Carboxylic butyronitrile latex for dip forming process, preparation method of carboxylic butyronitrile latex and dip formed product produced by carboxylic butyronitrile latex

Through emulsion copolymerization technology of water-soluble high molecular weight polyvinyl alcohol, conjugated diene monomer, acrylonitrile and vinyl unsaturated carboxylic acid monomer, combined with chain transfer agent and oxidizing agent, an excellent wearability and high stretching were prepared. The performance of carboxylic nitrile latex solves the problem that glove latex is difficult to achieve high tensile strength and good wearability in the prior art, and significantly improves the quality of impregnated molded products.

CN118909197APending Publication Date: 2024-11-08NANJING TECH UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410929481.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high tensile strength, elongation and good wearability of glove latex at the same time, and the prepared impregnated molded products are prone to form pinholes, affecting quality.

Method used

Carboxylic nitrile latex is prepared by emulsion copolymerization technology using water-soluble high molecular weight polyvinyl alcohol, conjugated diene monomer, acrylonitrile and vinyl unsaturated carboxylic acid monomer, and combined with chain transfer agent, water-soluble oxidant and reducing agent. The reaction temperature is controlled at 30-60°C, and the vulcanized dispersion is ball milled to form a vulcanized dispersion, and finally it is impregnated and molded in the coagulant.

Benefits of technology

Immersed molded products with excellent wearability, high tensile strength and low pinhole ratio were prepared, which significantly improved the durability and physical chemical properties of the gloves.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of preparation methods of latex, in particular to a preparation method of carboxylic butadiene-acrylonitrile latex for a dip-forming process and a dip-formed product produced by the carboxylic butadiene-acrylonitrile latex. A water-soluble high-molecular-weight polyvinyl alcohol polymer is arranged on the outer side of the latex, a conjugated diene monomer, an acrylonitrile monomer and a vinyl unsaturated carboxylic acid monomer are arranged on the inner side of the latex, and in the presence of a chain transfer agent, an electrolyte, a water-soluble oxidizing agent and a water-soluble reducing agent, the water-soluble high-molecular-weight polyvinyl alcohol polymer is added into the latex. The copolymer is prepared by an emulsion copolymerization method, the reaction temperature is 30-60 DEG C, and on the basis that the total mass of the monomers is 100 wt%, the conjugated diene monomer accounts for 60-75 wt%, the acrylonitrile monomer accounts for 38-15 wt%, and the vinyl unsaturated carboxylic acid monomer accounts for 2-10 wt%. The carboxyl butyronitrile latex is mixed with a vulcanized dispersion liquid formed by wet ball milling, and a dip-molded product is prepared by dipping and molding with a coagulant, washing with water and vulcanizing. A dip-molded product produced by the carboxylic butadiene-acrylonitrile latex has excellent durability, high tensile strength, high elongation and good wearing performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of latex preparation methods, in particular to a method for preparing carboxylated nitrile latex used in a dipping molding process and a dipping molded product produced by the method. Background Art

[0002] Glove latex is used to make gloves. Its main properties are puncture resistance, pollution resistance and isolation. It is widely used in medical, pharmaceutical, sanitation, beauty and hairdressing, food processing and other operating industries. Patent CN106397665A emphasizes the preparation of carboxylated nitrile latex for glove dipping by grafting three monomers of acrylonitrile, 1,3-butadiene and styrene on the surface of ABS resin latex. Because the ABS latex seed is too hard (high glass transition temperature), it is difficult for the latex prepared by this method to simultaneously achieve high tensile strength, elongation and good wearability of dip-molded products. CN201510679217.4 discloses a method for preparing high-performance carboxylated nitrile latex, which adopts a two-stage emulsion polymerization process, with styrene-butadiene latex as the seed emulsion, and semi-continuous emulsion polymerization with butadiene, acrylonitrile and unsaturated carboxylic acid as the main monomers in the presence of the latex, supplemented by functional monomers such as multi-double bond cross-linking monomers. The latex prepared by this method has too high a gel content, and the dip-molded products shrink unevenly after vulcanization, and pinholes are easily formed, so high-quality dip-molded products cannot be achieved. Patent CN01123473.3 discloses a method for preparing a carboxylated nitrile latex for thin dip-molded products. The method adopts an oxidation-reduction emulsion polymerization process, and uses butadiene, acrylonitrile, unsaturated carboxylic acid and unsaturated carboxylic acid ester as main monomers to prepare a latex with a lower gel content, thereby improving the physical and chemical properties of the latex products. The carboxylic acid ester contained in the latex prepared by this method has a high boiling point, and it is difficult to remove it by extraction technology in a medium and low temperature environment, which seriously affects the wearability of the dip-molded products. Summary of the invention

[0003] The object of the present invention is to provide a carboxylated nitrile latex for dip molding and a dip molding product produced therefrom, wherein the dip molding product has excellent wearability, high tensile strength and elongation, and low pinhole rate.

