Cemented filling material as well as preparation method and application thereof

By using a core-shell structure of slag powder and desulfurization ash combined with a modified oxidant in the filling material, the problems of shrinkage and strength reduction in the later stage of hardening of the filling body are solved, achieving a low-cost strength improvement that is suitable for mine filling.

CN118908683APending Publication Date: 2024-11-08FUJIAN LONGKING DSDN ENGINEERING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410953312.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional cement-based and slag powder-based backfill materials exhibit significant shrinkage and strength reduction in the later stages of hardening, leading to increased backfilling costs and safety hazards.

Method used

Slag powder is used as the main component of the cementitious material, combined with desulfurization ash as an activator, and a modified oxidant is used in a core-shell structure, with the core being the oxidant and the shell being calcium sulfate. By synergistically regulating the formation of ettringite and the oxidation of calcium sulfite, the later shrinkage of the filling material is reduced and the strength is increased.

Benefits of technology

It effectively solves the problems of shrinkage and strength reduction in the later stage of hardening of the filling material, reduces production costs, and improves the later strength of the filling material, thus having a good market prospect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947838120000121
    Figure BDA0004947838120000121
Patent Text Reader

Abstract

The invention belongs to the field of environmental protection, and particularly relates to a cemented filling material and a preparation method and application thereof. The cemented filling material provided by the invention comprises tailings, a cementing material and water, the cementing material comprises superfine slag powder and an exciting agent; the exciting agent comprises desulfurized fly ash and a modified oxidizing agent; the modified oxidizing agent is of a core-shell structure, an inner core is an oxidizing agent, and a shell is calcium sulfate. The superfine slag powder is used as a main component of a cementing material in the filling material, the desulfurized fly ash is used as a main exciting agent of the cementing material, the oxidizing agent coated and modified by the calcium sulfate is added in an auxiliary manner, and generation of ettringite and oxidation of calcium sulfite in the desulfurized fly ash are synergistically regulated and controlled; the later-stage shrinkage of the filling material can be reduced, and the later-stage strength is improved. The cemented filling material provided by the invention can effectively solve the problems of shrinkage and strength reduction in the later hardening stage of a filling body, and the filling material is relatively low in production cost and has a good market prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental protection, and in particular relates to a cementing filling material and a preparation method and application thereof. Background Art

[0002] In recent years, the total amount of tailings emissions has been rising year by year, mainly including the beneficiation tailings of nine kinds of minerals, including iron, copper, aluminum, lead, zinc, tungsten, tin, molybdenum, and gold. Most of them are stored in tailings ponds, which not only occupies a large amount of land, but also becomes an important source of pollution to the ecological environment. Some even become an important risk source for mining safety accidents.

[0003] Using tailings to assist cementitious materials for underground mine filling is the main way to dispose of tailings. It can effectively and quickly fill underground mining space and realize mining re-mining, and has good economic and ecological value. Traditional filling cementitious materials are mainly cement-based, but due to the continuous progress of my country's mining technology, tailings sand is becoming finer and finer. Traditional cement-based filling materials are prone to problems such as excessive water seepage, low strength, poor fluidity, and high cost. They have gradually been replaced by slag micropowder-based cementitious materials. The cementitious materials formed by slag micropowder combined with related stimulating materials (such as lime, gypsum, etc.) can better cooperate with tailings under recent mining processes. The resulting filling slurry has the advantages of good fluidity, high strength, rich resource sources, and low cost.

[0004] However, whether it is cement-based or slag micropowder-based mine filling materials, there is still the problem of obvious volume shrinkage after the filling body solidifies, resulting in a low filling top rate and a decrease in the later strength of the filling body, which increases safety hazards and requires secondary or even tertiary filling, greatly increasing the filling cost. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a bonding filling material and a preparation method and application thereof. The bonding filling material provided by the present invention can achieve later micro-expansion and increased strength, effectively solve the problems of later shrinkage and strength reduction of the filling body after hardening, and has low cost.

[0006] The present invention provides a cementitious filling material, comprising tailings, a cementitious material and water; the cementitious material comprises slag powder and an activator; the activator comprises desulfurized ash and a modified oxidant; the modified oxidant is a core-shell structure, wherein the core is an oxidant and the shell is calcium sulfate.

