Preparation method of ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramic

Through the preparation method of (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics, the Ti element is used to replace Zr atoms to form a solid solution, which solves the problem that the ablation layer of ZrB2-ZrC-SiC ceramics is prone to fall off and the sintering temperature is high. The low-temperature dense preparation and ablation resistance of ceramics have been achieved.

CN118908734AActive Publication Date: 2024-11-08DALIAN UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410958472.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The existing ZrB2-ZrC-SiC ceramics are prone to fall off in a high-temperature environment, resulting in insufficient ablation resistance, high sintering temperature and difficult densification.

Method used

The preparation method of (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics is adopted to prepare mixed slurries by ball milling, drying and sieving to obtain composite powders, and the rapid hot pressing and sintering technology is used to obtain 1500℃~1900℃. Densified sintering is achieved, and a solid solution (Zr,Ti)B2 and (Zr,Ti)C are formed by replacing Zr atoms with Ti elements to form a dense ablation layer.

Benefits of technology

The preparation of low-temperature dense block ceramics is realized, which reduces the sintering temperature and energy consumption, and significantly improves the ablation resistance of the ceramics. The linear ablation rate and mass ablation rate are significantly improved, compared with ZrB2-ZrC-SiC ceramics. Improved by 95.21%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908734A_ABST
    Figure CN118908734A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramic, and belongs to the field of high-temperature structural ceramic. The invention aims to solve the problems that the preparation temperature is high due to difficult densification sintering of the ZrB2-ZrC-SiC block ceramic prepared by the existing method, and the surface ablation layer is easy to fall off and the ablation resistance is insufficient in the high-temperature ablation process of the ZrB2-ZrC-SiC ceramic. The method comprises the following steps: 1, preparing mixed slurry; 2, preparing composite powder; and 3, rapid hot pressed sintering. According to the low-temperature preparation method of the ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramic, high sintering activity of raw material powder ZrSi2, TiSi2, B4C and C and reaction heat among the powder in the reaction sintering process are utilized, densification sintering of the ceramic is promoted, low-temperature preparation of the compact block ceramic is achieved, and the ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramic has excellent ablation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-temperature structural ceramics, and in particular relates to a method for preparing ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramics. Background Art

[0002] The safe service of high-temperature heat-resistant materials in extreme environments is a prerequisite for the development of aerospace technology. SiC ceramics and composite materials have been widely used in the aerospace field due to their excellent comprehensive performance in high-temperature environments. However, in harsh high-temperature oxygen-rich environments, SiC ceramics will suffer obvious ablation damage. The main reason is that the ablation layer formed on the surface quickly decomposes under the erosion of high-temperature heat flow and loses its protective effect on the ceramic matrix. Introducing ultra-high temperature ceramics (UHTCs) into the SiC matrix can effectively improve the high-temperature stability of the ablation layer and improve the ablation resistance of SiC ceramics.

[0003] Zr-based ultra-high temperature ceramics (ZrB2, ZrC, etc.) have a high melting point and high temperature stability. Introducing them into SiC to form two-phase composite ceramics such as ZrB2-SiC and ZrC-SiC can significantly improve the ablation resistance of SiC ceramics. On this basis, studies have shown that ZrB2-ZrC-SiC three-phase composite ceramics have better comprehensive properties than two-phase composite ceramics. This makes ZrB2-ZrC-SiC ceramics show excellent development potential in the field of aerospace heat protection.

[0004] However, the current preparation process of ZrB2-ZrC-SiC ceramics has problems such as difficulty in sintering densification and high sintering temperature. In addition, the ablation layer formed during the ablation of ZrB2-ZrC-SiC ceramics is a loose porous structure, which is easy to fall off and loses its protective effect on the material, resulting in the need to further improve the ablation resistance of ZrB2-ZrC-SiC ceramics.

