Fireproof anti-crack cement guniting plugging support material and preparation method thereof

Through the combination of nano-silica-coated glass fiber and corundum, the problem of insufficient strength and crack resistance of cement spray sealing materials is solved, and excellent fire resistance and crack resistance are achieved, and the compressive strength is achieved in 7 days. 32.4-46.2MPa, the compressive strength reaches 53.8-72.9MPa in 28 days, and maintains good performance at high temperatures.

CN118908666APending Publication Date: 2024-11-08SHANDONG DESHENG MINING ENG MATERIALS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411157130.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The cement spray sealing material has low strength, poor crack resistance and poor fire resistance.

Method used

Using nano-silica-coated glass fiber as an additive for cement spray sealing material, glass fibers are treated with hydrochloric acid and generated nano-silica on their surface, improving the toughness and mechanical strength of the fibers, and combining corundum and acrylic resin emulsion Make mixing.

Benefits of technology

It significantly improves the strength and crack resistance of cement spray sealing materials, improves the fire resistance and fire resistance, and the compressive strength reaches 32.4-46.2MPa in 7 days, the compressive strength reaches 53.8-72.9MPa in 28 days, and the burning is at 1200℃. After the production, maintain high compressive strength and extend the cracking time to 42-52 hours.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005319860000061
    Figure BDA0005005319860000061
  • Figure BDA0005005319860000071
    Figure BDA0005005319860000071
  • Figure BDA0005005319860000072
    Figure BDA0005005319860000072
Patent Text Reader

Abstract

The invention belongs to the technical field of cement, and discloses a fireproof anti-crack cement guniting plugging support material and a preparation method thereof, the fireproof anti-crack cement guniting plugging support material comprises 30-40 parts by weight of cement, 45-55 parts by weight of sand, 15-20 parts by weight of water, 3-10 parts by weight of corundum, 6-15 parts by weight of an acrylic resin emulsion, and 1.2-3 parts by weight of nano-silica coated glass fiber. The nano-silica coated glass fiber and corundum are used as additives of the cement guniting plugging material, the nano-silica coated glass fiber has better toughness and mechanical strength, the strength of the cement guniting plugging material can be improved, and the fused white corundum and tabular corundum have very strong fire resistance, so that the cement guniting plugging material has good fire resistance. Therefore, the cement guniting plugging material has excellent strength, fire resistance and cracking resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cement, and in particular relates to a fireproof and crack-resistant cement grouting plugging and supporting material and a preparation method thereof. Background Art

[0002] Cement is widely used in concrete structure crack repair, plugging, and leak plugging. It is of great significance to improve the strength, crack resistance, fire resistance, and other properties of cement. Adding additives such as fiber, slag, and polymer solution to cement can effectively improve the performance of cement. Among them, glass fiber has the advantages of strong heat resistance, good corrosion resistance, and high mechanical strength. It is widely used in cement, concrete and other construction projects. However, glass fiber is brittle and has poor toughness, and the improvement of the mechanical properties of cement and other materials is limited.

[0003] Nano silicon dioxide has a large specific surface area, is cheap and easy to obtain, has high mechanical strength, and is widely used. In addition, nano silicon dioxide has good compatibility with cement, and has a good effect on improving the mechanical strength, crack resistance and other properties of cement. The present invention aims to use nano silicon dioxide to coat and improve glass fiber, thereby improving the strength and toughness of glass fiber, and as an additive for cement material, improve its low strength, crack resistance, fire resistance and other properties. Summary of the invention

[0004] The invention solves the problems of low strength, poor crack resistance, poor fire resistance and fireproof performance of cement spraying plugging materials.

[0005] The technical solution of the present invention is: a fireproof and crack-resistant cement grouting plugging and supporting material, comprising 30-40 parts by weight of cement, 45-55 parts by weight of sand, 15-20 parts by weight of water, 3-10 parts by weight of corundum, 6-15 parts by weight of acrylic resin emulsion, and 1.2-3 parts by weight of nano-silicon dioxide coated glass fiber.

[0006] Preferably, the corundum is plate-like corundum or fused white corundum.