[0004] The present invention relates to a carboxylated nitrile latex for dip molding, wherein the latex has a water-soluble high molecular weight polyvinyl alcohol polymer on the outside and a conjugated diene monomer, acrylonitrile monomer and vinyl unsaturated carboxylic acid monomer on the inside, and is prepared by emulsion copolymerization technology in the presence of a chain transfer agent and a water-soluble oxidant and / or a water-soluble reducing agent, and the reaction temperature is 30-60° C. Taking the total weight of the monomers as 100wt% as the calculation basis, the conjugated diene monomer accounts for 60-75wt%, the acrylonitrile monomer accounts for 38-15wt%, and the vinyl unsaturated carboxylic acid monomer accounts for 2-10wt%.

[0005] The conjugated diene monomer is a mixture of one or more of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene and isoprene in any proportion.

[0006] The vinyl unsaturated carboxylic acid monomer is a mixture of one or more of acrylic acid, methacrylic acid, vinyl acetic acid, itaconic acid, maleic acid, maleic anhydride and fumaric acid in any proportion.

[0007] The water-soluble high molecular weight polyvinyl alcohol polymer has an average molecular weight of more than 10,000 and an alcoholysis degree of 60-99.5%. The usage amount of the water-soluble high molecular weight polyvinyl alcohol polymer is 1.5-5.0wt% of the total monomer amount.

[0008] The chain transfer agent is a mixture of one or more of dodecyl mercaptan, tert-dodecyl mercaptan, hexadecyl mercaptan, octadecyl mercaptan, 2-ethylhexyl thioglycolate, isooctyl thioglycolate, and isooctyl mercaptopropionate in any proportion; the amount of the chain transfer agent used is 0.3-2.0wt% of the total monomer amount. The electrolyte is a mixture of one or more of disodium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, sodium bicarbonate, and sodium pyrophosphate in any proportion; the amount of the electrolyte used is 0.02-0.3wt% of the total monomer amount.

[0009] The water-soluble oxidant is a mixture of one or more of sodium persulfate, potassium persulfate, ammonium persulfate, hydrogen peroxide and tert-butyl perbenzoate in any proportion; the amount of the water-soluble peroxide initiator used is 0.1-3.0wt% of the total monomer amount.

[0010] The water-soluble reducing agent is a mixture of one or more of sodium sulfite, sodium bisulfite, vitamin C, methanol, ethanol, ferrous sulfate, and sodium formaldehyde sulfoxylate in any proportion; the amount of the water-soluble reducing agent used is 0-5.0wt% of the total amount of the monomers.

[0011] The pH of the copolymer latex for dipping molding is 7.5-9.5.

[0012] The invention also discloses a method for preparing the carboxyl nitrile latex. The water-soluble high molecular weight polyvinyl alcohol polymer, conjugated diene monomer, acrylonitrile monomer and vinyl unsaturated carboxylic acid monomer are prepared by emulsion copolymerization in the presence of a chain transfer agent, an electrolyte, a water-soluble oxidant and a water-soluble reducing agent. The reaction temperature is 30-60°C. The total weight of the monomers is 100wt% as a calculation basis. The conjugated diene monomer accounts for 60-75wt%, the acrylonitrile monomer accounts for 38-15wt%, and the vinyl unsaturated carboxylic acid monomer accounts for 2-10wt%.

[0013] Furthermore, the present invention also provides a dip-molded product produced using the carboxylated nitrile latex, which is prepared by mixing the carboxylated nitrile latex with a vulcanized dispersion formed by wet ball milling, and then dipping and molding with a coagulant, washing with water, and vulcanizing to obtain the dip-molded product.

[0014] The coagulant is a boric acid aqueous solution, a sodium tetraborate aqueous solution, a potassium hydroxide aqueous solution or a sodium hydroxide aqueous solution.