[0005] Therefore, the key to overcoming the above problems is to develop a low-temperature densification sintering process for ZrB2-ZrC-SiC ceramics, realize the low-temperature rapid preparation of ZrB2-ZrC-SiC dense bulk ceramics, and form a dense and stable ablation layer during the ablation process by designing and modifying the composition of ZrB2-ZrC-SiC ceramics. Summary of the invention

[0006] The purpose of the present invention is to solve the problems of difficulty in densification sintering of ZrB2-ZrC-SiC bulk ceramics prepared by existing methods, high sintering temperature, easy shedding of surface ablation layer during high-temperature ablation of ZrB2-ZrC-SiC ceramics, and insufficient ablation resistance, and to provide a method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics.

[0007] A method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics is specifically completed by the following steps:

[0008] 1. Preparation of mixed slurry:

[0009] Add ZrSi2, TiSi2, B4C, C powders and anhydrous ethanol into a ball mill containing grinding balls, inject argon into the ball mill, and then seal the ball mill; fix the sealed ball mill on a ball mill, and mill the ball mill in an argon environment for a period of time to obtain a mixed slurry;

[0010] The molar ratio of the total amount of ZrSi2 and TiSi2 to B4C and C in step 1 is (5 / 18-1 / 2):(1 / 100-1 / 3):1; wherein the molar ratio of ZrSi2 to TiSi2 is (0.01-0.99):(0.01-0.99);

[0011] 2. Preparation of composite powder:

[0012] The mixed slurry is dried for a period of time at room temperature and under vacuum conditions, and after drying, it is sieved under the protection of an argon atmosphere to obtain a composite powder;

[0013] 3. Rapid hot pressing sintering:

[0014] First, the composite powder is compacted, and then hot-pressed and sintered for a period of time using a sintering device at 1500° C. to 1900° C. and an axial pressure of 20 MPa to 60 MPa to obtain ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramics;

[0015] The hot pressing sintering time in step 3 is 5 minutes to 20 minutes, and the environmental conditions are vacuum, argon or nitrogen.

[0016] Principle of the present invention:

[0017] The present invention proposes a low-temperature preparation method for ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics, which utilizes the high sintering activity of raw powders ZrSi2, TiSi2, B4C and C, and the reaction heat between the powders during the reaction sintering process to promote the densification sintering of ceramics and realize the low-temperature preparation of dense bulk ceramics. The method can achieve composition control of (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics by regulating the composition of the reactants. In addition, the present invention introduces the Ti element into the ZrC-ZrB2-SiC ceramic (part of the Zr atoms in the ZrB2 and ZrC lattices are replaced by Ti atoms to form a (Zr,Ti)B2 and (Zr,Ti)C solid solution), and utilizes the synergistic effect between the ablation products formed by each component during the ablation process of the (Zr,Ti)B2-(Zr,Ti)C-SiC multi-component ceramic to construct a continuous and dense ablation layer, thereby ensuring that the (Zr,Ti)C-(Zr,Ti)B2-SiC ceramic has better ablation resistance.

[0018] Beneficial effects of the present invention:

[0019] The present invention provides a method for preparing a (Zr, Ti) B2-(Zr, Ti) C-SiC multiphase ceramic, wherein the (Zr, Ti) B2-(Zr, Ti) C-SiC ceramic is obtained by reacting raw material powders ZrSi2, TiSi2, B4C and C powder during sintering, and the reaction process is carried out according to reaction formula (1), wherein MSi2 refers to a mixture of ZrSi2 and TiSi2; the molar ratio of ZrSi2 to TiSi2 in MSi2 is flexibly adjustable within the range of 0.99:0.01 to 0.01:0.99, thereby realizing flexible regulation of any Zr / Ti ratio of (Zr, Ti) C and (Zr, Ti) B2 solid solutions in the multiphase ceramic; in addition, by changing the values ​​of x and y, a (Zr, Ti) B2-(Zr, Ti) C-SiC multiphase ceramic with any molar ratio of (Zr, Ti) C and (Zr, Ti) B2 can be obtained;

[0020] (x+y)MSi2+y / 2B4C+(3x+3 / 2y)C=xMC+yMB2+2(x+y)SiC (1)

