Method for preparing self-leveling mortar from electrolytic manganese residues through medium-temperature calcination

By treating electrolytic manganese slag in medium temperature calcination and preparing self-leveling mortar with other materials, the problem of limited application of electrolytic manganese slag in cement-based building materials is solved, and the preparation of self-leveling mortar with efficient resource utilization and performance in accordance with standards is achieved.

CN118908675APending Publication Date: 2024-11-08GUIZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410954491.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Electrolytic manganese slag is limited in the application of cement-based building materials. Due to its high content of heavy metals such as ammonia nitrogen, sulfate and manganese, low activity, it affects product quality, and its resource utilization has not been effectively solved.

Method used

Medium-temperature calcination is used to treat electrolytic manganese slag, remove ammonia nitrogen, cure manganese ions, and activate the activity of volcanic ash. Combined with ordinary silicate cement, aluminate cement, pyrolytic electrolytic manganese slag and fine aggregates, combined with appropriate water reducing agent and boric acid Sodium, prepare cement-based self-leveling mortar for floor preparation.

Benefits of technology

The efficient resource utilization of electrolytic manganese slag has been realized. The flow and strength of the self-leveling mortar has reached industry standards. The electrolytic manganese slag can reach 30%, which reduces production costs and opens up a new way to the resources of electrolytic manganese slag. Use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908675A_ABST
    Figure CN118908675A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing self-leveling mortar through medium-temperature calcination of electrolytic manganese residues, and belongs to the technical field of self-leveling mortar preparation. Comprising the following steps: preparing pyrolysis electrolytic manganese residues: drying the electrolytic manganese residues, grinding, sieving, calcining the sieved electrolytic manganese residues in a muffle furnace, heating the muffle furnace to 800 DEG C, preserving heat for 120 minutes, calcining, and cooling to room temperature along with the furnace after calcining to obtain a medium-temperature calcined product, namely the pyrolysis electrolytic manganese residues; the preparation method comprises the following steps: mixing ordinary Portland cement, aluminate cement, pyrolyzed electrolytic manganese residues and fine aggregate in proportion to obtain a powder mixture; weighing tap water, a water reducing agent and sodium borate according to the proportion, and pouring into a stirrer; and pouring the powder mixture into a stirrer at a constant speed within 30 seconds, and stirring to obtain the cement-based self-leveling mortar prepared from the pyrolysis electrolytic manganese residues and used for the ground. The solid waste is used as the raw material, so that the production cost is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of self-leveling mortar preparation, and in particular to a method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature. Background Art

[0002] . Electrolytic manganese slag is an acidic waste residue (pH <5) produced after the manganese carbonate ore undergoes acid leaching, neutralization, and filtration during the production process. Electrolytic manganese slag contains soluble manganese, ammonia water, ammonium sulfate and other chemical agents added during the production process, as well as a large amount of pollutants such as ammonia nitrogen, zinc, copper, and chromium. For every ton of metallic manganese produced, 10-12 tons of electrolytic manganese slag will be produced. Based on the resource and environmental properties of electrolytic manganese slag, achieving breakthroughs in key technologies for its resource utilization has become a key common problem that the industry and even the entire society urgently need to solve. At present, electrolytic manganese slag cement-based building materials have not been widely used, mainly because the electrolytic manganese slag has high content and low activity of heavy metals such as ammonia nitrogen, sulfate and manganese. The preparation of cement-based materials will affect product quality. Studies have shown that electrolytic manganese slag can activate volcanic ash activity through heat treatment.