[0015] The vulcanization dispersion refers to a dispersion formed by mixing sulfur, a vulcanization accelerator, zinc oxide, titanium dioxide, a dispersant and water and subjecting them to ball milling.

[0016] The dip-molded product produced by using the carboxyl nitrile latex of the present invention has excellent durability, high tensile strength, elongation and good wearability. DETAILED DESCRIPTION

[0017] Below in conjunction with specific embodiment, the present invention is further described to the specific embodiment of the present invention.It should be understood that these embodiments are only used for the present invention and are not used to limit the scope of the present invention.It should be understood that after reading the content of the present invention, those skilled in the art make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.

[0018] Example 1

[0019] After the pressure container is evacuated, 100 kg of desalted water, 15 kg of a 10 wt% aqueous solution of polyvinyl alcohol (average molecular weight 10,000, degree of alcoholysis 99.5%), 0.3 kg of dodecyl mercaptan, 38 kg of acrylonitrile, and 2 kg of methacrylic acid are added in sequence, stirring is started, and after nitrogen filling and evacuation operations are performed multiple times, 60 kg of 1,3-butadiene is added and further emulsified for 30 minutes to obtain a monomer emulsified dispersion.

[0020] After the pressure-resistant polymerization reactor was evacuated, 20 kg of deionized water, 0.4 kg of 10 wt% tetrasodium ethylenediaminetetraacetate, and 5.0 kg of ethanol were added in sequence. After nitrogen filling and evacuation for multiple times, the temperature was raised to 38°C, 10 kg of 3 wt% sodium persulfate aqueous solution was added, and the above-prepared monomer emulsified dispersion was dripped into the reactor at the same time. The dripping was completed in 4 to 6 hours, and the reaction was continued after the dripping was completed. The total polymerization time was maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 38° C. and the reaction is maintained for 6 hours; the second stage is heated to 39° C. and the reaction is maintained for 3 hours; the third stage is heated to 43° C. and the reaction is maintained for 2 hours; the fourth stage is heated to 48° C. and the reaction is maintained. When the conversion rate reaches more than 95%, 3 kg of 10 wt% ammonia water and 0.5 kg of 5 wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated, and the pH is adjusted with an alkaline aqueous solution, so as to finally obtain a copolymer latex for dip molding with a solid content of 43-45% and a pH of 8.3-8.5.

[0021] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in a boric acid aqueous solution through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 30MPa, an elongation of 550%, and a stress retention rate of 50%.

[0022] Example 2

[0023] After the pressure container is evacuated, 100 kg of desalted water, 50 kg of a 10 wt% aqueous solution of polyvinyl alcohol (average molecular weight 50,000, degree of alcoholysis 60%), 2.0 kg of hexadecyl mercaptan, 15 kg of acrylonitrile, and 10 kg of acrylic acid are added in sequence, stirring is started, and after nitrogen filling and evacuation operations are performed multiple times, 75 kg of 2,3-dimethyl-1,3-butadiene is added and further emulsified for 30 minutes to obtain a monomer emulsified dispersion.

[0024] After the pressure-resistant polymerization reactor was evacuated, 20 kg of deionized water, 0.2 kg of 10 wt% disodium ethylenediaminetetraacetate, and 0.5 kg of a 10% aqueous sodium sulfite solution were added in sequence. After nitrogen filling and evacuation for multiple times, the temperature was raised to 30°C, 5 kg of a 2 wt% aqueous potassium persulfate solution was added, and at the same time, the above-prepared monomer emulsified dispersion was dripped into the reactor. The dripping was completed within 4 to 6 hours, and the reaction was continued after the dripping was completed. The total polymerization time was maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 30°C and the reaction is maintained for 6 hours; the second stage is heated to 35°C and the reaction is maintained for 3 hours; the third stage is heated to 40°C and the reaction is maintained for 2 hours; the fourth stage is heated to 50°C and the reaction is maintained. When the conversion rate reaches more than 95%, 3kg of 10wt% ammonia water and 0.5kg of 5wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated and the pH is adjusted with an alkaline aqueous solution, and finally a copolymer latex for dip molding with a solid content of 43-45% and a pH of 8.0-8.2 is obtained.

[0025] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in a sodium tetraborate aqueous solution through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 35MPa, an elongation of 560%, and a stress retention rate of 51%.