[0007] Preferably, the oxidant is one or more of iron oxide, manganese carbonate, titanium oxide, copper oxide, nickel oxide and aluminum oxide.

[0008] Preferably, the mass ratio of calcium sulfate to oxidant is (2-10):1.

[0009] Preferably, the modified oxidant is prepared according to the following steps:

[0010] The suspension containing the oxidant, calcium sulfate and the dispersant is spray-dried to obtain a modified oxidant;

[0011] Alternatively, a suspension containing the oxidant, calcium sulfate and dispersant is dried and crushed to obtain a modified oxidant.

[0012] Preferably, the spray drying temperature is 120-185°C; the drying temperature is 120-185°C.

[0013] Preferably, the modified oxidant accounts for 3-15% of the total mass of the desulfurized ash and the modified oxidant.

[0014] Preferably, the content of the slag powder in the cementitious material is 56-80wt%, and the content of the activator in the cementitious material is 20-44wt%.

[0015] Preferably, the cementitious material further comprises quicklime, and the content of the quicklime in the cementitious material is 0-11 wt %.

[0016] The present invention provides a method for preparing the cementitious filling material described in the above technical solution, comprising the following steps:

[0017] The tailings, cementitious material and water are mixed to obtain cementitious filling material.

[0018] The present invention provides a mine filling method, comprising the following steps:

[0019] The cementitious filling material described in the above technical solution or the cementitious filling material prepared by the preparation method described in the above technical solution is filled into a mine, and the cementitious filling material solidifies in the mine to form a cemented body.

[0020] Compared with the prior art, the present invention provides a cementitious filling material and its preparation method and application. The cementitious filling material provided by the present invention includes tailings, cementitious material and water; the cementitious material includes slag powder and an activator; the activator includes desulfurized ash and a modified oxidant; the modified oxidant is a core-shell structure, the inner core is an oxidant, and the outer shell is calcium sulfate. The present invention uses slag powder as the main component of the cementitious material in the filling material, uses desulfurized ash as the main activator of the cementitious material, and auxiliary addition of the oxidant modified by calcium sulfate coating. By synergistically regulating the formation of calcium sulfonite and the oxidation of calcium sulfite in the desulfurized ash, the late shrinkage of the filling material can be reduced and its late strength can be increased. The cementitious filling material provided by the present invention can effectively solve the problems of late shrinkage and strength reduction of the filling body after hardening, and the production cost of the filling material is low, and it has good market prospects. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] The present invention provides a cementitious filling material, comprising tailings, a cementitious material and water; the cementitious material comprises slag powder and an activator; the activator comprises desulfurized ash and a modified oxidant; the modified oxidant is a core-shell structure, wherein the core is an oxidant and the shell is calcium sulfate.

[0023] In the cementing filling material provided by the present invention, the tailings include but are not limited to one or more of iron ore tailings, gold ore tailings, silver ore tailings, copper ore tailings and lead-zinc ore tailings; the tailings have a D 50 The particle size is preferably 50 to 80 μm, more preferably 65 μm. 90 The particle size is preferably 170-210 μm, more preferably 188 μm; the SiO2 content of the tailings is preferably ≥70wt%, more preferably ≥75wt%; the Al2O3 content of the tailings is preferably ≥10wt%, more preferably ≥14wt%.

[0024] In the cementitious filling material provided by the present invention, in the cementitious material, the grade of the slag powder is S95 or above.

[0025] In the cementitious filling material provided by the present invention, the content of the slag powder in the cementitious material is preferably 56-80wt%, specifically 56wt%, 57wt%, 58wt%, 59wt%, 60wt%, 61wt%, 62wt%, 63wt%, 64wt%, 65wt%, 66wt%, 67wt%, 68wt%, 69wt%, 70wt%, 71wt%, 72wt%, 73wt%, 74wt%, 75wt%, 76wt%, 77wt%, 78wt%, 79wt% or 80wt%.