[0007] Preferably, the preparation method of nano-silicon dioxide coated glass fiber is:

[0008] (1) The glass fiber is placed in a resistance furnace for heat preservation treatment, washed with ethanol after cooling, dried, and then immersed in a hydrochloric acid solution. After filtering, the solution is washed with water and dried to obtain a hydroxylated glass fiber.

[0009] (2) Adding hydroxylated glass fiber, ethanol, and tetraethyl silicate to ammonia water, stirring the reaction and centrifuging, washing with water and ethanol in turn, placing the product in a resistance furnace after drying, heat-insulating treatment, and cooling to obtain nano-silica coated glass fiber.

[0010] Preferably, the molar concentration of the hydrochloric acid solution in (1) is 1-3 mol / L.

[0011] Preferably, the soaking temperature in (1) is 60-90° C. and the soaking time is 3-6 h.

[0012] Preferably, the pH of the ammonia water in (2) is 9-10.

[0013] Preferably, the mass ratio of hydroxylated glass fiber to tetraethyl silicate in (2) is 1:(3-15).

[0014] Preferably, the reaction temperature in (2) is 20-30°C and the reaction time is 24-36h.

[0015] Preferably, the temperature of the heat preservation treatment in (2) is 500-600° C. and the time is 2-3 hours.

[0016] Preferably, the method for preparing the fireproof and crack-resistant cement grouting plugging and supporting material is as follows: cement, sand, water, corundum, acrylic resin emulsion, and nano-silica coated glass fiber are stirred and mixed to obtain the fireproof and crack-resistant cement grouting plugging and supporting material.

[0017] The technical effect of the present invention is as follows: the present invention uses hydrochloric acid to perform active treatment on glass fiber, introduces a large number of hydroxyl groups on the surface of the glass fiber, and then uses hydroxylated glass fiber as a carrier and tetraethyl silicate as a silicon source to generate nano-silicon dioxide on the surface of the glass fiber through a hydrolysis reaction. The hydroxyl groups on the surface of the glass fiber have good affinity with the hydroxyl groups on the surface of the nano-silicon dioxide, which can improve the dispersion performance of the nano-silicon dioxide on the surface of the fiber, so that the nano-silicon dioxide has a better coating effect on the glass fiber. After the coating modification of the nano-silicon dioxide, it is beneficial to improve the brittleness of the glass fiber and improve the toughness.

[0018] The present invention uses nano-silicon dioxide coated glass fiber and corundum as additives for cement spraying plugging materials. The nano-silicon dioxide coated glass fiber has better toughness and mechanical strength, and can improve the strength of the cement spraying plugging material. The fused white corundum and plate-shaped corundum have strong fire resistance, so that the cement spraying plugging material has excellent strength, fire resistance and crack resistance. The compressive strength reaches 32.4-46.2MPa in 7 days. The compressive strength reaches 53.8-72.9MPa in 28 days. And after being fired at 1200°C for 24h, it still has a high compressive strength retention rate, and the cracking time reaches 42-52h. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0020] Example 1

[0021] (1) 5 g of glass fiber is placed in a resistance furnace, heated to 450° C. and kept for 1 h. After cooling, it is washed with ethanol and dried. Then, it is placed in 1500 mL of a 1 mol / L hydrochloric acid solution and soaked at 90° C. for 3 h. During the soaking process, it is condensed and refluxed. After filtering, it is washed with water and dried to obtain hydroxylated glass fiber.

[0022] (2) Add 4 g of hydroxylated glass fiber, 2500 mL of ethanol, and 60 g of tetraethyl silicate to 300 mL of ammonia water with a pH of 9, stir and react at 25° C. for 24 h, centrifuge, wash with water and ethanol in turn, and place the product in a resistance furnace after drying, heat it to 500° C., keep it warm for 3 h, and cool it to obtain nano-silica coated glass fiber.

[0023] (3) 350 g of PO42.5 cement, 450 g of sand, 200 g of water, 30 g of plate-shaped corundum, 120 g of acrylic resin emulsion (solid content 52%), and 12 g of nano-silica-coated glass fiber were stirred and mixed for 5 min to obtain a fire-resistant and crack-resistant cement spraying plugging support material.

