Silver-based composite transparent conductive film and preparation method thereof

By sputtering on a transparent substrate to form a transparent oxide layer, an island-shaped ultra-thin silver layer and a metal layer, the problem of increasing square resistance and decreasing light transmittance is solved, and a lower square resistance is achieved and higher light transmittance, and more flexible process parameters.

CN118908591APending Publication Date: 2024-11-08GUANGDONG COMM POLYTECHNIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411084247.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the silver film thickness is too low, which leads to an issue where the square resistance of the conductive film increases and the light transmittance decreases.

Method used

Using a method of preparing a silver-based composite transparent conductive film, the transparent oxide layer, an island-shaped ultra-thin silver layer, a metal layer and a second transparent oxide layer are formed by sputtering on a transparent substrate in turn, and the metal layer is connected to the isolated The silver island reduces the surface roughness and forms an interference effect through the difference in refractive index between the silver and the metal layer to improve the light transmittance.

Benefits of technology

It effectively reduces the square resistance of the conductive film, improves the light transmittance, and makes the process parameters more flexible and changeable, achieving better light transmittance than the traditional transparent oxide-metal-transparent oxide structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908591A_ABST
    Figure CN118908591A_ABST
Patent Text Reader

Abstract

The invention provides a silver-based composite transparent conductive film and a preparation method thereof. The preparation method comprises the following steps: cleaning a transparent substrate and putting the transparent substrate into a magnetron sputtering cavity filled with a silver target material, a metal target material and an oxide target material; a first transparent oxide layer, an island-shaped ultrathin silver layer, a metal layer (connecting the island-shaped ultrathin silver layer) and a second transparent oxide layer are sequentially formed on a transparent substrate through sputtering. Wherein the ultrathin silver thin film and the metal thin film play a key role in conductivity, and isolated silver islands are connected by utilizing a deposited metal layer, so that the surface roughness is reduced, and the sheet resistance is reduced. Meanwhile, on an ultrathin silver film / metal film interface, due to the refractive index difference between silver and deposited metal, an interference effect can be formed, so that light reflection is reduced, and the light transmittance is increased. And the ultrathin silver film and the metal film are relatively independent in deposition, so that process parameters are flexible and changeable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive film preparation, and in particular to a silver-based composite transparent conductive film and a preparation method thereof. Background Art

[0002] Transparent conductive films have the characteristics of high visible light transmittance and low square resistance, making them widely used in flat panel displays, solar cells, light-emitting diodes, electrochromic and other fields. At present, the transparent conductive film used in large-scale commercial applications is mainly indium tin oxide (ITO), but because ITO contains a large amount of scarce element indium, its cost is relatively high. At the same time, indium is toxic and can cause harm to the human body. At the same time, in order to obtain good electrical and optical properties, ITO needs to undergo high-temperature crystallization treatment. In addition, it has a certain degree of brittleness and is difficult to be used in the field of flexible electronics. Therefore, there are currently a lot of studies to seek to replace ITO transparent conductive films. At present, researchers have proposed a three-layer composite transparent conductive film with a transparent oxide-metal-transparent oxide structure, which is expected to replace ITO. This structure uses the high conductivity of the intermediate metal layer to keep the square resistance of the composite transparent conductive film at a low value. At the same time, by adjusting the thickness of the transparent oxide and metal layers, the interference effect is enhanced, thereby increasing the transmittance. Silver (Ag) is the most conductive material among metals, but it also absorbs light, so its thickness needs to be strictly controlled. However, due to the three-dimensional growth mode of the Ag film, when the thickness is less than 8nm, the Ag film forms an island shape and is discontinuous, which leads to increased scattering of carriers and photons, increased square resistance, and decreased transmittance. Summary of the invention

[0003] The purpose of the present invention is to provide a silver-based composite transparent conductive film and a preparation method thereof, which can solve the problem in the prior art that when the thickness of the silver film is too low, an island shape is formed, which increases the square resistance of the conductive film and reduces the transmittance.

[0004] The objective of the present invention is achieved through the following technical solutions: In a first aspect, the present invention provides a method for preparing a silver-based composite transparent conductive film, comprising the following steps: Step 1, clean the transparent substrate and place it in a magnetron sputtering chamber equipped with a silver target, a metal target and an oxide target; the silver target and the metal target are installed at the DC sputtering target position, and the oxide target is installed at the RF sputtering target position; Step 2: Pump the vacuum degree of the magnetron sputtering chamber to 5×10 -4 Pa, the temperature of the transparent substrate is maintained at room temperature, and then argon gas is introduced into the sputtering gas, and the pressure is controlled in the range of 0.5Pa~1Pa, and a first transparent oxide layer of 15nm~50nm is sputtered; an island-shaped ultra-thin silver layer of 4nm~8nm is sputtered on the first transparent oxide layer; Step 3: Continue to sputter on the island-shaped ultra-thin silver layer to form a 0.5nm~2nm metal layer to connect the island-shaped silver layers; and then sputter on the metal layer to form a second transparent oxide layer of 15nm~50nm.