[0026] In the cementitious filling material provided by the present invention, in the activator, the calcium sulfite content in the desulfurization ash is preferably ≥15wt%, more preferably ≥30wt%, specifically 16wt%, 28wt% or 68wt%; the calcium hydroxide content in the desulfurization ash is preferably ≥3wt%, specifically 5wt%, 8wt% or 13wt%; the calcium carbonate content in the desulfurization ash is preferably ≥15wt%, more preferably ≥20wt%, specifically 21wt% or 31wt%; the calcium sulfate content in the desulfurization ash is preferably 0-50wt%, specifically 18wt% or 42wt%.

[0027] In the cementitious filling material provided by the present invention, in the modified oxidant, the oxidant is preferably one or more of iron oxide, manganese carbonate, titanium oxide, copper oxide, nickel oxide and aluminum oxide.

[0028] In the cementitious filling material provided by the present invention, in the modified oxidant, the mass ratio of calcium sulfate to oxidant is preferably (2-10):1, specifically 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1 or 10:1.

[0029] In the cementitious filling material provided by the present invention, in the activator, the particle size of the modified oxidant is preferably 400-600 mesh, specifically 400 mesh, 410 mesh, 420 mesh, 430 mesh, 440 mesh, 450 mesh, 460 mesh, 470 mesh, 480 mesh, 490 mesh, 500 mesh, 510 mesh, 520 mesh, 530 mesh, 540 mesh, 550 mesh, 560 mesh, 570 mesh, 580 mesh, 590 mesh or 600 mesh.

[0030] In the cementitious filling material provided by the present invention, in the activator, the modified oxidant is preferably prepared according to the following steps:

[0031] A) spray drying a suspension containing an oxidant, calcium sulfate and a dispersant to obtain a modified oxidant;

[0032] or,

[0033] A') drying and crushing the suspension containing the oxidant, calcium sulfate and dispersant to obtain a modified oxidant.

[0034] In the cementitious filling material provided by the present invention, in the above-mentioned modified oxidant preparation step, the dispersant is preferably polyethyleneimine.

[0035] In the cementitious filling material provided by the present invention, in the above-mentioned modified oxidant preparation step, in step A), the specific preparation process of the suspension preferably includes: firstly stirring and mixing the oxidant, dispersant and water to obtain an oxidant dispersion; then ultrasonically mixing the oxidant dispersion with calcium sulfate to obtain the suspension. Wherein, the content of the oxidant in the oxidant dispersion is preferably 5 to 35wt%, specifically 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt% or 35wt%; the content of the dispersant in the oxidant dispersion is preferably 0.02 to 0.1wt%, specifically 0.02wt%, 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt% or 0.1wt%; the stirring and mixing time is preferably 5 to 15min, specifically 5min, 6m in, 7min, 8min, 9min, 10min, 11min, 12min, 13min, 14min or 15min; the mass ratio of the calcium sulfate to the oxidant is preferably (3-8):1, specifically 3:1, 4:1, 5:1, 6:1, 7:1 or 8:1; the ultrasonic mixing time is preferably 2-30min, specifically 2min, 3min, 4min, 5min, 6min, 7min, 8min, 9min, 10min, 11min, 12min, 15min, 20min, 25min or 30min.

[0036] In the cementitious filling material provided by the present invention, in the above-mentioned modified oxidant preparation step, in step A), the spray drying temperature is preferably 120-185°C, specifically 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C or 185°C.

[0037] In the cementitious filling material provided by the present invention, in the above-mentioned modified oxidant preparation step, in step A), after the spray drying is completed, the obtained modified oxidant particles are preferably air-selected to obtain a modified oxidant with a suitable particle size range.

[0038] In the cementitious filling material provided by the present invention, in the above-mentioned modified oxidant preparation step, in step A'), the specific preparation process of the suspension preferably includes: firstly stirring and mixing the oxidant, dispersant and water to obtain an oxidant dispersion; then ultrasonically mixing the oxidant dispersion with calcium sulfate to obtain the suspension. The content of the oxidant in the oxidant dispersion is preferably 5-35wt%, specifically 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt% or 35wt%; the content of the dispersant in the oxidant dispersion is preferably 0.05-0.15wt%, specifically 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, 0.1wt%, 0.11wt%, 0.12wt%, 0.13wt%, 0.14wt% or 0.15wt%; the stirring and mixing time is preferably 3-18min, specifically 3min, 4min, 5min in, 6min, 7min, 8min, 9min, 10min, 11min, 12min, 13min, 14min, 15min, 16min, 17min or 18min; the mass ratio of calcium sulfate to oxidant is preferably (4-10):1, specifically 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1; the ultrasonic mixing time is preferably 2-15min, specifically 2min, 3min, 4min, 5min, 6min, 7min, 8min, 9min, 10min, 11min, 12min, 13min, 14min or 15min.