[0024] Example 2

[0025] (1) 5 g of glass fiber is placed in a resistance furnace, heated to 450° C. and kept for 1 h. After cooling, it is washed with ethanol and dried. Then, it is placed in 1500 mL of a 3 mol / L hydrochloric acid solution and soaked at 80° C. for 3 h. During the soaking process, it is condensed and refluxed. After filtering, it is washed with water and dried to obtain hydroxylated glass fiber.

[0026] (2) Add 4 g of hydroxylated glass fiber, 2500 mL of ethanol, and 48 g of tetraethyl silicate to 400 mL of ammonia water with a pH of 9, stir and react at 20° C. for 36 h, centrifuge, wash with water and ethanol in turn, and place the product in a resistance furnace after drying, heat it to 550° C., keep it warm for 3 h, and cool it to obtain nano-silica coated glass fiber.

[0027] (3) 300 g of PO42.5 cement, 550 g of sand, 200 g of water, 100 g of fused white corundum, 60 g of acrylic resin emulsion (solid content 52%), and 25 g of nano-silica coated glass fiber were stirred and mixed for 5 min to obtain a fire-resistant and crack-resistant cement spraying plugging support material.

[0028] Example 3

[0029] (1) 5 g of glass fiber is placed in a resistance furnace, heated to 450° C. and kept for 1 h. After cooling, it is washed with ethanol and dried. Then, it is placed in 1500 mL of a 2 mol / L hydrochloric acid solution and soaked at 90° C. for 4 h. During the soaking process, it is condensed and refluxed. After filtering, it is washed with water and dried to obtain hydroxylated glass fiber.

[0030] (2) 4 g of hydroxylated glass fiber, 2000 mL of ethanol, and 36 g of tetraethyl silicate were added to 350 mL of ammonia water with a pH of 10, and the mixture was stirred at 30° C. for 24 h. The mixture was centrifuged and washed with water and ethanol in turn. After drying, the product was placed in a resistance furnace, heated to 500° C., kept warm for 3 h, and cooled to obtain nano-silica coated glass fiber.

[0031] (3) 300 g of PO42.5 cement, 480 g of sand, 150 g of water, 60 g of fused white corundum, 90 g of acrylic resin emulsion (solid content 52%), and 30 g of nano-silica coated glass fiber were stirred and mixed for 5 min to obtain a fire-resistant and crack-resistant cement spraying plugging support material.

[0032] Example 4

[0033] (1) 5 g of glass fiber is placed in a resistance furnace, heated to 450° C. and kept for 1 h. After cooling, it is washed with ethanol and dried. Then, it is placed in 1500 mL of a 2 mol / L hydrochloric acid solution and soaked at 60° C. for 6 h. During the soaking process, it is condensed and refluxed. After filtering, it is washed with water and dried to obtain hydroxylated glass fiber.

[0034] (2) Add 4 g of hydroxylated glass fiber, 2000 mL of ethanol, and 24 g of tetraethyl silicate to 300 mL of ammonia water with a pH of 9, stir and react at 20° C. for 30 h, centrifuge, wash with water and ethanol in turn, and after drying, place the product in a resistance furnace, heat it to 500° C., keep it warm for 3 h, and cool it to obtain nano-silica coated glass fiber.

[0035] (3) 400 g of PO42.5 cement, 550 g of sand, 200 g of water, 30 g of plate-shaped corundum, 120 g of acrylic resin emulsion (solid content 52%), and 18 g of nano-silica-coated glass fiber were stirred and mixed for 10 min to obtain a fire-resistant and crack-resistant cement spraying plugging support material.

[0036] Example 5

[0037] (1) 5 g of glass fiber is placed in a resistance furnace, heated to 450° C. and kept for 1 h. After cooling, it is washed with ethanol and dried. Then, it is placed in 1500 mL of a 1 mol / L hydrochloric acid solution and soaked at 90° C. for 4 h. During the soaking process, it is condensed and refluxed. After filtering, it is washed with water and dried to obtain hydroxylated glass fiber.