[0026] Example 3

[0027] After the pressure container is evacuated, 50 kg of desalted water, 20 kg of a 10 wt% aqueous solution of polyvinyl alcohol (average molecular weight 20,000, degree of alcoholysis 80%), 0.5 kg of octadecyl mercaptan, 22 kg of acrylonitrile, and 10 kg of vinyl acetic acid are added in sequence, stirring is started, and after nitrogen filling and evacuation are performed multiple times, 68 kg of 2-ethyl-1,3-butadiene is added and further emulsified for 30 minutes to obtain a monomer emulsified dispersion.

[0028] After the pressure-resistant polymerization reactor was evacuated, 20 kg of deionized water, 3 kg of 10 wt% sodium bicarbonate, and 10 kg of 10% sodium bisulfite aqueous solution were added in sequence. After nitrogen filling and evacuation for multiple times, the temperature was raised to 35° C., 100 kg of 3 wt% ammonium persulfate aqueous solution was added, and the above-prepared monomer emulsified dispersion was dripped into the reactor at the same time. The dripping was completed in 4 to 6 hours, and the reaction was continued after the dripping was completed. The total polymerization time was maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 35°C and the reaction is maintained for 5 hours; the second stage is heated to 40°C and the reaction is maintained for 3 hours; the third stage is heated to 45°C and the reaction is maintained for 3 hours; the fourth stage is heated to 60°C and the reaction is maintained. When the conversion rate reaches more than 95%, 3kg of 10wt% ammonia water and 0.5kg of 5wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated and the pH is adjusted with an alkaline aqueous solution, and finally a copolymer latex for dip molding with a solid content of 43-45% and a pH of 8.7-9.0 is obtained.

[0029] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in potassium hydroxide through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 40MPa, an elongation of 520%, and a stress retention rate of 45%.

[0030] Example 4

[0031] After the pressure container was evacuated, 100 kg of desalted water, 18 kg of a 10 wt% aqueous solution of polyvinyl alcohol (average molecular weight 22,000, degree of alcoholysis 75%), 0.3 kg of 2-ethylhexyl thioglycolate, 19 kg of acrylonitrile, and 7 kg of vinyl acetic acid were added in sequence, stirring was started, and after nitrogen filling and evacuation for multiple times, 74 kg of 2-ethyl-1,3-butadiene was added for further emulsification for 30 minutes to obtain a monomer emulsified dispersion.

[0032] After the pressure-resistant polymerization reactor was evacuated, 20 kg of deionized water, 0.8 kg of 10 wt% sodium pyrophosphate, and 0.5 kg of 10% vitamin C aqueous solution were added in sequence. After nitrogen filling and evacuation for multiple times, the temperature was raised to 33° C., 5 kg of 3 wt% hydrogen peroxide aqueous solution was added, and the above-prepared monomer emulsified dispersion was dripped into the reactor at the same time. The dripping was completed in 4 to 6 hours, and the reaction was continued after the dripping was completed. The total polymerization time was maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 33° C. and the reaction is maintained for 8 hours; the second stage is heated to 41° C. and the reaction is maintained for 2 hours; the third stage is heated to 48° C. and the reaction is maintained for 2 hours; the fourth stage is heated to 60° C. and the reaction is maintained. When the conversion rate reaches more than 95%, 3 kg of 10 wt% ammonia water and 0.5 kg of 5 wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated, and the pH is adjusted with an alkaline aqueous solution, so as to finally obtain a copolymer latex for dip molding with a solid content of 43-45% and a pH of 8.3-8.5.

[0033] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in a boric acid aqueous solution through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 32MPa, an elongation of 650%, and a stress retention rate of 52%.

[0034] Example 5

[0035] After the pressure container was evacuated, 100 kg of desalted water, 22 kg of a 10 wt% aqueous solution of polyvinyl alcohol (average molecular weight 16,000, degree of alcoholysis 88%), 1.2 kg of isooctyl thioglycolate, 34 kg of acrylonitrile and 4 kg of itaconic acid were added in sequence, stirring was started, and after nitrogen filling and evacuation for multiple times, 62 kg of 1,3-pentadiene was added for further emulsification for 30 minutes to obtain a monomer emulsified dispersion.