[0005] Furthermore, the metal layer is a metal titanium layer or a metal aluminum layer.

[0006] Furthermore, the transparent substrate is one of soda-lime glass, high-aluminum glass and high-borosilicate glass.

[0007] Furthermore, the oxide target is one of a pure zinc oxide target, a pure tin oxide target, a zinc oxide doped target, and a tin oxide doped target.

[0008] Furthermore, the sputtering power of the island-shaped ultra-thin silver layer is 60W~80W.

[0009] Furthermore, the sputtering power of the metal layer is 20W~50W.

[0010] Furthermore, the sputtering power of the first transparent oxide layer and the second transparent oxide layer is 80W-150W.

[0011] In a second aspect, the present invention provides a silver-based composite transparent conductive film, which is prepared according to the above-mentioned preparation method, and includes a first transparent oxide layer, an island-shaped ultra-thin silver layer, a metal layer, and a second transparent oxide layer, which are sequentially sputtered on a transparent substrate.

[0012] Furthermore, the sputtering target material of the first transparent oxide layer and the second transparent oxide layer is one of oxide targets such as a pure zinc oxide target material, a pure tin oxide target material, and a tin oxide dopant target material.

[0013] Furthermore, the metal layer is a metal aluminum layer or a metal titanium layer.

[0014] The silver-based composite transparent conductive film and preparation method thereof of the present invention forms a four-layer composite film through a transparent oxide film, an ultra-thin silver film, a metal film and a transparent oxide film, wherein the ultra-thin silver film and the metal film play a key role in the conductive performance, and the deposited metal layer is used to connect the isolated silver islands, thereby reducing the surface roughness and reducing the square resistance. At the same time, at the interface of the ultra-thin silver film / metal film, due to the difference in refractive index between silver and the deposited metal, an interference effect can also be formed, thereby reducing the reflection of light and increasing the light transmittance.

[0015] In addition, in order to suppress the island growth of Ag, the prior art usually adopts a co-sputtering method to introduce other metals during the sputtering of Ag. However, the co-sputtering method has requirements on the content of the metal co-sputtered with Ag. Therefore, once the process parameters of sputtering Ag change, the process parameters of the co-sputtered metal must also be adjusted accordingly, resulting in the preparation process being not flexible and changeable. In the preparation method of the present invention, the deposition of ultra-thin silver film and metal film is relatively independent, so the process parameters are flexible and changeable. At the same time, due to the addition of an ultra-thin silver film / metal film, by adjusting the corresponding parameters, a better transmittance can be obtained compared to the three-layer composite transparent conductive film of the traditional transparent oxide-metal-transparent oxide structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The transmittance spectra of the transparent conductive film prepared according to the preparation method of Example 1 of the present invention and the transparent conductive film of the prior art in the visible light range; Figure 2 A comparison diagram of the sheet resistance change between a transparent conductive film prepared according to the preparation method of Example 1 of the present invention and a transparent conductive film in the prior art; Figure 3 The transmittance spectra of the transparent conductive film prepared according to the preparation method of the second embodiment of the present invention and the transparent conductive film of the prior art in the visible light range; Figure 4 A comparison diagram of the sheet resistance change between a transparent conductive film prepared according to the preparation method of Example 2 of the present invention and a transparent conductive film in the prior art; Figure 5 It is a diagram of the preparation process of the silver-based composite transparent conductive film preparation method of the present invention. DETAILED DESCRIPTION

[0017] The embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.

[0018] The following describes the embodiments of the present disclosure through specific examples, and those skilled in the art can easily understand other advantages and effects of the present disclosure from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present disclosure, rather than all of the embodiments. The present disclosure can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present disclosure. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present disclosure.

[0019] Embodiment 1 A method for preparing a silver-based composite transparent conductive film comprises the following steps: Step 1: ultrasonically clean and dry the transparent substrate in deionized water, alcohol, and acetone in turn, with each ultrasonic cleaning time being 30 minutes, and then place it in a magnetron sputtering chamber equipped with a silver target, a metal aluminum target, and an aluminum-doped zinc oxide target (AZO).