[0039] In the cementitious filling material provided by the present invention, in the above-mentioned modified oxidant preparation step, in step A'), the drying temperature is preferably 120-185°C, specifically 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C or 185°C; the crushing method is preferably grinding.

[0040] In the cementitious filling material provided by the present invention, in the activator, the modified oxidant preferably accounts for 3-15% of the total mass of the desulfurized ash and the modified oxidant, specifically 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%.

[0041] In the cementitious filling material provided by the present invention, the content of the activator in the cementitious material is preferably 20-44wt%, specifically 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt% or 44wt%.

[0042] In the cementitious filling material provided by the present invention, the cementitious material preferably also includes quicklime; the purity of the quicklime is preferably ≥85%; the fineness of the quicklime is preferably 100-300 mesh, specifically 100 mesh, 150 mesh, 200 mesh, 250 mesh or 300 mesh.

[0043] In the cementitious filling material provided by the present invention, the content of quicklime in the cementitious material is preferably 0-11wt%, specifically 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% or 11wt%.

[0044] In the cementitious filling material provided by the present invention, the mass ratio of the cementitious material to tailings is preferably 1:(4-8), specifically 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5 or 1:8; the total content of the cementitious material and tailings in the cementitious filling material is preferably 70-80wt%, specifically 70wt%, 71wt%, 72wt%, 73wt%, 74wt%, 75wt%, 76wt%, 77wt%, 78wt%, 79wt% or 80wt%.

[0045] The present invention also provides a method for preparing the cementitious filling material described in the above technical solution, comprising the following steps:

[0046] The tailings, cementitious material and water are mixed to obtain cementitious filling material.

[0047] The present invention also provides a mine filling method, comprising the following steps:

[0048] The cementitious filling material described in the above technical solution or the cementitious filling material prepared by the preparation method described in the above technical solution is filled into a mine, and the cementitious filling material solidifies in the mine to form a cemented body.

[0049] The technical solution provided by the invention uses slag powder as the main component of the cementitious material in the filling material, utilizes desulfurized ash as the main activator of the cementitious material, and auxiliaryly adds an oxidant modified by calcium sulfate coating. By synergistically regulating the formation of calcium sulfonite and the oxidation of calcium sulfite in the desulfurized ash, the later shrinkage of the filling material can be reduced and its later strength can be increased. Its main principles include: first, slag powder will undergo hydration reaction under alkaline conditions to generate calcium silicate hydrate (CSH), calcium aluminate hydrate (CAH), etc. to form a certain strength; secondly, calcium sulfate coated on the surface of the oxidant with a certain thickness will directly react with the hydration product of the slag powder to generate calcium sulfonate, which further provides strength for the filling body in the early stage and reduces early shrinkage; secondly, as calcium sulfonate is continuously generated, the calcium sulfate coated on the surface of the oxidant is gradually consumed, gradually exposing the coated oxidant, and the calcium sulfite in the filling body is oxidized by the oxidant to generate plate-shaped calcium sulfate, accompanied by volume expansion; finally, part of the newly generated calcium sulfate slowly reacts with the hydration product of the slag powder again to generate calcium sulfonate, which is also accompanied by volume expansion and strength increase. The cementitious filling material provided by the present invention can effectively solve the problems of shrinkage and strength reduction in the late hardening of the filling body, and the production cost of the filling material is low, and it has a good market prospect.