[0003] As a new type of functional building mortar with high added value, self-leveling mortar has been widely used in recent years. It is mainly used in public buildings such as factories, schools, hospitals, and office buildings. Self-leveling mortar is mainly made of a mixture of cementitious materials, aggregates, and chemical admixtures. The characteristics of self-leveling mortar are that it can level itself and has high early strength. Self-leveling mortar materials mainly include gypsum-based self-leveling mortar, cement-based self-leveling mortar, and multi-cementitious self-leveling mortar. At present, multi-cementitious calcium sulfonate self-leveling mortar is the mainstream of self-leveling materials. Electrolytic manganese slag contains a large amount of dihydrate gypsum and silicon-aluminum compounds. After calcination to activate the activity, the gypsum phase can react with cement to form calcium sulfonate, which can be used to prepare self-leveling mortar. Summary of the invention

[0004] In view of the deficiencies in the above-mentioned prior art, the present invention has conducted extensive research on the application of pyrolytic electrolytic manganese slag in self-leveling mortar, and has studied the process of preparing self-leveling mortar from calcined electrolytic manganese slag. The influence of water reducer on the performance of self-leveling mortar from calcined electrolytic manganese slag is studied, and the influence of the dosage of calcined electrolytic manganese slag on the macroscopic and microscopic properties of self-leveling mortar is studied. The process of preparing self-leveling mortar from electrolytic manganese slag is obtained. The technical problem solved by the present invention is to provide a new method for the resource utilization of electrolytic manganese slag.

[0005] To achieve its purpose, the present invention adopts the following technical solution: a method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature, comprising the following steps:

[0006] S1. Preparation of pyrolytic electrolytic manganese slag: drying the electrolytic manganese slag, grinding it, sieving it, placing it in a muffle furnace for calcination, heating it to 800° C. in the muffle furnace, keeping it warm for 120 min, cooling it to room temperature with the furnace after calcination, and obtaining a medium-temperature calcination product, pyrolytic electrolytic manganese slag;

[0007] S2, mixing ordinary Portland cement, aluminate cement, pyrolysis electrolytic manganese slag and fine aggregate according to proportion to obtain a powder mixture;

[0008] S3. Weigh tap water, water reducing agent and sodium borate in proportion and pour them into a blender;

[0009] S4. Pour the powder mixture into the mixer at a uniform speed within 30 seconds, stir at a low speed for 1 minute, stop stirring, and scrape off the uneven mixture on the stirring blades and the wall of the material pot with a scraper within 30 seconds, then stir at a high speed for 1 minute, stop for 1 minute, and continue stirring at a high speed for 15 seconds to obtain cement-based self-leveling mortar for the floor prepared from pyrolytic electrolytic manganese slag.

[0010] Preferably, in step S1: after the electrolytic manganese slag is dried, it is ground to a particle size less than 200 mesh, and the heating rate of the electrolytic manganese slag is 5° C. / min.

[0011] Preferably, in step S2: the model of ordinary Portland cement is P.O42.5R; the model of aluminate cement is CA-50.

[0012] Preferably, in step S2: the pyrolytic electrolytic manganese slag calcined at 800° C. in the cementitious material replaces cement at 10%-50%.

[0013] Preferably, in step S2, the mass ratio of silicate cement to aluminate cement is 3:2.

[0014] Preferably, in step S2, the fine aggregate is 40-80 mesh quartz sand and 80-120 mesh quartz sand, and the mortar-sand ratio is 1:1, wherein the mass ratio of 40-80 mesh quartz sand to 80-120 mesh quartz sand is 1:1.

[0015] Preferably, in step S3: the water-to-binder ratio is 0.4.

[0016] Preferably, in step S3, the water reducer is at least one of a polycarboxylate water reducer, a naphthalene-based water reducer and a sodium lignin sulfonate water reducer.

[0017] Preferably, in step S3: the sodium borate is used as a retarder, accounting for 0.05% of the total mass of the base material.

[0018] Preferably, in step S3: the amount of water reducer added is as follows: the amount of polycarboxylate water reducer added is 0.1%-0.5% of the total mass of the base material, or the amount of naphthalene water reducer added is 0.5%-1.5% of the total mass of the base material, or the amount of sodium lignin sulfonate water reducer added is 0.5%-1.5% of the total mass of the base material.

[0019] Beneficial effects of the present invention:

[0020] (1) After the electrolytic manganese slag is calcined at medium temperature, the ammonia nitrogen in the electrolytic manganese slag is effectively removed, the manganese ions are solidified, and the harm of ammonia nitrogen substances and manganese ions to the environment is effectively avoided. In addition, the volcanic ash activity of the electrolytic manganese slag is activated by calcining the electrolytic manganese slag at medium temperature.