[0036] After the pressure-resistant polymerization reactor is evacuated, 20 kg of deionized water, 1.5 kg of 10 wt% tetrasodium ethylenediaminetetraacetate, 0.4 kg of 10 wt% disodium ethylenediaminetetraacetate, and 0.7 kg of methanol are added in sequence. After nitrogen filling and evacuation for multiple times, the temperature is raised to 32° C., 20 kg of 3 wt% tert-butyl perbenzoate is added, and the above-prepared monomer emulsified dispersion is dripped into the reactor at the same time. The dripping is completed in 4 to 6 hours, and the reaction is continued after the dripping is completed. The total polymerization time is maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 32° C. and the reaction is maintained for 6 hours; the second stage is heated to 39° C. and the reaction is maintained for 3 hours; the third stage is heated to 45° C. and the reaction is maintained for 2 hours; the fourth stage is heated to 55° C. and the reaction is maintained. When the conversion rate reaches more than 95%, 3 kg of 10 wt% ammonia water and 0.5 kg of 5 wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated, and the pH is adjusted with an alkaline aqueous solution, so as to finally obtain a copolymer latex for dip molding with a solid content of 43-45% and a pH of 8.3-8.5.

[0037] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in a boric acid aqueous solution through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 32MPa, an elongation of 630%, and a stress retention rate of 48%.

[0038] Example 6

[0039] After the pressure container is evacuated, 80 kg of desalted water, 26 kg of 10 wt% aqueous solution of polyvinyl alcohol (average molecular weight 45,000, degree of alcoholysis 65%), 1.0 kg of isooctyl mercaptopropionate, 23 kg of acrylonitrile and 4 kg of maleic acid are added in sequence, stirring is started, and after nitrogen filling and evacuation operations are performed multiple times, 73 kg of isoprene is added and further emulsified for 30 minutes to obtain a monomer emulsified dispersion.

[0040] After the pressure-resistant polymerization reactor is evacuated, 20 kg of deionized water, 0.4 kg of 10 wt% tetrasodium ethylenediaminetetraacetate, 1.4 kg of 10 wt% sodium bicarbonate, and 3.0 kg of 10% ferrous sulfate aqueous solution are added in sequence. After nitrogen filling and evacuation for multiple times, the temperature is raised to 40° C., 10 kg of 3 wt% sodium persulfate aqueous solution and 50 kg of 3 wt% potassium persulfate aqueous solution are added, and the above-prepared monomer emulsified dispersion is added dropwise to the reactor at the same time. The addition is completed in 4 to 6 hours, and the reaction is continued after the addition is completed. The total polymerization time is maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 40° C. and the reaction is maintained for 4 hours; the second stage is heated to 43° C. and the reaction is maintained for 4 hours; the third stage is heated to 48° C. and the reaction is maintained for 2 hours; the fourth stage is heated to 53° C. and the reaction is maintained. When the conversion rate reaches more than 95%, 3 kg of 10 wt% ammonia water and 0.5 kg of 5 wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated, and the pH is adjusted with an alkaline aqueous solution, so as to finally obtain a copolymer latex for dip molding with a solid content of 43-45% and a pH of 8.5-8.7.

[0041] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in a boric acid aqueous solution through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 36MPa, an elongation of 370%, and a stress retention rate of 55%.

[0042] Example 7

[0043] After the pressure container is evacuated, 100 kg of desalted water, 40 kg of 10 wt% polyvinyl alcohol (average molecular weight 33,000, degree of alcoholysis 70%) aqueous solution, 0.3 kg of dodecyl mercaptan, 0.5 kg of hexadecyl mercaptan, 30 kg of acrylonitrile, and 8 kg of maleic anhydride are added in sequence, stirring is started, and after nitrogen filling and vacuuming operations are performed multiple times, 60 kg of 1,3-butadiene and 2 kg of 2,3-dimethyl-1,3-butadiene are added for further emulsification for 30 minutes to obtain a monomer emulsified dispersion.