[0020] The silver target and the metal aluminum target are installed in the DC sputtering target position, and the aluminum-doped zinc oxide target AZO is installed in the RF sputtering target position. The mass ratio of aluminum oxide to zinc oxide in the AZO target is 2:98.

[0021] The aluminum-doped zinc oxide target can be replaced by one of the oxide targets such as a pure zinc oxide target, a pure tin oxide target, a tin oxide dopant target, etc.

[0022] The metal aluminum target can be replaced by a metal titanium target.

[0023] Step 2: Pump the background vacuum of the magnetron sputtering chamber to 5×10 -4 Pa, the substrate temperature is kept at room temperature, and then argon gas is introduced with a flow rate of 30 sccm and a pressure of about 1 Pa. A 25nm first transparent aluminum-doped zinc oxide layer is formed by sputtering; and a 6nm island-shaped ultra-thin silver layer is formed on the first transparent aluminum-doped zinc oxide layer by sputtering.

[0024] Step 3: Continue to sputter on the island-shaped ultra-thin silver layer to form a 1 nm metal aluminum layer to connect the island-shaped ultra-thin silver layer; and then sputter on the metal aluminum layer to form a second transparent zinc oxide layer of 25 nm.

[0025] The thickness of the first transparent aluminum-doped zinc oxide layer and the second transparent aluminum-doped zinc oxide layer can be the same or different. The thickness is within the range of 15nm to 50nm, which can achieve the purpose of the present invention.

[0026] Furthermore, the sputtering power of the first transparent aluminum-doped zinc oxide layer and the second transparent aluminum-doped zinc oxide layer is 80 W, and the sputtering time is 600 s, the sputtering power of the island-shaped ultra-thin silver layer is 60 W, and the sputtering time is 20 s, and the sputtering power of the metal aluminum layer is 20 W, and the sputtering time is 20 s, thereby preparing a transparent zinc oxide layer / island-shaped ultra-thin silver layer / metal aluminum layer / transparent zinc oxide layer (AZO / Ag / Al / AZO) composite transparent conductive film.

[0027] A silver-based composite transparent conductive film is prepared according to the above preparation method, comprising a first transparent aluminum-doped zinc oxide layer, an island-shaped ultra-thin silver layer, a metal aluminum layer, and a second transparent aluminum-doped zinc oxide layer, which are sequentially sputtered on a transparent substrate.

[0028] In order to compare the superiority of the preparation method of the present invention and the conductive film prepared according to the preparation method, the first transparent aluminum-doped zinc oxide layer / silver-aluminum co-sputtering layer / second transparent aluminum-doped zinc oxide layer (AZO / Ag~Al / AZO) conductive film of the prior art and the transparent aluminum-doped zinc oxide layer / island-shaped ultra-thin silver layer / metal aluminum layer / transparent aluminum-doped zinc oxide layer (AZO / Ag / Al / AZO) conductive film of the present invention were prepared with the same sputtering parameters, and the transmittance and square resistance test experiments were performed on them respectively. Ag~Al represents the film layer formed when silver and aluminum are co-sputtered.

[0029] Figure 1 The transmittance spectra of the conductive film AZO / Ag / Al / AZO of the first embodiment of the present invention, the conductive film AZO / Al-Ag / AZO of the prior art, and the conductive film AZO / Ag / AZO of the prior art in the visible light range are shown in Figure 1. The average transmittance of the conductive film of the present invention in the visible light range is 86.3%, 79.4%, and 73.8%, respectively. It is obvious that the conductive film AZO / Ag / Al / AZO of the present invention has a better transmittance.

[0030] Figure 2 The comparison diagram of the square resistance change of the conductive film AZO / Ag / Al / AZO of Example 1 of the present invention, the conductive film AZO / Al-Ag / AZO of the prior art, and the conductive film AZO / Ag / AZO of the prior art shows that, although co-sputtering can reduce the square resistance, the preparation method of the present invention can obtain lower square resistance in comparison.

[0031] comprehensive Figure 1 and Figure 2 The results show that the preparation method of the present invention can improve both the optical and electrical properties.

[0032] The present invention discloses a preparation method for improving the performance of an ultra-thin silver-based three-layer composite transparent conductive film, which comprises sputtering a first transparent aluminum-doped oxide layer, an ultra-thin silver layer, a metal layer, and a second transparent aluminum-doped oxide layer in sequence. The ultra-thin silver layer and the metal layer play a key role in the conductive performance. Since the ultra-thin silver layer of 4nm to 8nm is in an island shape, it is necessary to sputter a metal layer of 0.5nm to 2nm to connect the isolated Ag islands, thereby reducing the roughness and lowering the square resistance. At the same time, the difference in refractive index between the ultra-thin silver layer and the metal layer also provides the possibility of further improving the transmittance by utilizing the interference effect. The bottom and top transparent oxide layers are also for increasing the transmittance by utilizing the interference effect.