[0021] (2) The fluidity and strength of the self-leveling mortar made from electrolytic manganese slag calcined at medium temperature can meet the requirements of the industry standard "Cement-based Self-leveling Mortar for Floors" (JC / T 985-2017).

[0022] (3) Under the condition of ensuring the fluidity and strength of the self-leveling mortar for the floor, the dosage of the electrolytic manganese slag after medium-temperature calcination can reach 30%, which greatly improves the utilization rate of the pyrolytic electrolytic manganese slag without affecting the performance of the cement-based self-leveling mortar for the floor.

[0023] (4) The present invention utilizes solid waste as raw materials, which greatly reduces production costs. In addition, it opens up a new way for the preparation of cement-based self-leveling mortar for ground use and the resource utilization of electrolytic manganese slag, and has good practicality. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] For ease of explanation, the present invention is described in detail with reference to the following specific embodiments and the accompanying drawings.

[0025] Figure 1 This is a process flow chart for preparing self-leveling mortar by pyrolysis and electrolytic manganese slag;

[0026] Figure 2 It is a schematic diagram of the fluidity of the prepared self-leveling mortar;

[0027] Figure 3 is the X-ray diffraction pattern of the prepared self-leveling mortar;

[0028] Figure 4 is a scanning electron microscope image of the prepared self-leveling mortar; DETAILED DESCRIPTION

[0029] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments; in the following description, specific details such as specific configurations are provided only to help fully understand the embodiments of the present invention. Therefore, it should be clear to those skilled in the art that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the present invention.

[0030] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0031] Unless otherwise specified, the materials, practices and experimental equipment involved in the implementation cases of the present invention are all in line with the commercially available products of the relevant chemical industry.

[0032] Example 1

[0033] As shown in the figure, a method for preparing self-leveling mortar using electrolytic manganese slag after medium-temperature calcination activation treatment includes the following steps:

[0034] (1) drying the electrolytic manganese slag, grinding it and sieving it. The sifted electrolytic manganese slag is placed in a muffle furnace for calcination. The temperature of the muffle furnace is raised to 800°C at a heating rate of 5°C / min, and the temperature is kept for 120min for calcination. After the calcination is completed, the muffle furnace is cooled to room temperature to obtain medium-temperature calcined electrolytic manganese slag;

[0035] (2) ordinary Portland cement, aluminate cement, pyrolytic electrolytic manganese slag and fine aggregate are mixed in proportion to obtain a powder mixture, wherein the pyrolytic electrolytic manganese slag replaces cement in an amount of 30%, and the mass ratio of Portland cement to aluminate cement is 3:2; the fine aggregate is 40-80 mesh quartz sand and 80-120 mesh quartz sand, the mortar-sand ratio is 1:1, and the mass ratio of 40-80 mesh quartz sand to 80-120 mesh quartz sand is 1:1.

[0036] (3) Weigh tap water, water reducer and sodium borate in proportion, wherein the water-to-binder ratio is 0.4, the sodium borate is 0.05% of the total mass of the base material, and the water reducer is a polycarboxylic acid water reducer, and the addition amount is 0.3% of the total mass of the base material.

[0037] (4) Pour the powder mixture into the mixer at a uniform speed within 30 seconds, stir at a low speed for 1 minute, stop stirring, scrape off the uneven mixture on the stirring blade and the wall of the material pot with a scraper within 30 seconds, stir at a high speed for 1 minute, stop for 1 minute, and continue stirring at a high speed for 15 seconds to obtain a cement-based self-leveling mortar for the floor prepared from pyrolytic electrolytic manganese slag.

[0038] The cement-based self-leveling mortar for the floor prepared according to the method of Example 1 has a fluidity as shown in the figure below: Figure 2As shown. After testing, the fresh fluidity is 137mm, and the fluidity after 20 minutes is 135mm. The flexural strength of the self-leveling mortar after testing is 3.845MPa in one day, 8.788MPa in 28 days, 10.268MPa in one day, and 38.9MPa in 28 days.