[0044] After the pressure-resistant polymerization reactor was evacuated, 20 kg of deionized water, 2.0 kg of 10 wt% disodium ethylenediaminetetraacetate, 0.1 kg of 10 wt% sodium bicarbonate, and 5.0 kg of 10% sodium formaldehyde sulfoxylate aqueous solution were added in sequence. After nitrogen filling and evacuation for multiple times, the temperature was raised to 43° C., 15 kg of 3 wt% ammonium persulfate aqueous solution and 15 kg of 3 wt% hydrogen peroxide aqueous solution were added, and the above-prepared monomer emulsified dispersion was dripped into the reactor at the same time. The dripping was completed in 4 to 6 hours, and the reaction was continued after the dripping was completed. The total polymerization time was maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 43° C. and the reaction is maintained for 6 hours; the second stage is heated to 48° C. and the reaction is maintained for 3 hours; the third stage is heated to 53° C. and the reaction is maintained for 2 hours; the fourth stage is heated to 58° C. and the reaction is maintained. When the conversion rate reaches more than 95%, 3 kg of 10 wt% ammonia water and 0.5 kg of 5 wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated, and the pH is adjusted with an alkaline aqueous solution, so as to finally obtain a copolymer latex for dip molding with a solid content of 43-45% and a pH of 8.1-8.3.

[0045] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in a potassium hydroxide aqueous solution through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 44MPa, an elongation of 540%, and a stress retention rate of 52%.

[0046] Example 8

[0047] After the pressure container is evacuated, 80 kg of desalted water, 31 kg of a 10 wt% aqueous solution of polyvinyl alcohol (average molecular weight 48,000, degree of alcoholysis 62%), 1.0 kg of tert-dodecyl mercaptan, 0.2 kg of 2-ethylhexyl thioglycolate, 28 kg of acrylonitrile, and 7 kg of fumaric acid are added in sequence, stirring is started, and after nitrogen filling and vacuuming operations are performed multiple times, 62 kg of 1,3-butadiene and 3 kg of 2-ethyl-1,3-butadiene are added for further emulsification for 30 minutes to obtain a monomer emulsified dispersion.

[0048] After the pressure-resistant polymerization reactor is evacuated, 20 kg of deionized water, 0.2 kg of 10 wt% sodium bicarbonate, 1.8 kg of 10 wt% sodium pyrophosphate, 0.2 kg of methanol and 0.2 kg of ethanol are added in sequence. After nitrogen filling and evacuation for multiple times, the temperature is raised to 38°C, 22 kg of 3 wt% sodium persulfate aqueous solution and 45 kg of 3 wt% tert-butyl perbenzoate aqueous solution are added, and the above-prepared monomer emulsified dispersion is added dropwise to the reactor at the same time. The addition is completed in 4 to 6 hours, and the reaction is continued after the addition is completed. The total polymerization time is maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 38° C. and the reaction is maintained for 9 hours; the second stage is heated to 44° C. and the reaction is maintained for 1 hour; the third stage is heated to 48° C. and the reaction is maintained for 1 hour; the fourth stage is heated to 53° C. and the reaction is maintained. When the conversion rate reaches more than 95%, 3 kg of 10 wt% ammonia water and 0.5 kg of 5 wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated, and the pH is adjusted with an alkaline aqueous solution, so as to finally obtain a copolymer latex for dip molding with a solid content of 43-45% and a pH of 9.0-9.5.

[0049] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in a sodium hydroxide aqueous solution through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 38MPa, an elongation of 600%, and a stress retention rate of 49%.

[0050] Example 9

[0051] After the pressure container is evacuated, 100 kg of desalted water, 36 kg of 10 wt% aqueous solution of polyvinyl alcohol (average molecular weight 43,000, degree of alcoholysis 70%), 0.1 kg of isooctyl thioglycolate, 0.4 kg of isooctyl thiopropionate, 25 kg of acrylonitrile, 4 kg of acrylic acid, and 2 kg of methacrylic acid are added in sequence, stirring is started, and after nitrogen filling and evacuation operations are performed multiple times, 64 kg of 1,3-butadiene and 5 kg of 1,3-pentadiene are added for further emulsification for 30 minutes to obtain a monomer emulsified dispersion.

[0052] After the pressure-resistant polymerization reactor was evacuated, 20 kg of deionized water, 0.8 kg of 10 wt% tetrasodium ethylenediaminetetraacetate, 1.1 kg of 10 wt% sodium pyrophosphate, 2.0 kg of 10% sodium sulfite aqueous solution, and 1.0 kg of 10% sodium bisulfite aqueous solution were added in sequence. After nitrogen filling and evacuation for multiple times, the temperature was raised to 36°C, 8 kg of 3 wt% potassium persulfate aqueous solution and 18 kg of 3 wt% ammonium persulfate aqueous solution were added, and the above-prepared monomer emulsified dispersion was added dropwise to the reactor at the same time. The addition was completed in 4 to 6 hours, and the reaction was continued after the addition was completed. The total polymerization time was maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 36° C. and the reaction is maintained for 6 hours; the second stage is heated to 42° C. and the reaction is maintained for 3 hours; the third stage is heated to 48° C. and the reaction is maintained for 2 hours; the fourth stage is heated to 53° C. and the reaction is maintained. When the conversion rate reaches more than 95%, 3 kg of 10 wt% ammonia water and 0.5 kg of 5 wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated, and the pH is adjusted with an alkaline aqueous solution, so as to finally obtain a copolymer latex for dip molding with a solid content of 43-45% and a pH of 8.3-8.5.