[0050] For the sake of clarity, the following examples are used to explain in detail. In the following examples of the present invention, three kinds of desulfurized ash are used, as follows:

[0051] Ash sample A comes from a steel plant, and its main components are: calcium sulfite 68wt%, calcium hydroxide 5wt%, calcium carbonate 21wt%, and other 6wt%;

[0052] Ash sample B comes from a power plant, and its main components are: calcium sulfite 28wt%, calcium hydroxide 8wt%, calcium carbonate 31wt%, calcium sulfate 18wt%, and others 15wt%;

[0053] Ash sample C comes from a chemical plant, and its main components are: 16wt% calcium sulfite, 13wt% calcium hydroxide, 21wt% calcium carbonate, 42wt% calcium sulfate, and 8wt% others.

[0054] In the following embodiments of the present invention, the slag powder used is of grade S95. In the following embodiments of the present invention, the quicklime used has a purity of CaO>85% and a fineness of 200 mesh.

[0055] In the following embodiments of the present invention, the calcium sulfate used has a purity of more than 92%, a fineness of 800 meshes, and a moisture content of less than 2%.

[0056] In the following embodiments of the present invention, the oxidant used has a fineness of 325 mesh and a pass rate of more than 95%.

[0057] In the following embodiments of the present invention, the tailings are iron ore tailings, and D 50 =65μm, D 90 =188μm, the composition is shown in Table 1:

[0058] Table 1 Iron ore tailings composition

[0059] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO <![CDATA[K2O]]> MgO 76.220wt% 14.590wt% 0.624wt% 1.428wt% 5.260wt% 0.617wt%

[0060] In the following embodiments of the present invention, the mass ratio of the cementitious material to the tailings is 1:6, and the total content of the cementitious material and the tailings in the cementitious filling material is 75 wt%.

[0061] Example 1

[0062] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 72wt% slag powder, 26wt% activator, and 2wt% quicklime; wherein the activator comprises: 95wt% ash sample A desulfurized ash, 5wt% modified oxidant, and the modified oxidant is a core-shell structure, wherein the core is the oxidant (iron oxide) and the shell is calcium sulfate.

[0063] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 5 minutes, and preparing a suspension with an oxidant concentration of 5wt% and a polyethyleneimine concentration of 0.02wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 0:1, and ultrasonic stirring is performed for 7 minutes; after spray drying at 156°C, selecting particles between 400 mesh and 600 mesh to obtain a modified oxidant; after mixing the modified oxidant with desulfurization ash, an activator is obtained.

[0064] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0065] Example 2

[0066] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 68wt% slag powder, 29wt% activator and 3wt% quicklime; wherein the activator comprises: 94wt% ash sample A desulfurized ash and 6wt% modified oxidant, wherein the modified oxidant is a core-shell structure, wherein the core is an oxidant (iron oxide) and the shell is calcium sulfate.

[0067] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 8 minutes, and preparing a suspension with an oxidant concentration of 6wt% and a polyethyleneimine concentration of 0.03wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 10:1, and ultrasonic stirring for 8 minutes; after spray drying at 160°C, selecting particles between 400 mesh and 600 mesh to obtain a modified oxidant; mixing the modified oxidant with desulfurization ash to obtain an activator.

[0068] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0069] Example 3

[0070] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 68wt% slag powder, 29wt% activator and 3wt% quicklime; wherein the activator comprises: 94wt% ash sample A desulfurized ash and 6wt% modified oxidant, wherein the modified oxidant is a core-shell structure, wherein the core is an oxidant (iron oxide) and the shell is calcium sulfate.

[0071] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 6 minutes, and preparing a suspension with an oxidant concentration of 7wt% and a polyethyleneimine concentration of 0.03wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 2:1, and ultrasonic stirring is performed for 9 minutes; after spray drying at 162°C, selecting particles between 400 mesh and 600 mesh to obtain a modified oxidant; after mixing the modified oxidant with desulfurization ash, an activator is obtained.

[0072] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0073] Example 4

[0074] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 71wt% slag powder, 27wt% activator and 2wt% quicklime; wherein the activator comprises: 92wt% ash sample A desulfurized ash, 8wt% modified oxidant, wherein the modified oxidant is a core-shell structure, wherein the core is an oxidant (iron oxide and manganese carbonate, with a mass ratio of 1:3) and the shell is calcium sulfate.