[0039] The cement-based self-leveling mortar for the floor prepared according to the method of Example 1 has a phase composition as follows: Figure 3 As shown in the figure, it can be seen that the physical composition of the self-leveling mortar is mainly composed of calcium sulfonate, gypsum, quartz, calcium hydroxide, hydrated calcium aluminate, calcium silicate, etc.

[0040] The cement-based self-leveling mortar for the floor prepared according to the method of Example 1 has a microscopic morphology as follows: Figure 4 As shown. Figure 4 It can be seen that the main hydration products include needle-like substance ettringite, ettringite crystals in the form of slender needles and some leaf-bud-like ettringite crystals growing on the surface of the self-leveling mortar material, gel-like substance C-(A)-SH gel and hexagonal prism-shaped substance gypsum. These substances are intertwined and overlapped with each other, which is the source of strength of the pyrolytic electrolytic manganese slag-based self-leveling mortar material.

[0041] Example 2

[0042] The difference between Example 2 and Example 1 is that the type of water reducer is polycarboxylic acid water reducer, the amount of water reducer is 0.1% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0043] Example 3

[0044] The difference between Example 3 and Example 1 is that the type of water reducer is polycarboxylic acid water reducer, the amount of water reducer is 0.5% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0045] Example 4

[0046] The difference between Example 4 and Example 1 is that the type of water reducer is a naphthalene-based water reducer, the amount of the water reducer is 0.5% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0047] Example 5

[0048] The difference between Example 5 and Example 1 is that the type of water reducer is a naphthalene-based water reducer, the amount of the water reducer is 1.0% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0049] Example 6

[0050] The difference between Example 6 and Example 1 is that the type of water reducer is a naphthalene-based water reducer, the amount of the water reducer is 1.5% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0051] Example 7

[0052] The difference between Example 7 and Example 1 is that the type of water reducer is sodium lignin sulfonate water reducer, the amount of water reducer is 0.5% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0053] Example 8

[0054] The difference between Example 8 and Example 1 is that the type of water reducer is sodium lignin sulfonate water reducer, the amount of water reducer is 1.0% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0055] Example 9

[0056] The difference between Example 9 and Example 1 is that the type of water reducer is sodium lignin sulfonate water reducer, the amount of water reducer is 1.5% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0057] Example 10

[0058] The difference between Example 10 and Example 1 is that medium-temperature pyrolytic electrolytic manganese slag replaces 10% of cement, the water reducer is a polycarboxylic acid water reducer, and the amount of the water reducer is 0.5% of the total mass of the base material. Other preparation conditions and methods remain unchanged.

[0059] Embodiment 11

[0060] The difference between Example 11 and Example 1 is that medium-temperature pyrolytic electrolytic manganese slag replaces 20% of cement, the water reducer is a polycarboxylic acid water reducer, and the amount of the water reducer is 0.5% of the total mass of the base material. Other preparation conditions and methods remain unchanged.

[0061] Example 12

[0062] The difference between Example 12 and Example 1 is that medium-temperature pyrolytic electrolytic manganese slag replaces 30% of cement, the water reducer is a polycarboxylic acid water reducer, and the amount of the water reducer is 0.5% of the total mass of the base material. Other preparation conditions and methods remain unchanged.

[0063] Example 13

[0064] The difference between Example 13 and Example 1 is that medium-temperature pyrolytic electrolytic manganese slag replaces 40% of cement, the water reducer is a polycarboxylic acid water reducer, the amount of the water reducer is 0.5% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0065] Embodiment 14

[0066] The difference between Example 14 and Example 1 is that medium-temperature pyrolytic electrolytic manganese slag replaces 50% of cement, the water reducer is a polycarboxylic acid water reducer, the amount of the water reducer is 0.5% of the total mass of the base material, and other preparation conditions and methods remain unchanged.