[0053] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in a boric acid aqueous solution through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 33MPa, an elongation of 580%, and a stress retention rate of 54%.

[0054] Example 10

[0055] After the pressure container was evacuated, 80 kg of desalted water, 21 kg of a 10 wt% aqueous solution of polyvinyl alcohol (average molecular weight 22,000, degree of alcoholysis 85%), 1.3 kg of dodecyl mercaptan, 0.1 kg of 2-ethylhexyl thioglycolate, 21 kg of acrylonitrile, 3 kg of itaconic acid, and 2 kg of methacrylic acid were added in sequence, stirring was started, and after nitrogen filling and evacuation for multiple times, 64 kg of 1,3-butadiene and 10 kg of isoprene were added for further emulsification for 30 minutes to obtain a monomer emulsified dispersion.

[0056] After the pressure-resistant polymerization reactor was evacuated, 20 kg of deionized water, 0.4 kg of 10 wt% disodium ethylenediaminetetraacetate, and 0.8 kg of 10 wt% sodium pyrophosphate were added in sequence. After nitrogen filling and evacuation for multiple times, the temperature was raised to 33° C., 60 kg of 3 wt% sodium persulfate aqueous solution was added, and the above-prepared monomer emulsified dispersion was dripped into the reactor at the same time. The dripping was completed in 4 to 6 hours, and the reaction was continued after the dripping was completed. The total polymerization time was maintained for 13 to 16 hours. The polymerization reaction is subjected to four-stage step temperature control, wherein the first stage is 33° C. and the reaction is maintained for 5 hours; the second stage is heated to 39° C. and the reaction is maintained for 3 hours; the third stage is heated to 45° C. and the reaction is maintained for 3 hours; the fourth stage is heated to 50° C. and the reaction is maintained. When the conversion rate reaches more than 95%, 3 kg of 10 wt% ammonia water and 0.5 kg of 5 wt% sodium methylaminodithiocarbamate aqueous solution are added to stop the reaction, a defoaming agent is added, and then the residual monomers are removed, the mixture is concentrated, and the pH is adjusted with an alkaline aqueous solution, so as to finally obtain a copolymer latex for dip molding with a solid content of 43-45% and a pH of 7.5-8.0.

[0057] 1.0 weight part of sulfur, 0.5 weight part of vulcanization accelerator EZ, 1.5 weight part of zinc oxide, 1.5 weight part of titanium dioxide, 0.005 weight part of potassium hydroxide, dispersant and water are added in sequence and mixed and ball milled to prepare a vulcanized dispersion. The dispersion is filtered through 300 meshes, and the vulcanized dispersion is slowly added to the latex while stirring. The pH is adjusted to 9.5-10 with 5% KOH, and finally the solid content of the latex is adjusted to 30%, and stirring is maintained for 24 hours. Then, a dip-molded product is prepared in a mixed sample solution of potassium hydroxide aqueous solution and sodium hydroxide aqueous solution through processes such as dip molding, water washing, and vulcanization. The product has a tensile strength of 45MPa, an elongation of 520%, and a stress retention rate of the dip-molded product of 55%.

Claims

1. A carboxylated nitrile latex for use in a dip molding process, characterized in that: The latex has a water-soluble high molecular weight polyvinyl alcohol polymer on the outside and a conjugated diene monomer, acrylonitrile monomer and vinyl unsaturated carboxylic acid monomer on the inside. It is prepared by an emulsion copolymerization method in the presence of a chain transfer agent, an electrolyte, a water-soluble oxidant and a water-soluble reducing agent. The reaction temperature is 30-60° C. The total weight of the monomers is 100wt% as a calculation basis, the conjugated diene monomer accounts for 60-75wt%, the acrylonitrile monomer accounts for 38-15wt%, and the vinyl unsaturated carboxylic acid monomer accounts for 2-10wt%.