[0038] (2) Add 4 g of hydroxylated glass fiber, 2000 mL of ethanol, and 12 g of tetraethyl silicate to 300 mL of ammonia water with a pH of 9, stir and react at 30° C. for 24 h, centrifuge, wash with water and ethanol in turn, and place the product in a resistance furnace after drying, heat it to 600° C., keep it warm for 2 h, and cool it to obtain nano-silica coated glass fiber.

[0039] (3) 320 g of PO42.5 cement, 480 g of sand, 200 g of water, 60 g of fused white corundum, 150 g of acrylic resin emulsion (solid content 52%), and 25 g of nano-silica coated glass fiber were stirred and mixed for 10 min to obtain a fire-resistant and crack-resistant cement spraying plugging support material.

[0040] Comparative Example 1

[0041] 350 g PO42.5 cement, 450 g sand, 200 g water, 30 g plate-shaped corundum, and 120 g acrylic resin emulsion (solid content 52%) were stirred and mixed for 5 minutes to obtain a fire-resistant and crack-resistant cement spraying plugging support material.

[0042] Comparative Example 2

[0043] (1) 5 g of glass fiber is placed in a resistance furnace, heated to 450° C. and kept for 1 h. After cooling, it is washed with ethanol and dried. Then, it is placed in 1500 mL of a 1 mol / L hydrochloric acid solution and soaked at 90° C. for 3 h. During the soaking process, it is condensed and refluxed. After filtering, it is washed with water and dried to obtain hydroxylated glass fiber.

[0044] (2) Add 4 g of hydroxylated glass fiber, 2500 mL of ethanol, and 60 g of tetraethyl silicate to 300 mL of ammonia water with a pH of 9, stir and react at 25° C. for 24 h, centrifuge, wash with water and ethanol in turn, and place the product in a resistance furnace after drying, heat it to 500° C., keep it warm for 3 h, and cool it to obtain nano-silica coated glass fiber.

[0045] (3) 350 g of PO42.5 cement, 450 g of sand, 200 g of water, 120 g of acrylic resin emulsion (solid content 52%), and 12 g of nano-silica coated glass fiber were stirred and mixed for 5 min to obtain a fire-resistant and crack-resistant cement spraying plugging support material.

[0046] Comparative Example 3

[0047] (1) 4 g of glass fiber, 2500 mL of ethanol, and 60 g of tetraethyl silicate were added to 300 mL of ammonia water with a pH of 9, and the mixture was stirred at 25° C. for 24 h, centrifuged, washed with water and ethanol in turn, and after drying, the product was placed in a resistance furnace, heated to 500° C., kept warm for 3 h, and cooled to obtain nano-silica coated glass fiber.

[0048] (2) 350 g of PO42.5 cement, 450 g of sand, 200 g of water, 30 g of plate-shaped corundum, 120 g of acrylic resin emulsion (solid content 52%), and 12 g of nano-silica-coated glass fiber were stirred and mixed for 5 min to obtain a fire-resistant and crack-resistant cement spraying plugging support material.

[0049] Pour the fireproof and crack-resistant cement shotcrete plugging support material into the mold, vibrate and compact it, and cure it at 25°C for 7-28 days after demoulding. Test the compressive strength according to GB / T 17671-2021 method.

[0050] Pour the fireproof and crack-resistant cement spraying plugging support material into the mold, vibrate and compact it, and after demoulding, cure it at 25℃ for 7-28 days, then place it in a rotary kiln, burn it at 1200℃ for 24h, and then test the compressive strength. The test results are shown in the table below.

[0051] Table 1 7d compressive strength of cement shotcrete plugging material

[0052]

[0053]

[0054] Table 2 28d compressive strength of cement shotcrete plugging material

[0055]

[0056] Pour the fire-proof and crack-resistant cement spraying sealing support material into the mold, vibrate and compact it, and oxidize it at 25°C after demoulding. Observe the cement surface every 1 hour and record the cracking time.