[0067] Embodiment 15

[0068] The performance tests were performed on the self-leveling mortar samples prepared in Examples 1-14.

[0069] Fresh state fluidity test method: Place a metal hollow cylinder with an inner diameter of (30±0.1) mm and a height of (50±0.1) mm in the center of a flat plate with an area greater than 300 mm×300 mm. The test plate should be flat, smooth and free of water droplets. Fill the fluidity test mold with the stirred self-leveling mortar, scrape off the excess mortar on the top of the test mold, and then lift it vertically upward by 50mm-100mm within 2s. Keep it for 10s-15s to allow the sample to flow freely. Start timing after the time preparation is completed. After 4 minutes, measure the diameters in two vertical directions and take the arithmetic average as the measured value.

[0070] 20-minute fluidity test method: After stirring, place the same batch of samples in the stirrer for 20 minutes, stir at a low speed for 15 seconds, and measure the diameters in two vertical directions. The arithmetic average is taken as the measured value.

[0071] Test method for flexural strength: Self-leveling mortar specimens were prepared according to the different components and proportions in Implementation 1-14. The specimen size was 160mm×40mm×40mm. The specimens were demoulded after being placed for 24 hours and then placed in a constant temperature and humidity curing box for curing. The curing conditions of the constant temperature and humidity curing box were 20±2℃ and the relative humidity was 90%. The cured self-leveling mortar samples were placed on a universal testing machine to measure the flexural strength that the samples could withstand. The flexural rate was 50N / s. Three samples were tested in each group, and the average value was taken as the final result of the flexural strength of the reorganized samples.

[0072] Test method for compressive strength: Self-leveling mortar specimens were prepared according to the different components and proportions in Implementation 1-14. The specimen size was 160mm×40mm×40mm. The specimens were demoulded after being placed for 24 hours and then placed in a constant temperature and humidity curing box for curing. The curing conditions of the constant temperature and humidity curing box were 20±2℃ and the relative humidity was 90%. The cured self-leveling mortar samples were placed on a universal testing machine to measure the compressive strength that the samples could withstand. The compression rate was 1.2KN / s. A total of 6 samples were tested in each group, and the average value was taken as the final result of the flexural strength of the group of samples.

[0073] Examples 1-3 are studies on the dosage of the polycarboxylate water-reducing agent in the present invention. The research results are shown in Table 1.

[0074] Table 1 Performance test results of self-leveling mortar prepared in Examples 1-3

[0075] Table 1 Performance test results of self-leveling mortar prepared in Examples 1-3

[0076]

[0077] It can be seen from the data in Table 1 that when the content of polycarboxylate water-reducing agent reaches 0.3%, the initial fluidity and 20-min fluidity both reach 130 mm, and its compressive and flexural strengths reach the maximum. The compressive and flexural strengths reach 10.27 MPa and 3.85 MPa at 1 day, and 38.90 MPa and 8.79 MPa at 28 days. The fluidity of electrolytic manganese slag cement slurry is most sensitive to the dosage of PC water-reducing agent. Polycarboxylate high-efficiency water-reducing agent is adsorbed on the surface of gypsum and cement particles. In addition to electrostatic repulsion and lubrication, it also benefits from the steric hindrance generated by its molecular side chain to play a dispersing role, thereby improving the fluidity of the slurry. At the same time, it helps cement particles to contact more fully with electrolytic manganese slag particles and water. The gypsum in the electrolytic manganese slag reacts with calcium aluminate in aluminate cement and calcium hydroxide formed by hydration of silicate cement to form calcium sulfonite.

[0078] Examples 4-6 are studies on the dosage of the naphthalene-based water reducer in the present invention. The research results are shown in Table 2.