[0075] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 4 minutes, and preparing a suspension with an oxidant concentration of 7wt% and a polyethyleneimine concentration of 0.03wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 6:1, and ultrasonic stirring is performed for 10 minutes; after spray drying at 175°C, selecting particles between 400 mesh and 600 mesh to obtain a modified oxidant; after mixing the modified oxidant with desulfurization ash, an activator is obtained.

[0076] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0077] Example 5

[0078] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 71wt% slag powder, 27wt% activator and 2wt% quicklime; wherein the activator comprises: 93wt% ash sample A desulfurized ash and 7wt% modified oxidant, wherein the modified oxidant is a core-shell structure, wherein the core is an oxidant (iron oxide) and the shell is calcium sulfate.

[0079] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 5 minutes, and preparing a suspension with an oxidant concentration of 7wt% and a polyethyleneimine concentration of 0.02wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 6:1, and ultrasonic stirring is performed for 10 minutes; after spray drying at 177°C, selecting particles between 400 mesh and 600 mesh to obtain a modified oxidant; after mixing the modified oxidant with desulfurization ash, an activator is obtained.

[0080] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0081] Example 6

[0082] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 73wt% slag powder, 25wt% activator and 2wt% quicklime; wherein the activator comprises: 93wt% ash sample A desulfurized ash and 7wt% modified oxidant, wherein the modified oxidant is a core-shell structure, wherein the core is an oxidant (manganese carbonate) and the shell is calcium sulfate.

[0083] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 7 minutes, and preparing a suspension with an oxidant concentration of 7wt% and a polyethyleneimine concentration of 0.02wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 6:1, and ultrasonic stirring is performed for 8 minutes; after spray drying at 172°C, selecting particles between 400 mesh and 600 mesh to obtain a modified oxidant; mixing the modified oxidant with desulfurized ash to obtain an activator.

[0084] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0085] Example 7

[0086] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 69wt% slag powder, 28wt% activator, and 3wt% quicklime; wherein the activator comprises: 92wt% ash sample A desulfurized ash, 8wt% modified oxidant, and the modified oxidant is a core-shell structure, wherein the core is the oxidant (iron oxide) and the shell is calcium sulfate.

[0087] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 6 minutes, and preparing a suspension with an oxidant concentration of 8wt% and a polyethyleneimine concentration of 0.03wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 5:1, and ultrasonic stirring for 5 minutes; after spray drying at 192°C, selecting particles between 400 mesh and 600 mesh to obtain a modified oxidant; mixing the modified oxidant with desulfurized ash to obtain an activator.

[0088] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0089] Example 8

[0090] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 71wt% slag powder, 27wt% activator and 2wt% quicklime; wherein the activator comprises: 95wt% ash sample B desulfurized ash, 5wt% modified oxidant, the modified oxidant being a core-shell structure, wherein the core is an oxidant (iron oxide and manganese carbonate, with a mass ratio of 1:3) and the shell is calcium sulfate.

[0091] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 5 minutes, and preparing a suspension with an oxidant concentration of 7wt% and a polyethyleneimine concentration of 0.03wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 6:1, and ultrasonic stirring is performed for 11 minutes; after spray drying at 176°C, selecting particles between 400 mesh and 600 mesh to obtain a modified oxidant; mixing the modified oxidant with desulfurized ash to obtain an activator.

[0092] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0093] Example 9

[0094] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 72wt% slag powder, 27wt% activator and 1wt% quicklime; wherein the activator comprises: 96wt% ash sample C desulfurized ash, 4wt% modified oxidant, wherein the modified oxidant is a core-shell structure, wherein the core is an oxidant (iron oxide and manganese carbonate, with a mass ratio of 1:3) and the shell is calcium sulfate.

[0095] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 5 minutes, and preparing a suspension with an oxidant concentration of 5wt% and a polyethyleneimine concentration of 0.03wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 6:1, and ultrasonic stirring is performed for 11 minutes; after spray drying at 176°C, selecting particles between 400 mesh and 600 mesh to obtain a modified oxidant; after mixing the modified oxidant with desulfurization ash, an activator is obtained.