[0021] In summary, the method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics proposed in the present invention can achieve flexible regulation of the composition and organizational structure of (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics, providing a basis and premise for optimizing material design in combination with different service environment requirements;

[0022] In addition, the raw material powders ZrSi2, TiSi2, B4C and C used in the present invention have high sintering activity; during the reaction sintering process, the energy released by the powder reaction provides a driving force for sintering, which helps to reduce the sintering temperature. The present invention achieves low-temperature preparation of (Zr,Ti)B2-(Zr,Ti)C-SiC dense bulk ceramics at 1700°C, solving the problems of high sintering temperature and difficulty in densification in the prior art preparation of UHTCs / SiC ceramics; the present invention greatly reduces the energy consumption in the preparation process;

[0023] On the other hand, the present invention proposes to use Ti atoms to replace part of the Zr atoms in the ZrB2-ZrC-SiC multiphase ceramic to obtain (Zr,Ti)B2-(Zr,Ti)C-SiC multiphase ceramic; the mutual matching and synergistic effect of the microstructure and melting point between the ablation products of each component ensure that the ceramic can form a continuous and dense oxide layer during the ablation process, thereby improving the ablation resistance; the existing ZrC-ZrB2-SiC ablation layer is easy to fall off, and the ablation resistance is insufficient. The problems; when Zr / Ti=9:1, the linear ablation rate of the (Zr,Ti)B2-(Zr,Ti)C-SiC multiphase ceramic is only -0.00077mm / s, and the mass ablation rate is only 0.00015g / s, which is 95.21% better than the mass ablation rate of the ZrB2-ZrC-SiC ceramic. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The XRD patterns of the composite powders prepared in the comparative example 1 and the examples 1 to 3 of the present invention, wherein Zr / Ti=7:3 is the example 3, Zr / Ti=8:2 is the example 2, Zr / Ti=9:1 is the example 1, and Zr / Ti=10:0 is the comparative example 1;

[0025] Figure 2 XRD patterns of the multiphase ceramics prepared in Comparative Example 1 and Examples 1 to 3 of the present invention;

[0026] Figure 3 XRD patterns of the multiphase ceramics prepared in Examples 4 to 7 of the present invention;

[0027] Figure 4 Surface SEM images of the multiphase ceramics prepared in Control Example 1 and Examples 1 to 3 of the present invention after oxyacetylene ablation. DETAILED DESCRIPTION

[0028] Specific implementation method 1: This implementation method is a method for preparing ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramics, which is specifically completed in the following steps:

[0029] 1. Preparation of mixed slurry:

[0030] Add ZrSi2, TiSi2, B4C, C powders and anhydrous ethanol into a ball mill containing grinding balls, inject argon into the ball mill, and then seal the ball mill; fix the sealed ball mill on a ball mill, and mill the ball mill in an argon environment for a period of time to obtain a mixed slurry;

[0031] The molar ratio of the total amount of ZrSi2 and TiSi2 to B4C and C in step 1 is (5 / 18-1 / 2):(1 / 100-1 / 3):1; wherein the molar ratio of ZrSi2 to TiSi2 is (0.01-0.99):(0.01-0.99);

[0032] 2. Preparation of composite powder:

[0033] The mixed slurry is dried for a period of time at room temperature and under vacuum conditions, and after drying, it is sieved under the protection of an argon atmosphere to obtain a composite powder;

[0034] 3. Rapid hot pressing sintering:

[0035] First, the composite powder is compacted, and then hot-pressed and sintered for a period of time at 1500° C. to 1700° C. and an axial pressure of 20 MPa to 60 MPa using a sintering device to obtain ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramics;

[0036] The hot pressing sintering time in step 3 is 5 minutes to 20 minutes, and the environmental conditions are vacuum, argon or nitrogen.

[0037] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the material of the grinding balls in step 1 is ZrO2, and the ball-to-material mass ratio is (10-20): 1. The other steps are the same as those in specific implementation method 1.