[0033] Embodiment 2 A method for preparing a silver-based composite transparent conductive film comprises the following steps: Step 1: ultrasonically clean and dry the transparent substrate in deionized water, alcohol and acetone in turn, with each ultrasonic cleaning time being 30 minutes, and then place it in a magnetron sputtering chamber equipped with a silver target, a metal titanium target and a pure zinc oxide target.

[0034] The silver target and the metal titanium target are installed in the DC sputtering target position, and the pure zinc oxide target is installed in the RF sputtering target position.

[0035] Step 2: Pump the background vacuum of the magnetron sputtering chamber to 5×10 -4 Pa, the substrate temperature is kept at room temperature, and then argon gas is introduced into the sputtering gas, the flow rate is controlled at 30 sccm, and the pressure is controlled at about 0.5 Pa. A 15nm first transparent zinc oxide layer is sputtered, and a 4nm island-shaped ultra-thin silver layer is sputtered on the first transparent zinc oxide layer.

[0036] Step 3: Continue to sputter to form a 0.5 nm metal titanium layer on the island-shaped ultra-thin silver layer to connect the island-shaped ultra-thin silver layer; and then sputter to form a second transparent zinc oxide layer of 15 nm on the metal titanium layer.

[0037] Furthermore, the sputtering power of the first transparent zinc oxide layer and the second transparent zinc oxide layer is 120W, and the sputtering time is 400s, the sputtering power of the island-shaped ultra-thin silver layer is 70W, and the sputtering time is 15s, and the sputtering power of the metal titanium layer is 30W, and the sputtering time is 20s, thereby preparing a transparent zinc oxide layer / island-shaped ultra-thin silver layer / metal titanium layer / transparent zinc oxide layer (ZnO / Ag / Ti / ZnO) composite transparent conductive film. There are some inevitable connections between sputtering power and sputtering time. For example, if the power is high, the sputtering time can be slightly shorter, and if the power is low, the sputtering time can be longer. The specific values ​​of sputtering power and sputtering time should not be used as limitations on the scope of protection of the present invention.

[0038] A silver-based composite transparent conductive film is prepared according to the above preparation method, comprising a first transparent zinc oxide layer, an island-shaped ultra-thin silver layer, a metal titanium layer, and a second transparent zinc oxide layer, which are sequentially sputtered on a transparent substrate.

[0039] Figure 3 The transmittance spectra of the conductive film ZnO / Ag / Ti / ZnO of the second embodiment of the present invention, the conductive film ZnO / Ti-Ag / ZnO of the prior art, and the conductive film ZnO / Ag / ZnO of the prior art in the visible light range. Figure 4A comparison chart of the square resistance change of the conductive film ZnO / Ag / Ti / ZnO of the second embodiment of the present invention, the conductive film ZnO / Ti-Ag / ZnO of the prior art, and the conductive film ZnO / Ag / ZnO of the prior art in the visible light range. Obviously, the conductive film of the present invention has a lower square resistance and a higher light transmittance. Since its light transmittance is slightly lower than that of the prior art ZnO / Ti-Ag / ZnO, we use the most common evaluation parameter quality factor in the field of transparent conductive films (the 10th power of the light transmittance divided by the square resistance) to measure. According to the data, the quality factors are 0.02 and 0.019, respectively, that is, the quality factor of the conductive film of the present invention is higher than the quality factor of the prior art ZnO / Ti-Ag / ZnO, indicating that the comprehensive optical and electrical properties of the conductive film of the present invention are better than the optical and electrical properties of the prior art ZnO / Ti-Ag / ZnO.

[0040] Embodiment 3 A method for preparing a silver-based composite transparent conductive film comprises the following steps: Step 1: ultrasonically clean and dry the transparent substrate in deionized water, alcohol and acetone in turn, with each ultrasonic cleaning time being 30 minutes, and then place it in a magnetron sputtering chamber equipped with a silver target, a metal titanium target and a pure tin oxide target.

[0041] The silver target and the metal titanium target are installed in the DC sputtering target position, and the pure tin oxide target is installed in the RF sputtering target position.

[0042] Step 2: Pump the background vacuum of the magnetron sputtering chamber to 5×10 -4 Pa, the substrate temperature is kept at room temperature, and then sputtering gas argon is introduced, with its flow rate controlled at 30sccm and pressure controlled at about 0.5Pa. A 50nm first transparent tin oxide layer is sputtered, and an 8nm island-shaped ultra-thin silver layer is sputtered on the first transparent tin oxide layer.