2. The carboxyl nitrile latex for dip molding process according to claim 1, characterized in that: The conjugated diene monomer is a mixture of one or more of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene and isoprene in any proportion.

3. The carboxylated nitrile latex for dip molding process according to claim 1, characterized in that: The vinyl unsaturated carboxylic acid monomer is a mixture of one or more of acrylic acid, methacrylic acid, vinyl acetic acid, itaconic acid, maleic acid, maleic anhydride and fumaric acid in any proportion.

4. The carboxylated nitrile latex for dip molding process according to claim 1, characterized in that: The water-soluble high molecular weight polyvinyl alcohol polymer has an average molecular weight equal to or greater than 10,000 and an alcoholysis degree of 60-99.5%. The usage amount of the water-soluble high molecular weight polyvinyl alcohol polymer is 1.5-5.0wt% of the total monomer amount.

5. The carboxylated nitrile latex for dip molding process according to claim 1, characterized in that: The chain transfer agent is a mixture of one or more of dodecyl mercaptan, tert-dodecyl mercaptan, hexadecyl mercaptan, octadecyl mercaptan, 2-ethylhexyl thioglycolate, isooctyl thioglycolate, and isooctyl mercaptopropionate in any proportion; the amount of the chain transfer agent used is 0.3-2.0wt% of the total amount of the monomer; the electrolyte is a mixture of one or more of disodium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, sodium bicarbonate, and sodium pyrophosphate in any proportion; the amount of the electrolyte used is 0.02-0.3wt% of the total amount of the monomer.

6. The carboxylated nitrile latex for dip molding process according to claim 1, characterized in that: The water-soluble oxidant is a mixture of one or more of sodium persulfate, potassium persulfate, ammonium persulfate, hydrogen peroxide and tert-butyl perbenzoate in any proportion; the usage amount of the water-soluble oxidant is 0.1-3.0wt% of the total monomer amount; the water-soluble reducing agent is a mixture of one or more of sodium sulfite, sodium bisulfite, vitamin C, methanol, ethanol, ferrous sulfate and sodium formaldehyde sulfoxylate in any proportion; the usage amount of the water-soluble reducing agent is 0.0-5.0wt% of the total monomer amount.

7. The carboxylated nitrile latex for dip molding process according to claim 1, characterized in that: The pH value of the carboxyl nitrile latex is 7.5-9.

5.

8. The method for preparing a carboxylated nitrile latex for dip molding process according to claim 1, characterized in that: The water-soluble high molecular weight polyvinyl alcohol polymer, conjugated diene monomer, acrylonitrile monomer and vinyl unsaturated carboxylic acid monomer are prepared by emulsion copolymerization in the presence of a chain transfer agent, an electrolyte, a water-soluble oxidant and a water-soluble reducing agent. The reaction temperature is 30-60° C. The total weight of the monomers is 100wt% as the calculation basis, the conjugated diene monomer accounts for 60-75wt%, the acrylonitrile monomer accounts for 38-15wt%, and the vinyl unsaturated carboxylic acid monomer accounts for 2-10wt%.

9. A dip-molded product produced using the carboxylated nitrile latex for dip-molding process according to claim 1, characterized in that: The carboxyl nitrile latex according to claim 1 is mixed with a vulcanized dispersion formed by wet ball milling, and the mixture is subjected to coagulant dipping molding, water washing, and vulcanization to prepare a dip-molded product.

10. The preparation method according to claim 9, characterized in that: The coagulant is a mixture of one or more of boric acid aqueous solution, sodium tetraborate aqueous solution, potassium hydroxide aqueous solution and sodium hydroxide aqueous solution in any proportion.

Citation Information

Patent Citations

  • Method for preparing high performance carboxylic acrylonitrile butadiene rubber latexes

    CN105237682A

  • Preparation method of carboxylic butadiene-acrylonitrite latex for impregnation of industrial gloves

    CN106397665A

  • Prepn of carboxyl butadiene-acrylonitrile latex with low gel content for soaking thin product

    CN1347924A

  • Preparation method of carboxylated acrylonitrile-butadiene latex for disposable gloves

    CN110615924A

  • Preparation method of copolymer latex for dip-molding process and dip-molded product produced thereby

    CN115043981A