[0038] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the rotation speed of the ball mill in step 1 is 300 r / min to 500 r / min, and the effective ball milling time is 10 h to 48 h. The other steps are the same as those of specific implementation method 1 or 2.

[0039] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the anhydrous ethanol described in step 1 accounts for 20% to 50% of the total mass of the ZrSi2, TiSi2, B4C and C powders. The other steps are the same as those of specific embodiments 1 to 3.

[0040] Specific implementation method 5: This implementation method is different from specific implementation methods 1 to 4 in that: in step 2, the mixed slurry is dried at room temperature and vacuum conditions for 20 hours to 100 hours. The other steps are the same as those of specific implementation methods 1 to 4.

[0041] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: in step 2, after drying, the mixture is sieved through a 100-200 mesh sieve under the protection of an argon atmosphere to obtain a composite powder. The other steps are the same as those of specific embodiments 1 to 5.

[0042] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the specific method for compacting the composite powder in step 3 is: placing graphite paper close to the wall of the graphite mold, pouring the composite powder stored in an argon atmosphere into the circular graphite mold, and then separating the graphite gasket and the composite powder, and the composite powder and the pressure head with graphite paper; placing the graphite mold containing the composite powder under a hydraulic press and manually pressing to obtain a composite powder green body. The other steps are the same as those of specific embodiments 1 to 6.

[0043] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that the diameter of the graphite mold is 10 mm to 40 mm. The other steps are the same as those of specific embodiments 1 to 7.

[0044] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the sintering equipment is a rapid hot pressing sintering furnace. The other steps are the same as those of specific embodiments 1 to 7.

[0045] The following examples are used to verify the beneficial effects of the present invention:

[0046] Comparative Example 1: Preparation method of ZrB2-ZrC-SiC multiphase ceramic, denoted as Z10T0B1C1-S. Specifically, the preparation is completed in the following steps:

[0047] 1. Preparation of mixed slurry:

[0048] Add ZrSi2, B4C, C powders and anhydrous ethanol into a ball mill with grinding balls, flush the ball mill with argon, and seal the ball mill; fix the sealed ball mill on the ball mill, so that the system is ball milled under argon environment, and the effective ball milling time is 24 hours to obtain a mixed slurry;

[0049] The material of the grinding balls described in step 1 is ZrO2, and the ball-to-material ratio is 10:1;

[0050] The rotation speed of the ball mill described in step 1 is 350r / min;

[0051] The molar ratio of ZrSi2, B4C and C in step 1 is 4:1.05:9.45 (the calculated values ​​of B4C and C are both in excess of 5%).

[0052] The anhydrous ethanol described in step 1 accounts for 31.6% of the total mass of the ZrSi2, B4C and C powders;

[0053] 2. Preparation of composite powder:

[0054] The mixed slurry was dried at room temperature and vacuum conditions for 24 h, and after drying, passed through a 140-mesh sieve under argon atmosphere protection to obtain a composite powder;

[0055] 3. Rapid hot pressing sintering:

[0056] First, the composite powder was compacted and rapidly hot-pressed for 15 min in a rapid hot-pressing sintering furnace at 1700°C and an axial pressure of 40 MPa in a vacuum environment to obtain a ZrB2-ZrC-SiC multiphase ceramic, which was denoted as Z10T0B1C1-S.

[0057] The specific method for compacting the composite powder in step three is: placing graphite paper close to the wall of the graphite mold, pouring the composite powder preserved in an argon atmosphere into a circular graphite mold, and then separating the graphite gasket and the composite powder, and the composite powder and the pressure head with graphite paper; placing the graphite mold containing the composite powder under a hydraulic press and manually pressing it to obtain a composite powder embryo; the diameter of the graphite mold is 30 mm.