[0057] Table 3 Cement shotcrete plugging material cracking time

[0058]

[0059]

[0060] After testing, in Examples 1-5, nano-silicon dioxide coated glass fiber and fused white corundum were used as additives for cement spraying plugging materials, and the compressive strength reached 32.4-46.2MPa in 7 days. The compressive strength reached 53.8-72.9MPa in 28 days. And after being fired at 1200℃ for 24h, it still had a high compressive strength retention rate. And the cracking time reached 42-52h, showing excellent strength, fire resistance and cracking resistance.

[0061] Compared with Example 1, in Comparative Example 1, nano-silica-coated glass fibers were not added, and the compressive strength of the cement spraying plugging material was poor, which was significantly lower than that of Example 1.

[0062] In comparative example 2, plate-shaped corundum was not added, and after the cement spraying sealing material was fired at 1200° C., the compressive strength decreased significantly, the retention rate was very large, and the fire resistance and fireproof performance were poor.

[0063] The glass fiber of Comparative Example 3 has not been activated by hydrochloric acid, has very little hydroxyl content on the surface, and has low interfacial properties with the generated nano-silicon dioxide, resulting in the nano-silicon dioxide not being well coated on the glass fiber, and the improvement in the compressive strength of the cement material is low.

[0064] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A fireproof and crack-resistant cement spraying plugging support material, characterized in that: The fireproof and crack-resistant cement grouting plugging and supporting material comprises 30-40 parts by weight of cement, 45-55 parts by weight of sand, 15-20 parts by weight of water, 3-10 parts by weight of corundum, 6-15 parts by weight of acrylic resin emulsion, and 1.2-3 parts by weight of nano-silicon dioxide coated glass fiber.

2. The fireproof and crack-resistant cement spraying plugging support material and preparation method according to claim 1 is characterized in that: The corundum is plate-shaped corundum or fused white corundum.

3. The fireproof and crack-resistant cement spraying plugging support material according to claim 1 is characterized in that: The preparation method of the nano-silicon dioxide coated glass fiber is as follows: (1) placing the glass fiber in a resistance furnace, heat-insulating the fiber, cooling it, washing it with ethanol, drying it, and then soaking it in a hydrochloric acid solution, filtering it, washing it with water, and drying it to obtain a hydroxylated glass fiber; (2) Adding hydroxylated glass fiber, ethanol, and tetraethyl silicate to ammonia water, stirring the reaction and centrifuging, washing with water and ethanol in turn, placing the product in a resistance furnace after drying, heat-insulating treatment, and cooling to obtain nano-silica coated glass fiber.

4. The fireproof and crack-resistant cement spraying plugging support material according to claim 1 is characterized in that: The molar concentration of the hydrochloric acid solution in (1) is 1-3 mol / L.

5. The fireproof and crack-resistant cement spraying plugging and supporting material according to claim 1 is characterized in that: The soaking temperature in (1) is 60-90° C. and the soaking time is 3-6 hours.

6. The fireproof and crack-resistant cement spraying plugging support material according to claim 1 is characterized in that: The pH of the ammonia water in (2) is 9-10.

7. The fireproof and crack-resistant cement spraying plugging and supporting material according to claim 1 is characterized in that: The mass ratio of hydroxylated glass fiber to tetraethyl silicate in (2) is 1:(3-15).

8. The fireproof and crack-resistant cement spraying plugging and supporting material according to claim 1 is characterized in that: The reaction temperature in (2) is 20-30°C and the reaction time is 24-36h.

9. The fireproof and crack-resistant cement spraying plugging and supporting material according to claim 1, characterized in that: The temperature of the heat preservation treatment in (2) is 500-600°C and the time is 2-3h.

10. The method for preparing the fireproof and crack-resistant cement spraying plugging support material according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: mixing cement, sand, water, corundum, acrylic resin emulsion and nano-silicon dioxide coated glass fiber to obtain a fireproof and crack-resistant cement spraying plugging and supporting material.

Citation Information

Patent Citations

  • Crack-resistant thermal insulation mortar

    CN103708797A

  • Fire-retardant and thermal-insulation mortar

    CN103787631A

  • Concrete constant-solid high temperature resistant material and preparation method therefor

    CN105110741A

  • Anti-crack mortar

    CN109133814A

  • Mining air leakage stoppage polymer cement mortar material as well as preparation method and application thereof