[0079] Table 2 Performance test results of self-leveling mortar prepared in Examples 4-6

[0080]

[0081] From the data in Table 2, it can be seen that the initial fluidity and 20-minute fluidity of the Nai-series water reducer both reach 130 mm when the dosage is 1.0%. Its compressive and flexural strengths reach the maximum. The 1-day compressive and flexural strengths reach 8.343 MPa and 2.332 MPa, respectively, and the 28-day compressive and flexural strengths reach 32.2 MPa and 6.936 MPa. Hydrated calcium aluminate and calcium aluminate are the main hydration products. The Nai-series water reducer is an anionic surfactant, in which the ionized hydrophilic group -SO3 - It can be adsorbed on the surface of cement particles to disperse the cement particles so that they can fully contact with water. However, excessive water reducer causes water bleeding in the mortar, which has a negative impact on its strength.

[0082] Examples 7-9 are studies on the dosage of the sodium lignin sulfonate water-reducing agent in the present invention. The research results are shown in Table 3.

[0083] Table 3 Performance test results of self-leveling mortar prepared in Examples 7-9

[0084]

[0085] From the data in Table 3, it can be seen that the initial fluidity and 20-min fluidity of sodium lignin sulfonate water reducer both reach 130 mm when the dosage is 1.0%. Its compressive and flexural strengths reach the maximum. The 1-day compressive and flexural strengths reach 8.392 MPa and 2.259 MPa, respectively, and the 28-day compressive and flexural strengths reach 29.909 MPa and 7.442 MPa. Sodium lignin sulfonate has the worst dispersion performance on cement.

[0086] Examples 10-14 are studies on the dosage of pyrolysis electrolytic manganese slag in the present invention. The research results are shown in Table 4.

[0087] Table 4 Performance test results of self-leveling mortar prepared in Examples 10-14

[0088]

[0089]

[0090] It can be seen from the data in Table 4 that as the amount of electrolytic manganese slag increases from 10% to 50%, the initial fluidity and fluidity after 20 minutes of the self-leveling mortar show a downward trend. This shows that a large amount of electrolytic manganese slag has a significant adverse effect on the fluidity of the self-leveling mortar. When the amount reaches 40%, the fluidity of the self-leveling mortar after 20 minutes does not reach the fluidity requirement of 130mm in the national standard (JC / T 985-2017). The particle size of electrolytic manganese slag is small. When the amount is low, the electrolytic manganese slag plays a filling role, filling between quartz and cement, so the fluidity is higher. However, electrolytic manganese slag has a unique surface property that has an adsorption effect on water. With the increase of the amount of electrolytic manganese slag, on the one hand, the filling effect of the electrolytic manganese slag is weakened, and on the other hand, a large amount of electrolytic manganese slag adsorbs water. Therefore, with the increase of the amount of electrolytic manganese slag, the free water used for lubrication in the system is significantly reduced. When the dosage of pyrolytic electrolytic manganese slag increases from 10% to 50%, the 1-day compressive strength decreases from 11.35MPa to 5.78MPa, and the flexural strength decreases from 6.24MPa to 1.91MPa; the 28-day compressive strength decreases from 53.81MPa to 24.70MPa, and the flexural strength decreases from 9.54MPa to 5.72MPa. When the dosage is 50%, the 1-day and 28-day compressive and flexural strengths fail to reach the minimum strength of the surface cement self-leveling mortar in the standard JC / T 985-2017. After adding excessive electrolytic manganese slag, the hydration product is mainly calcium sulfonate. The presence of excessive calcium sulfonate crystals in the system causes internal stress in the material, resulting in a decrease in strength. When the dosage of electrolytic manganese slag is low, the electrolytic manganese slag with smaller particle size plays a "filling" and "nucleation" role, which can have a positive effect on the strength of the self-leveling mortar to a certain extent.

[0091] In summary, in the research process of preparing self-leveling mortar with pyrolytic electrolytic manganese slag, when the electrolytic manganese slag calcined at 800°C replaced 30% cement and 0.3% polycarboxylic acid water reducer was added to the total mass of the base material, the initial fluidity and 20min fluidity of the prepared self-leveling mortar sample reached 137mm and 135mm respectively, the 1-day compressive and flexural strength reached 10.27MPa and 3.85MPa respectively, and the 28-day compressive and flexural strength reached 38.90MPa and 8.79MPa respectively.