[0058] Example 1: A method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics is specifically completed by the following steps:

[0059] 1. Preparation of mixed slurry:

[0060] Under the protection of argon atmosphere, ZrSi2, TiSi2, B4C, C powders and anhydrous ethanol are added to a ball mill, and then grinding balls are added to the ball mill, and then the ball mill is sealed; the sealed ball mill is fixed on a ball mill, argon is introduced after vacuuming, and the ball mill is milled for 24 hours under argon environment to obtain a mixed slurry;

[0061] The material of the grinding balls described in step 1 is ZrO2, and the ball-to-material ratio is 10:1;

[0062] The rotation speed of the ball mill described in step 1 is 350r / min;

[0063] The molar ratio of ZrSi2:TiSi2:B4C:C described in step 1 is 3.6:0.4:1.05:9.45 (the calculated values ​​of B4C and C are both in excess of 5%);

[0064] The anhydrous ethanol described in step 1 accounts for 31.6% of the total mass of ZrSi2, TiSi2, B4C and C powders;

[0065] 2. Preparation of composite powder:

[0066] The mixed slurry was dried at room temperature and vacuum conditions for 24 h, and after drying, passed through a 140-mesh sieve under argon atmosphere protection to obtain a composite powder;

[0067] 3. Rapid hot pressing sintering:

[0068] First, the composite powder is compacted, and then sintered in a rapid hot pressing sintering furnace at 1700°C and an axial pressure of 40 MPa for 15 minutes in a vacuum environment to obtain ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramic, in which the molar ratio of Zr: Ti is 9: 1 and (Zr, Ti) C: (Zr, Ti) B2 is 1: 1, denoted as Z9T1B1C1-S.

[0069] The specific method for compacting the composite powder in step three is: placing graphite paper close to the wall of the graphite mold, pouring the composite powder preserved in an argon atmosphere into a circular graphite mold, and then separating the graphite gasket and the composite powder, and the composite powder and the pressure head with graphite paper; placing the graphite mold containing the composite powder under a hydraulic press and manually pressing it to obtain a composite powder embryo; the diameter of the graphite mold is 30 mm.

[0070] Embodiment 2: The difference between this embodiment and embodiment 1 is that the molar ratio of ZrSi2:TiSi2:B4C:C in step 1 is 3.2:0.8:1.05:9.45 (the calculated values ​​of B4C and C are both 5% excess); in step 3, the molar ratio of Zr:Ti in the ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic is 8:2, which is recorded as Z8T2B1C1-S. The other steps and parameters are the same as those in embodiment 1.

[0071] Example 3: The difference between this example and Example 1 is that the molar ratio of ZrSi2:TiSi2:B4C:C in step 1 is 2.8:1.2:1.05:9.45 (the calculated values ​​of B4C and C are both 5% excess); in step 3, the molar ratio of Zr:Ti in the ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic is 7:3, which is recorded as Z7T3B1C1-S. The other steps and parameters are the same as those in Example 1.

[0072] Example 4: The difference between this example and Example 1 is that the molar ratio of ZrSi2:TiSi2:B4C:C in step 1 is 0.9:0.1:0:3.3 (C is 10% more than the calculated value in the reaction formula); the ceramic obtained in step 3 is (Zr,Ti)C-SiC without (Zr,Ti)B2 phase, and the molar ratio of Zr:Ti in (Zr,Ti)C is 9:1, which is recorded as Z9T1B0C1-S. The other steps and parameters are the same as those in Example 1.

[0073] Embodiment 5: The difference between this embodiment and embodiment 1 is that the molar ratio of ZrSi2:TiSi2:B4C:C in step 1 is 5.4:0.6:1.1:16.5 (the calculated values ​​of B4C and C are both in excess of 10%); the molar ratio of (Zr,Ti)C:(Zr,Ti)B2=2:1 in the ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic obtained in step 3 is denoted as Z9T1B1C2-S. The other steps and parameters are the same as those in embodiment 1.

[0074] Example 6: The difference between this example and Example 1 is that the molar ratio of ZrSi2:TiSi2:B4C:C in step 1 is 2.7:0.3:1.1:6.6 (B4C and C are both in excess of 10%); in step 3, the molar ratio of (Zr,Ti)C:(Zr,Ti)B2=1:2 in the ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic is obtained, which is recorded as Z9T1B2C1-S. The other steps and parameters are the same as those in Example 1.

