural silicon oxide particles in an outer deposition zone to produce an outer cladding, thereby obtaining a preform.
[0208] 40. A method for manufacturing a preform for an optical fiber, the method comprising the following steps in order: i) depositing a non-vitrified silica layer on the inner surface of a hollow substrate tube; ii) depositing a vitrified silica layer on the inner surface of the non-vitrified silica layer deposited in step i) inside the hollow substrate tube; iii) removing the hollow substrate tube from the vitrified silica layer deposited in step ii) and the non-vitrified silica layer deposited in step i) to obtain a deposited tube; iv) optionally, shrinking the deposited tube obtained in step iii) to obtain a deposited rod including at least one inner optical cladding and an optical core from the periphery to the center; v) preparing an intermediate layer by the following steps: * depositing the non-vitrified silica layer on the inner surface of the non-vitrified silica layer deposited in step i) using a glass-forming precursor by a flame hydrolysis process in an outer reaction zone; ii) or on the outer side surface of the deposited tube obtained in step iv) or on the deposited rod obtained in step iv), and subsequently; * drying and consolidating the non-vitrified silica layer to form a vitrified fluorine-doped silica intermediate cladding; and * shrinking with the previous step iv) omitted; thereby providing a solid rod comprising, from the periphery to the center, an intermediate layer, at least one inner optical cladding and an optical core; wherein a fluorine-containing gas is used during deposition and / or drying and / or consolidation, and wherein the intermediate layer has a ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core of at least 3.5; vi) depositing natural silica on the outer side surface of the intermediate cladding of the solid rod obtained in step v) by melting natural silica particles in an outer deposition zone to produce an outer cladding, thereby obtaining a preform.
Claims
1. A method for manufacturing a preform for an optical fiber, the method comprising the following steps in order: i) depositing a non-vitrified silicon oxide layer on the inner surface of the hollow substrate tube by means of an inner plasma reaction zone having first reaction conditions generated inside the hollow substrate tube by means of electromagnetic radiation; ii) depositing a vitrified silica layer on the inner surface of the non-vitrified silica layer deposited in step i) inside the hollow substrate tube by generating an inner plasma reaction zone having second reaction conditions inside the hollow substrate tube by means of electromagnetic radiation to form at least an inner optical cladding layer and an optical core layer from the periphery to the center; iii) removing the hollow substrate tube from the vitrified silica layer deposited in step ii) and the non-vitrified silica layer deposited in step i) to obtain a deposited tube; iv) optionally, shrinking the deposited tube obtained in step iii) to obtain a deposited rod comprising, from the periphery to the center, at least one inner optical cladding and an optical core; v) preparing the intermediate layer by the following steps: * depositing a non-vitrified silicon oxide layer on the outer side surface of the deposition tube obtained in step iii) or the deposition rod obtained in step iv) using a glass-forming precursor in an outer reaction zone by a flame hydrolysis process, and subsequently; * drying and consolidating the non-vitrified silica layer into a vitrified fluorine-doped silica intermediate cladding, wherein a fluorine-containing gas is used during the drying of the non-vitrified silica layer; and *Contraction without omitting the previous step iv); thereby providing a solid rod comprising, from the periphery to the center, the intermediate layer, at least one inner optical cladding and an optical core; wherein a fluorine-containing gas is used during deposition and / or drying and / or consolidation, and wherein the intermediate layer has a ratio between the outer diameter (C) of the intermediate cladding and the outer diameter (A) of the optical core of at least 3.5; vi) depositing natural silicon oxide on the outer side surface of the intermediate cladding of the solid rod obtained in step v) by melting natural silicon oxide particles in an outer deposition zone to produce an outer cladding, thereby obtaining a preform, wherein the natural silicon oxide particles have an iron content greater than 0 ppm and less than 0.1 ppm, and the absolute difference in refractive index between the intermediate cladding and the outer cladding is between 0 and 1×10 -3 between, The simultaneous drying and doping of the non-vitrified glass layer with fluorine occur by heating the entire deposition tube or deposition rod at a temperature of 1000° C. to 1350° C. and by exposing the deposition tube or deposition rod to an atmosphere containing a chlorine-containing gas and a fluorine-containing gas, wherein the non-vitrified glass layer is included on the outer surface of the deposition tube or deposition rod.
2. The method of claim 1, wherein the intermediate layer is doped with at least 1100 ppm of fluorine.
3. The method according to claim 1 or 2, wherein the fluorine-containing gas is used during consolidation of the non-vitrified silicon oxide layer in step v), and / or wherein the fluorine-containing gas is selected from the group consisting of SiF4, SF6, CF4, and C2F6.
4. The method according to claim 3, wherein the fluorine-containing gas is selected from the group consisting of SF6 and C2F6.
5. The method of claim 1 or 2, wherein the C / A ratio is at least 4.
0.
6. The method according to claim 1 or 2, wherein the glass-forming precursor used in step v) is a gaseous silicon precursor.
7. The method according to claim 6, wherein the glass-forming precursor used in step v) is silicon tetrahalide or has the formula [(CH3)2SiO] y wherein y is 4, 5 or 6.
8. The method according to claim 6, wherein the glass-forming precursor used in step v) is SiCl4 or octamethylcyclotetrasiloxane.
9. The method according to claim 1 or 2, wherein step ii) comprises depositing one or more layers of vitrified fluorine-doped silicon oxide, wherein the refractive index difference between the vitrified fluorine-doped silicon oxide and the undoped silicon oxide is within -1×10 -3 and -10×10 -3 between.
10. The method according to claim 1 or 2, wherein a plasma flame is used for the deposition of native silicon oxide in step vi).
11. The method according to claim 1 or 2, wherein: The content of the fluorine-containing gas in the atmosphere is 0.01 volume % to 0.50 volume %.
12. The method according to claim 11, wherein: After simultaneous drying and doping with fluorine of the non-vitrified glass layer, the non-vitrified glass layer is consolidated at a consolidation temperature of 1500° C. to 1650° C.
13. A preform obtained or obtainable by a method according to any one of the preceding claims.
14. An optical fiber obtained by drawing the preform according to claim 13.
15. The optical fiber according to claim 14, which is a single-mode optical fiber.
16. An optical fiber according to claim 14 or 15, wherein the outer diameter of the optical core is between 8 and 10 microns.
17. The optical fiber of claim 14 or 15, wherein the outer diameter of the inner optical cladding is between 16 and 24 microns.
18. The optical fiber of claim 14 or 15, wherein the outer diameter of the intermediate layer is between 28 and 40 microns.
19. The optical fiber according to claim 14 or 15, wherein the diameter of the outer cladding is between 100 and 150 microns.