[0092] Therefore, the present invention provides a method for preparing self-leveling mortar using electrolytic manganese slag after medium-temperature calcination activation treatment. After the electrolytic manganese slag is subjected to medium-temperature pyrolysis treatment, the ammonia nitrogen in the electrolytic manganese slag is effectively removed, the manganese ions are solidified, and the volcanic ash activity of the electrolytic manganese slag is stimulated. At the same time, the present invention uses solid waste as raw materials, greatly reducing the production cost, the pyrolysis electrolytic manganese slag dosage can reach 30%, and the prepared ground cement-based self-leveling mortar fluidity and strength performance meet the requirements of standard JC / T985-2017, which opens up a new way for the preparation of ground cement-based self-leveling mortar and the resource utilization of electrolytic manganese slag, and has good practicality.

[0093] Those skilled in the art to which the present application belongs may make various modifications or additions to the specific embodiments described or replace them in a similar manner, but they will not deviate from the inventive concept of the present application or exceed the scope defined by the attached claims.

Claims

1. A method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature, It is characterized in that The steps include: S1. Preparation of pyrolytic electrolytic manganese slag: drying the electrolytic manganese slag, grinding it, sieving it, placing it in a muffle furnace for calcination, heating it to 800° C. in the muffle furnace, keeping it warm for 120 min, cooling it to room temperature with the furnace after calcination, and obtaining a medium-temperature calcination product, pyrolytic electrolytic manganese slag; S2, mixing ordinary Portland cement, aluminate cement, pyrolysis electrolytic manganese slag and fine aggregate according to proportion to obtain a powder mixture; S3. Weigh tap water, water reducing agent and sodium borate in proportion and pour them into a blender; S4. Pour the powder mixture into the mixer at a uniform speed within 30 seconds, stir at a low speed for 1 minute, stop stirring, and scrape off the uneven mixture on the stirring blades and the wall of the material pot with a scraper within 30 seconds, then stir at a high speed for 1 minute, stop for 1 minute, and continue stirring at a high speed for 15 seconds to obtain cement-based self-leveling mortar for the floor prepared from pyrolytic electrolytic manganese slag.

2. The method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature according to claim 1, It is characterized in that In step S1: after the electrolytic manganese slag is dried, it is ground to a particle size less than 200 meshes, and the heating rate of the electrolytic manganese slag is 5° C. / min.

3. The method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature according to claim 1, It is characterized in that In step S2: the model of ordinary Portland cement is P.O42.5R; the model of aluminate cement is CA-50.

4. The method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature according to claim 1, It is characterized in that In step S2: the pyrolytic electrolytic manganese slag calcined at 800° C. in the cementitious material replaces cement by 10%-50%.

5. The method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature according to claim 1, It is characterized in that In step S2: the mass ratio of silicate cement to aluminate cement is 3:

2.

6. The method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature according to claim 1, It is characterized in that In step S2: the fine aggregate is 40-80 mesh quartz sand and 80-120 mesh quartz sand, the mortar-sand ratio is 1:1, and the mass ratio of 40-80 mesh quartz sand to 80-120 mesh quartz sand is 1:

1.

7. The method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature according to claim 1, It is characterized in that In step S3: the water-to-binder ratio is 0.

4.

8. The method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature according to claim 1, It is characterized in that In step S3: the sodium borate is used as a retarder, accounting for 0.05% of the total mass of the base material.

9. The method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature according to claim 1, It is characterized in that In step S3: the water reducing agent is at least one of a polycarboxylate water reducing agent, a naphthalene-based water reducing agent, and a sodium lignin sulfonate water reducing agent.

10. The method for preparing self-leveling mortar by calcining electrolytic manganese slag at medium temperature according to claim 9, It is characterized in that In step S3: the amount of water reducer added is as follows: the amount of polycarboxylate water reducer added is 0.1%-0.5% of the total mass of the base material, or the amount of naphthalene water reducer added is 0.5%-1.5% of the total mass of the base material, or the amount of sodium lignin sulfonate water reducer added is 0.5%-1.5% of the total mass of the base material.