[0075] Example 7: The difference between this example and Example 1 is that the molar ratio of ZrSi2:TiSi2:B4C:C in step 1 is 1.8:0.2:1.1:3.3 (B4C and C are both in excess of 10%); the ceramic prepared in step 3 is (Zr,Ti)B2-SiC without (Zr,Ti)C phase, wherein the molar ratio of Zr:Ti in (Zr,Ti)B2 is 9:1, recorded as Z9T1B2C0-S. The other steps and parameters are the same as those in Example 1.

[0076] Figure 1 The XRD patterns of the composite powders prepared in the comparative example 1 and the examples 1 to 3 of the present invention, wherein Zr / Ti=7:3 is the example 3, Zr / Ti=8:2 is the example 2, Zr / Ti=9:1 is the example 1, and Zr / Ti=10:0 is the comparative example 1;

[0077] from Figure 1 It can be seen that with the increase of TiSi2 content, the diffraction peak of TiSi2 in the spectrum becomes more obvious.

[0078] Figure 2 XRD patterns of the multiphase ceramics prepared in Comparative Example 1 and Examples 1 to 3 of the present invention;

[0079] from Figure 2 It can be seen that: with the increase of Ti element content, the diffraction peaks of (Zr, Ti) C and (Zr, Ti) B2 both shift toward the large angle direction, which further proves the formation of solid solution and causes the lattice constants of (Zr, Ti) C and (Zr, Ti) B2 to change.

[0080] Figure 3 XRD patterns of the multiphase ceramics prepared in Examples 4 to 7 of the present invention;

[0081] from Figure 3 It can be seen that: with the increase of B4C / C ratio, the phase composition of multiphase ceramics has evolved from (Zr,Ti)C-SiC to (Zr,Ti)B2-(Zr,Ti)C-SiC to (Zr,Ti)B2-SiC. This proves that the reaction sintering method proposed in the present invention can realize the low-temperature rapid preparation of (Zr,Ti)B2-(Zr,Ti)C-SiC multiphase ceramics with any Zr / Ti ratio and any (Zr,Ti)C / (Zr,Ti)B2 two-phase ratio.

[0082] Using oxygen-acetylene flame flow as the heat source, ablation test was carried out on (Zr,Ti)B2-(Zr,Ti)C-SiC multiphase ceramics. The distance from the flame nozzle to the surface of the ablated sample was 10 mm. The diameter of the ablated sample was 30 mm and the thickness was 5 mm. The pressure and flow rate of oxygen and acetylene used in the test process of all samples were the same. The linear ablation rate (R d ) and mass ablation rate (R m ) is calculated according to formula (2) and formula (3).

[0083]

[0084] Among them, d b ,d a 、m b 、m a and ΔT are the original thickness of the sample after ablation (mm), the thickness of the sample after ablation (mm), the original mass of the sample after ablation (g), the mass of the sample after ablation (g), and the ablation time (s), respectively.

[0085] Figure 4 Surface SEM images of the multiphase ceramics prepared in Control Example 1 and Examples 1 to 3 of the present invention after oxyacetylene ablation.

[0086] Depend on Figure 4It can be seen that the surface phase composition of the ZrB2-ZrC-SiC ceramics prepared in the control example after ablation is mainly ZrO2, and the surface morphology presents a loose and porous structure. The ablation layer is prone to mechanical erosion under the scouring of high-temperature airflow. After the introduction of the Ti element, in addition to ZrO2, the ablation product also contains a low-melting point phase containing the Ti element. This promotes the formation of a relatively dense / stable ablation layer. It solves the problems of the ablation layer of ZrC-ZrB2-SiC ceramics being easy to fall off and having insufficient ablation resistance.

[0087] Table 1 shows the ablation resistance data of the multiphase ceramics prepared in Comparative Example 1 and Examples 1 to 2 of the present invention. The pressure and flow rate of oxygen and acetylene used in the test process of all samples are the same. When the ablation duration is 60s, the surface temperature of all samples is 2100±200K.