[0096] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0097] Example 10

[0098] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 71wt% slag powder, 27wt% activator and 2wt% quicklime; wherein the activator comprises: 92wt% ash sample A desulfurized ash, 8wt% modified oxidant, wherein the modified oxidant is a core-shell structure, wherein the core is an oxidant (iron oxide and manganese carbonate, with a mass ratio of 1:3) and the shell is calcium sulfate.

[0099] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 6 minutes, and preparing a suspension with an oxidant concentration of 7wt% and a polyethyleneimine concentration of 0.05wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 6:1, and ultrasonic stirring for 10 minutes; after drying and crushing at 175°C, selecting particles between 400 mesh and 600 mesh, and obtaining a modified oxidant; mixing the modified oxidant with desulfurization ash, the activator is obtained.

[0100] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0101] Embodiment 11

[0102] A cementitious filling material for mine filling, comprising: tailings, cementitious material and water; wherein the cementitious material is composed of a mixture of the following substances: 73wt% slag powder, 27wt% activator, and 0wt% quicklime; wherein the activator comprises: 92wt% ash sample A desulfurized ash, 8wt% modified oxidant, and the modified oxidant is a core-shell structure, wherein the core is an oxidant (iron oxide and manganese carbonate, with a mass ratio of 1:3) and the shell is calcium sulfate.

[0103] The activator is prepared according to the following steps: adding the oxidant into water, adding polyethyleneimine, stirring for 6 minutes, and preparing a suspension with an oxidant concentration of 7wt% and a polyethyleneimine concentration of 0.03wt%; adding calcium sulfate into the above oxidant suspension, the mass ratio of calcium sulfate to oxidant is 6:1, and ultrasonic stirring for 10 minutes; after drying and crushing at 175°C, selecting particles between 400 mesh and 600 mesh, and obtaining a modified oxidant; mixing the modified oxidant with desulfurization ash, the activator is obtained.

[0104] The above-mentioned cementitious material is mixed with tailings and water in proportion to obtain a cementitious filling material; the test values ​​of the 3d, 7d, 28d, 56d strength and 7d, 28d, 56d expansion rate of the filling material are shown in Table 2.

[0105] Table 2 Performance test results of filling materials prepared in the embodiments of the present invention

[0106]

[0107] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A cementing filling material, characterized in that: It includes tailings, cementitious materials and water; the cementitious materials include slag powder and an activator; the activator includes desulfurized ash and a modified oxidant; the modified oxidant is a core-shell structure, the core is the oxidant and the shell is calcium sulfate.

2. The cementitious filling material according to claim 1, characterized in that: The oxidant is one or more of iron oxide, manganese carbonate, titanium oxide, copper oxide, nickel oxide and aluminum oxide.

3. The cementitious filling material according to claim 1, characterized in that: The mass ratio of the calcium sulfate to the oxidant is (2-10):

1.

4. The cementitious filling material according to claim 1, characterized in that: The modified oxidant is prepared according to the following steps: The suspension containing the oxidant, calcium sulfate and the dispersant is spray-dried to obtain a modified oxidant; Alternatively, a suspension containing the oxidant, calcium sulfate and dispersant is dried and crushed to obtain a modified oxidant.

5. The cementitious filling material according to claim 4, characterized in that: The temperature of the spray drying is 120-185°C; the temperature of the drying is 120-185°C.

6. The cementitious filling material according to claim 1, characterized in that: The modified oxidant accounts for 3-15% of the total mass of the desulfurized ash and the modified oxidant.

7. The cementitious filling material according to claim 1, characterized in that: The content of the slag powder in the cementitious material is 56-80wt%, and the content of the activator in the cementitious material is 20-44wt%.

8. The cementitious filling material according to claim 1, characterized in that: The cementitious material also includes quicklime, and the content of the quicklime in the cementitious material is 0-11 wt %.

9. A method for preparing a cementitious filling material according to any one of claims 1 to 8, characterized in that: The following steps are involved: The tailings, cementitious material and water are mixed to obtain cementitious filling material.

10. A mine filling method, characterized in that: The following steps are involved: The cementitious filling material according to any one of claims 1 to 8 or the cementitious filling material prepared by the preparation method according to claim 9 is filled into a mine, and the cementitious filling material solidifies in the mine to form a cemented body.