[0043] Step 3: Continue to sputter to form a 2nm metal titanium layer on the island-shaped ultra-thin silver layer to connect the island-shaped ultra-thin silver layer; and then sputter to form a second transparent tin oxide layer of 50nm on the metal titanium layer.

[0044] Furthermore, the sputtering power of the first transparent tin oxide layer and the second transparent tin oxide layer is 150 W, and the sputtering time is 600 s, the sputtering power of the island-shaped ultra-thin silver layer is 80 W, and the sputtering time is 20 s, and the sputtering power of the metal titanium layer is 50 W, and the sputtering time is 40 s, thereby preparing a transparent tin oxide layer / island-shaped ultra-thin silver layer / metal titanium layer / transparent tin oxide layer (SnO / Ag / Ti / SnO) composite transparent conductive film.

[0045] A silver-based composite transparent conductive film is prepared according to the above preparation method, comprising a first transparent tin oxide layer, an island-shaped ultra-thin silver layer, a metal titanium layer, and a second transparent tin oxide layer, which are sequentially sputtered on a transparent substrate.

[0046] The conductive film SnO prepared in this example 2 / Ag / Ti / SnO 2 The average transmittance in the visible light range is 83.7%, while the conductive film SnO 2 / Ag-Ti / SnO 2 And the conductive film SnO 2 / Ag / SnO 2 The average transmittances of SnO 2 / Ag / Ti / SnO 2 The square resistance (10.7Ω / sq.) is smaller than SnO 2 / Ag-Ti / SnO 2 The square resistance (11.5Ω / sq.) and the conductive film SnO 2 / Ag / SnO 2 Square resistance (12.8Ω / sq.). The above is only for explaining the implementation mode of the present invention and is not intended to limit the present invention. For those skilled in the art, any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention without creative work should be included in the protection scope of the present invention.

Claims

1. A method for preparing a silver-based composite transparent conductive film, characterized in that: The following steps are involved: Step 1, clean the transparent substrate and place it in a magnetron sputtering chamber equipped with a silver target, a metal target and an oxide target; the silver target and the metal target are installed at the DC sputtering target position, and the oxide target is installed at the RF sputtering target position; Step 2: Pump the vacuum degree of the magnetron sputtering chamber to 5×10 -4 Pa, the temperature of the transparent substrate is maintained at room temperature, and then argon gas is introduced into the sputtering gas, and the pressure is controlled in the range of 0.5Pa~1Pa, and a first transparent oxide layer of 15nm~50nm is sputtered; an island-shaped ultra-thin silver layer of 4nm~8nm is sputtered on the first transparent oxide layer; Step 3: Continue to sputter on the island-shaped ultra-thin silver layer to form a 0.5nm~2nm metal layer to connect the island-shaped silver layers; and then sputter on the metal layer to form a second transparent oxide layer of 15nm~50nm.

2. The method for preparing the silver-based composite transparent conductive film according to claim 1, characterized in that: The metal layer is a metal titanium layer or a metal aluminum layer.

3. The method for preparing the silver-based composite transparent conductive film according to claim 1, characterized in that: The transparent substrate is one of soda-lime glass, high-aluminum glass and high-borosilicate glass.

4. The method for preparing the silver-based composite transparent conductive film according to claim 1, characterized in that: The oxide target is one of a pure zinc oxide target, a pure tin oxide target, a zinc oxide dopant target, and a tin oxide dopant target.

5. The method for preparing the silver-based composite transparent conductive film according to claim 1, characterized in that: The sputtering power of the island-shaped ultra-thin silver layer is 60W-80W.

6. The method for preparing the silver-based composite transparent conductive film according to claim 1, characterized in that: The sputtering power of the metal layer is 20W-50W.

7. The method for preparing the silver-based composite transparent conductive film according to claim 1, characterized in that: The sputtering power of the first transparent oxide layer and the second transparent oxide layer is 80W-150W.

8. A silver-based composite transparent conductive film, characterized in that: The method according to any one of claims 1 to 7 comprises a first transparent oxide layer, an island-shaped ultra-thin silver layer, a metal layer, and a second transparent oxide layer which are sequentially sputtered on a transparent substrate.

9. The silver-based composite transparent conductive film according to claim 8, characterized in that: The sputtering target material of the first transparent oxide layer and the second transparent oxide layer is one of oxide target materials such as a pure zinc oxide target material, a pure tin oxide target material, and a tin oxide dopant target material.

10. The silver-based composite transparent conductive film according to claim 8, characterized in that: The metal layer is a metal aluminum layer or a metal titanium layer.