[0088] Table 1

[0089]

[0090] It can be seen from Table 1 that a certain amount of Ti solid solution can effectively improve the ablation resistance of composite ceramics. When Zr / Ti=9:1, the linear ablation rate of (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics is only -0.00077mm / s. The mass ablation rate is only 0.00015g / s, which is 95.21% better than that of ZrB2-ZrC-SiC ceramics.

Claims

1. A method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramics, characterized in that The preparation method is specifically completed according to the following steps:

1. Preparation of mixed slurry: Add ZrSi2, TiSi2, B4C, C powders and anhydrous ethanol into a ball mill containing grinding balls, inject argon into the ball mill, and then seal the ball mill; fix the sealed ball mill on a ball mill, and mill the ball mill in an argon environment for a period of time to obtain a mixed slurry; The molar ratio of the total amount of ZrSi2 and TiSi2 to B4C and C in step 1 is (5 / 18-1 / 2):(1 / 100-1 / 3):1; wherein the molar ratio of ZrSi2 to TiSi2 is (0.01-0.99):(0.01-0.99); 2. Preparation of composite powder: The mixed slurry is dried for a period of time at room temperature and under vacuum conditions, and after drying, it is sieved under the protection of an argon atmosphere to obtain a composite powder; 3. Rapid hot pressing sintering: First, the composite powder is compacted, and then hot-pressed and sintered for a period of time using a sintering device at 1500° C. to 1900° C. and an axial pressure of 20 MPa to 60 MPa to obtain ablation-resistant (Zr, Ti) B2-(Zr, Ti) C-SiC ceramics; The hot pressing sintering time in step 3 is 5 minutes to 20 minutes, and the environmental conditions are vacuum, argon or nitrogen.

2. The method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic according to claim 1, characterized in that The material of the grinding balls described in step 1 is ZrO2, and the mass ratio of balls to materials is (10-20):

1.

3. The method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic according to claim 1, characterized in that The rotation speed of the ball mill described in step 1 is 300r / min to 500r / min, and the effective ball milling time is 10h to 48h.

4. The method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic according to claim 1, characterized in that The anhydrous ethanol described in step 1 accounts for 20% to 50% of the total mass of the ZrSi2, TiSi2, B4C and C powders.

5. The method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic according to claim 1, characterized in that In step 2, the mixed slurry is dried at room temperature under vacuum conditions for 20 h to 100 h.

6. The method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic according to claim 1, characterized in that After drying in step 2, the mixture is sieved through a 100-200 mesh sieve under the protection of an argon atmosphere to obtain a composite powder.

7. The method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic according to claim 1, characterized in that The specific method for compacting the composite powder in step three is: placing graphite paper tightly against the wall of the graphite mold, pouring the composite powder preserved in an argon atmosphere into a circular graphite mold, and then separating the graphite gasket and the composite powder, and the composite powder and the pressing head with graphite paper; placing the graphite mold containing the composite powder under a hydraulic press and manually pressing it to obtain a composite powder green body.

8. The method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic according to claim 7, characterized in that The diameter of the graphite mold is 10 mm to 40 mm.

9. The method for preparing ablation-resistant (Zr,Ti)B2-(Zr,Ti)C-SiC ceramic according to claim 1, characterized in that The sintering equipment is a rapid hot pressing sintering furnace.

Citation Information

Patent Citations

  • Method for preparing Cf / ZrC-SiC superhigh-temperature ceramic composite material through hot-pressing sintering / precursor cracking process

    CN104311090A

  • Preparation method of molybdenum disilicide / silicon carbide / boron carbide three phase strength composite ceramic

    CN105198433A

  • Preparation method and application of antioxidant diboride-carbide solid solution ceramic

    CN114394837A

  • Efficient ceramic epoxy resin composite material and preparation method thereof

    CN117106287A

  • Hot pressed ZrB2-SiC using zirconium silicides as precursor and manufacturing method of the same

    KR1020120029167A